Method for producing boron nitride powder, boron nitride powder, and resin sealing material
By controlling the preparation process of boron nitride powder, including decarburization crystallization, acid treatment and pressure nitriding, the uranium content is reduced, solving the problem of high uranium content in boron nitride powder, and achieving high thermal conductivity and insulation properties for resin sealing materials suitable for semiconductor memory devices.
Patent Information
- Application Number
- CN202380020380.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2023-01-31
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-01-31
AI Technical Summary
The high uranium content in existing boron nitride powders is difficult to reduce, which affects its application as a material that does not easily emit alpha rays in resin sealing materials for semiconductor memory devices.
The preparation process includes decarburization crystallization, acid treatment, and pressure nitriding. The amount of boron source and carbonate used is controlled, and the boron carbide powder is treated with hydrofluoric acid solution to reduce the uranium content, forming aggregated particles composed of primary boron nitride particles.
A significant reduction in uranium content was achieved, and the orientation index of boron nitride powder was reduced to below 15, making it suitable for resin sealing materials of semiconductor memory elements and improving the thermal conductivity and insulation of the material.
Smart Images

Figure BDA0004978869520000201 
Figure BDA0004978869520000221
Abstract
Description
Technical Field
[0001] This disclosure relates to a method for manufacturing boron nitride powder, boron nitride powder, and resin sealing materials. Background Technology
[0002] Boron nitride powder, as an aggregate of boron nitride particles, possesses lubricity, high thermal conductivity, and insulation properties, and is widely used in solid lubricating materials, thermally conductive fillers, and insulating fillers.
[0003] Because boron nitride particles (especially hexagonal boron nitride particles) have a large anisotropy in thermal conductivity, it has been studied to produce boron nitride aggregated particles by aggregating the primary boron nitride particles, thereby suppressing the anisotropy in thermal conductivity caused by the orientation of the primary particles (e.g., Patent Document 1, etc.).
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-135731 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] One example of materials requiring improved thermal conductivity is resin sealing materials for semiconductor memory devices. In resin sealing materials for semiconductor memory devices, materials that do not easily emit alpha rays are needed to prevent soft errors in the semiconductor memory devices. Materials with low uranium content are particularly desirable for this purpose.
[0009] On the other hand, the aggregated particles disclosed in Patent Document 1 typically contain trace amounts of uranium. Furthermore, their structure makes it difficult to remove uranium that has entered the aggregated particles. Therefore, it is difficult to reduce the uranium content of the particles after they have formed.
[0010] Therefore, one aspect of this disclosure is to provide a method for manufacturing boron nitride powder with reduced uranium content, the boron nitride powder comprising aggregated particles formed by the aggregation of primary boron nitride particles. Another aspect of this disclosure is to provide boron nitride powder comprising aggregated particles formed by the aggregation of primary boron nitride particles, and having a sufficiently low uranium content. Furthermore, another aspect of this disclosure is to provide a resin sealing material for semiconductor memory devices containing the aforementioned boron nitride powder.
[0011] Methods for solving problems
[0012] This public document provides at least the following [1] to [9].
[0013] [1] A method for manufacturing boron nitride powder, comprising a decarburization crystallization step, wherein primary boron nitride particles are generated by calcining a raw material mixture comprising boron carbonitride powder, a boron source and a carbonate, and powder comprising aggregated particles formed by the aggregation of the aforementioned primary particles is obtained. In the aforementioned decarburization crystallization step, the amount of the aforementioned boron source used is 55% by mass or more based on the total mass of the aforementioned raw material mixture, and the amount of the aforementioned carbonate used is 4% by mass or more based on the total mass of the aforementioned raw material mixture.
[0014] [2] The method for manufacturing boron nitride powder as described in [1], wherein the firing temperature in the aforementioned decarburization and crystallization process is above 1800°C and the firing time is above 8 hours.
[0015] [3] The method for manufacturing boron nitride powder as described in [1], wherein the firing temperature in the aforementioned decarburization and crystallization process is above 2000°C and the firing time is above 4 hours.
[0016] [4] The method for manufacturing boron nitride powder as described in any one of [1] to [3] further includes a preparation step for preparing the aforementioned boron carbonitride powder, the aforementioned preparation step including: an acid treatment step of contacting the boron carbonitride powder with an acid solution containing hydrofluoric acid to acid treat the aforementioned boron carbonitride powder; and a pressure nitriding step of calcining the acid-treated aforementioned boron carbonitride powder under a nitrogen pressure atmosphere.
[0017] [5] The method for manufacturing boron nitride powder as described in [4], wherein the aforementioned acid solution is a mixed acid containing the aforementioned hydrofluoric acid, and the proportion of hydrofluoric acid in all acid components of the aforementioned mixed acid is 10% by mass or more.
[0018] [6] The method for manufacturing boron nitride powder as described in [4] or [5], wherein the processing temperature in the aforementioned acid treatment step is 60°C or higher, the processing time in the aforementioned acid treatment step is 3 hours or higher, and the acid concentration of the aforementioned acid solution is 20% by mass or higher.
[0019] [7] Boron nitride powder, comprising aggregated particles formed by the aggregation of primary boron nitride particles, wherein the orientation index of the aforementioned boron nitride powder is 15 or less and the uranium content is 20 ppb or less by mass.
[0020] [8] The boron nitride powder described in [7] has a purity of 98.5% by mass or more, an average particle size of 10 to 90 μm, and a crushing strength of the aforementioned aggregated particles of 5 MPa or more.
[0021] [9] A resin sealing material for semiconductor memory elements, comprising the boron nitride powder described in [7] or [8].
[0022] Invention Effects
[0023] According to one aspect of this disclosure, a method for manufacturing boron nitride powder with reduced uranium content can be provided, the boron nitride powder comprising aggregated particles formed by the aggregation of primary boron nitride particles. Furthermore, according to another aspect of this disclosure, boron nitride powder comprising aggregated particles formed by the aggregation of primary boron nitride particles, and having a sufficiently low uranium content, can be provided. Additionally, according to yet another aspect of this disclosure, a resin sealing material for semiconductor memory devices can be provided containing the aforementioned boron nitride powder. Detailed Implementation
[0024] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. Regarding the content of each component in the composition, if multiple substances are present as components, unless otherwise specified, the content refers to the total amount of those substances present in the composition. In this specification, numerical ranges indicated by “~” represent the ranges including the minimum and maximum values before and after the “~”. Furthermore, unless otherwise specified, the units of the values before and after the “~” are the same. The upper or lower limit of the numerical range described in this specification can be replaced with the values shown in the examples. Additionally, the separately stated upper and lower limits can be combined arbitrarily.
[0025] The following describes embodiments of this disclosure. However, these embodiments are merely examples for illustrating this disclosure and are not intended to limit this disclosure to its contents.
[0026] <Method for manufacturing boron nitride powder>
[0027] One embodiment of the boron nitride powder manufacturing method includes a decarburization crystallization step, wherein primary boron nitride particles are generated by calcining a raw material mixture containing boron carbonitride powder, a boron source and a carbonate, and powder containing aggregated particles formed by the aggregation of the primary particles is obtained.
[0028] The inventors' research results in this application show that, in the above-mentioned decarburization crystallization process, by using a boron source and carbonates in amounts specified or higher, the uranium content in the final boron nitride powder can be reduced. Specifically, if the amount of boron source used is 55% by mass or higher based on the total mass of the raw material mixture, and the amount of carbonate used in the crystallization process is 4% by mass or higher based on the total mass of the raw material mixture, the uranium content is reduced.
[0029] One embodiment of the method for manufacturing boron nitride powder may further include a preparation step for preparing boron carbonitride powder used in the aforementioned decarburization crystallization process. The preparation step may include, for example, a pressure nitriding step in which boron carbide powder is calcined under a nitrogen pressure atmosphere. The preparation step may also include an acid treatment step (first acid treatment step) in which the boron carbide powder is acid-treated by contacting an acid solution containing hydrofluoric acid with the boron carbide powder. When the preparation step includes the first acid treatment step, the acid-treated boron carbide powder obtained in the pressure nitriding step is used. The preparation step may also include an acid treatment step (second acid treatment step) in which the boron carbonitride powder is acid-treated by contacting an acid solution containing hydrofluoric acid with the boron carbonitride powder. The boron carbonitride powder used in the second acid treatment step may be the powder obtained in the pressure nitriding step. When the preparation step includes the second acid treatment step, the acid-treated boron carbonitride powder obtained in the acid treatment step is used in the decarburization crystallization process. By implementing the first acid treatment step and / or the second acid treatment step, the uranium content in the final boron nitride powder can be reduced. Therefore, based on ensuring that the amounts of boron source and carbonate used in the above-mentioned decarburization crystallization step are within the specified ranges, implementing the first acid treatment step and / or the second acid treatment step can further reduce the uranium content in the final boron nitride powder.
[0030] The following describes in detail each step of the method for manufacturing boron nitride powder. The second acid treatment step is identical to the first acid treatment step, except that boron carbonitride powder is used instead of boron carbide powder; therefore, the description of the second acid treatment step is omitted.
[0031] (Preparation process)
[0032] [First Acid Treatment Process]
[0033] In the first acid treatment step, by contacting a hydrofluoric acid-containing acid solution with boron carbide powder (B4C powder), the portion of the boron carbide particles in contact with the acid solution can be dissolved. As a result, at least a portion of the uranium present in the boron carbide powder (particularly uranium present near the surface of the boron carbide particles) is removed.
[0034] Boron carbide powder is an aggregate of boron carbide particles. The purity (boron carbide content) of the boron carbide powder is preferably, for example, 97% by mass or more. Commercially available boron carbide powder or separately prepared boron carbide powder can be used. For example, boron carbide powder can be obtained by a method including the following steps: mixing boric acid and acetylene black, heating at 1800–2400°C for 1–10 hours in an inert gas atmosphere to obtain boron carbide blocks; and pulverizing the obtained boron carbide blocks and then appropriately sieving, washing, removing impurities, and drying to prepare boron carbide powder. From the viewpoint of improving the uranium removal efficiency during acid treatment, boron carbide powder with an average particle size of 10 μm or more (e.g., 10–50 μm) is preferred. From the same viewpoint, boron carbide powder with a specific surface area of 1 m² is preferred. 2 / g or less (e.g., 0.05 to 1m) 2 Boron carbide powder (g)
[0035] An acid solution is an aqueous solution containing hydrofluoric acid as its acid component. Although aqueous solutions of hydrogen fluoride are sometimes referred to as hydrofluoric acid, in this specification, the compound represented by HF among the acid components contained in the aqueous solution (acid solution) is referred to as hydrofluoric acid. Furthermore, an acid component is defined as a substance that dissolves in water and releases hydrogen ions.
[0036] From the perspective of improving uranium removal efficiency, the concentration of hydrofluoric acid in the acid solution can be 0.1% by mass or more, or 1% by mass or more, 2% by mass or more, 3% by mass or more, or 10% by mass or more. From the perspective of manufacturing cost and safety, the concentration of hydrofluoric acid in the acid solution can be less than 50% by mass, or less than 45% by mass, 40% by mass or less, or 30% by mass or less. From these perspectives, the concentration of hydrofluoric acid in the acid solution can be, for example, 0.1–50% by mass, 1–50% by mass, 2–45% by mass, 3–40% by mass or 10–30% by mass. It should be noted that the above-mentioned concentration of hydrofluoric acid refers to the content of hydrofluoric acid (HF) based on the total mass of the acid solution.
[0037] The acid solution can also be a mixed acid that includes acid components other than hydrofluoric acid. In this case, from the viewpoint of improving uranium removal efficiency, the proportion of hydrofluoric acid in the total acid components of the acid solution can be 4% by mass or more, or 10% by mass or more, 20% by mass or more, 30% by mass or more, or 40% by mass or more. From the viewpoint of manufacturing cost and safety, the proportion of hydrofluoric acid in the total acid components can be less than 80% by mass, or less than 70% by mass or less, or less than 60% by mass. From these viewpoints, the proportion of hydrofluoric acid in the total acid components can, for example, be 4–80% by mass, 10–70% by mass, 20–60% by mass, 30–60% by mass, or 40–60% by mass.
[0038] Examples of acids that can be included in an acid solution, other than hydrofluoric acid, include hydrochloric acid (HCl), nitric acid (HNO3), and sulfuric acid (HSO4). From the viewpoint of improving uranium removal efficiency, hydrochloric acid is preferred.
[0039] From the perspective of efficiently promoting removal, the concentration of hydrochloric acid in the acid solution can be 2% by mass or more, or 3% by mass or more, 5% by mass or more, 7% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, or 40% by mass or more. From the perspective of manufacturing cost and safety, the concentration of hydrochloric acid in the acid solution can be less than 60% by mass, or less than 50% by mass, less than 35% by mass, less than 30% by mass, or less than 25% by mass. From these perspectives, the concentration of hydrochloric acid in the acid solution can, for example, be 2–60% by mass, 3–60% by mass, 5–60% by mass, 7–60% by mass, 10–60% by mass, 20–60% by mass, 30–60% by mass, or 40–60% by mass, or 5–35% by mass, 7–30% by mass, or 10–25% by mass. It should be noted that the above-mentioned concentration of hydrochloric acid refers to the content of hydrochloric acid (HCl) based on the total mass of the acid solution.
[0040] From the perspective of improving uranium removal efficiency, the acid concentration of the acid solution can be 2% by mass or more, or 3% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, or 40% by mass or more. From the perspective of manufacturing cost and safety, the acid concentration of the acid solution can be less than 50% by mass, or less than 45% by mass or less, or less than 40% by mass. From these perspectives, the acid concentration of the acid solution can be, for example, 2–50% by mass, 3–45% by mass, 5–40% by mass, 10–50% by mass, 20–50% by mass, 30–50% by mass, or 40–50% by mass. It should be noted that the above acid concentrations refer to the content of all acid components based on the total mass of the acid solution.
[0041] There are no particular limitations on the method of contacting the acid solution with the boron carbide powder. Examples include mixing the boron carbide powder with the acid solution by adding the powder into the solution, and continuously injecting the acid solution into the boron carbide powder. In the method of mixing the boron carbide powder with the acid solution, from the viewpoint of improving uranium removal efficiency, the mixture containing the boron carbide powder and the acid solution can be stirred. Stirring can be performed using, for example, a mixer, an electromagnetic stirrer, or a disperser. When acid treating the boron carbide powder by mixing it with the acid solution, the acid treatment can be repeated multiple times. For example, the following series of operations can be repeated: mixing the boron carbide powder with the acid solution, separating the boron carbide powder from the acid solution after a certain period of time, and then mixing the separated boron carbide powder with a new acid solution. The amount of acid solution used relative to 100 parts by mass of boron carbide powder can be, for example, 80 parts by mass or more, 500 parts by mass or less, or 80 to 500 parts by mass.
[0042] From the viewpoint of improving uranium removal efficiency, the processing temperature in the acid treatment process can be above 40°C, 60°C, or 75°C. From the viewpoints of suppressing the reduction in processing efficiency due to the volatilization of hydrogen fluoride and from the viewpoints of safety, the processing temperature in the acid treatment process can be below 95°C, 92°C, or 90°C. From these viewpoints, the processing temperature in the acid treatment process can be, for example, 40–95°C, 60–92°C, or 75–90°C. It should be noted that the above processing temperature refers to the temperature of the acid solution in contact with the boron carbide powder during acid treatment. When acid treatment of boron carbide powder is performed by mixing boron carbide powder with an acid solution, the above processing temperature can also be referred to as the temperature of the mixture containing boron carbide powder and acid solution.
[0043] From the perspective of increasing uranium removal, the processing time in the acid treatment process can be more than 1 hour, or more than 2 hours, 3 hours, or more than 5 hours. From the perspective of manufacturing cost and safety, the processing time in the acid treatment process can be less than 15 hours, or less than 12 hours, or less than 10 hours. Considering these points, the processing time in the acid treatment process can be, for example, 1–15 hours, 2–12 hours, 3–10 hours, or 5–10 hours. It should be noted that the above processing times refer to the contact time between boron carbide powder and acid solution.
[0044] From the viewpoint of further increasing the amount of uranium removed, it is preferable to set the processing temperature in the acid treatment process to 60°C or higher and the processing time in the acid treatment process to 3 hours or higher. More preferably, the processing temperature in the acid treatment process is set to 60°C or higher, the processing time in the acid treatment process is set to 3 hours or higher, and the acid concentration of the acid solution is set to 20% by mass or higher.
[0045] [Pressure nitriding process]
[0046] In the pressure nitriding process, boron carbide powder is sintered under a nitrogen pressure atmosphere, thereby nitriding the boron carbide and obtaining a sintered product containing boron carbonitride. The obtained sintered product tends to contain hexagonal boron carbonitride with high purity. The same boron carbide powder as exemplified as the boron carbide powder used in the first acid treatment process described above can be used as an example. When performing the first acid treatment process, the acid-treated boron carbide powder obtained after the first acid treatment process is used.
[0047] The firing temperature in the pressure nitriding process is preferably higher than that in the decarburization and crystallization process. For example, the firing temperature in the pressure nitriding process can be 1900–2200°C, 2000–2200°C, or 2100–2200°C. By keeping the firing temperature within the above range, the crystallinity of boron carbonitride can be improved, and the proportion of hexagonal boron carbonitride can be increased. The firing time in the pressure nitriding process is not particularly limited, as long as nitriding is sufficiently carried out; for example, it can be 6–30 hours, 8–25 hours, or 10–20 hours.
[0048] The pressure (atmosphere pressure) in the pressurized nitriding process can be, for example, 0.6–1 MPa, 0.7–1 MPa, or 0.8–1 MPa. By keeping the pressure within these ranges, manufacturing costs can be reduced, and the nitriding of boron carbide can be carried out efficiently and thoroughly. It should be noted that the pressures mentioned above refer to gauge pressure.
[0049] In the pressurized nitriding process, the nitrogen concentration of the pressurized atmosphere can be, for example, 95% by volume or more, 98% by volume or more, or 99.9% by volume or more. The upper limit of the nitrogen concentration is 100% by volume. By keeping the nitrogen concentration within the above range, boron carbide nitriding can be carried out under milder conditions. It should be noted that the above nitrogen concentrations are volume concentrations based on standard conditions.
[0050] The calcined material obtained in the pressure nitriding process can be used directly in the decarburization crystallization process, or it can be used in the decarburization crystallization process after appropriate crushing, grading, cleaning, and heat treatment (e.g., oxidation treatment in an oxygen-containing atmosphere). The crushing process can be carried out using general crushers or pulverizers such as ball mills, vibratory mills, and jet mills. It should be noted that "crushing" in this specification also includes "pulverizing".
[0051] (Decarburization crystallization process)
[0052] In the decarburization crystallization process, boron carbonitride powder (B4CN4 powder) is calcined together with a boron source and carbonates, which decarburizes the boron carbonitride and increases its crystallinity. As a result, boron nitride powder (BN powder) containing aggregated particles formed by the aggregation of primary boron nitride particles can be obtained. The boron nitride in the boron nitride powder obtained by this method is typically hexagonal boron nitride, containing aggregated particles formed by the aggregation of primary hexagonal boron nitride particles in a scaly pattern.
[0053] Boron carbonitride powder is an aggregate of boron carbonitride particles. The purity (boron carbonitride content) of the boron carbonitride powder is preferably 98% by mass or more. Commercially available boron carbonitride powder or the boron carbonitride powder prepared in the above-described preparation process can be used. From the viewpoint of increasing the proportion of hexagonal boron carbonitride in the obtained boron nitride powder, it is preferable to use boron carbonitride powder with a high proportion of hexagonal boron carbonitride, and more preferably, boron carbonitride powder obtained through the above-described pressure nitriding process.
[0054] Examples of boron sources include boric acid and boron oxide. One type can be used alone, or two or more can be used in combination. From the viewpoints of easily achieving a growth-promoting effect on primary particles and easily reducing uranium content, boric acid is preferred as a boron source.
[0055] Examples of carbonates include sodium carbonate, calcium carbonate, and strontium carbonate. They can be used alone or in combination of two or more. From the viewpoints of easily achieving a growth-promoting effect on primary particles and easily reducing uranium content, sodium carbonate is preferred as the carbonate.
[0056] From the perspective of reducing uranium content, the amount of boron source used can be 55% by mass or more, or 57% by mass or more, or 59% by mass or more. From the perspective of improving the crushing strength of aggregated particles, the amount of boron source used can be 70% by mass or less, 65% by mass or less, or 60% by mass or less. The amount of boron source used can also be less than 55% by mass. However, if the amount of boron source used is 50% by mass or more, it is easy to promote the growth of primary boron nitride particles, and it is easy to obtain boron nitride powder with an average particle size of 10-90 μm and a crushing strength of 5 MPa or more. From the above perspectives, the amount of boron source used can be 50-70% by mass, 55-70% by mass, 57-70% by mass, 59-70% by mass, 55-65% by mass, 57-65% by mass, 59-65% by mass, 55-60% by mass, 57-60% by mass, or 59-60% by mass. It should be noted that the above usage amount is based on the total mass of the raw material mixture, but the usage amount based on the total amount of boron carbonitride powder, boron source and carbonate can also be within the above range.
[0057] From the perspective of reducing uranium content, the amount of carbonate used can be 4% by mass or more, or 5% by mass or more, or 6% by mass or more. From the perspective of improving the crushing strength of aggregated particles, the amount of carbonate used can be less than 10% by mass, less than 8% by mass, or less than 6% by mass. The amount of carbonate used can also be less than 4% by mass. Among these, if the amount of carbonate used is 1% by mass or more, it is easy to promote the growth of primary boron nitride particles, and it is easy to obtain boron nitride powder with an average particle size of 10-90 μm and a crushing strength of 5 MPa or more. From the above perspective, the amount of carbonate used can be 1-10% by mass, 4-10% by mass, 5-10% by mass, 6-10% by mass, 4-8% by mass, 5-8% by mass, 6-8% by mass, 4-6% by mass, or 5-6% by mass. It should be noted that the above usage amounts are based on the total mass of the raw material mixture, but the usage amounts based on the total amount of boron carbonitride powder, boron source, and carbonate can also be within the above range.
[0058] In the decarburization crystallization process, materials other than boron carbonitride powder, boron source, and carbonate can be used, or only boron carbonitride powder, boron source, and carbonate can be used.
[0059] The firing temperature in the decarburization crystallization process is preferably 1800°C or higher, but can also be 1900°C or higher, or 2000°C or higher. Setting the firing temperature to 1800°C or higher allows for more complete growth of primary particles. The firing temperature in the decarburization crystallization process is preferably 2400°C or lower, but can also be 2200°C or lower, or 2100°C or lower. Setting the firing temperature to 2400°C or lower suppresses yellowing of the boron nitride powder. From the above perspective, the firing temperature in the decarburization crystallization process can be, for example, 1800–2400°C, 1900–2200°C, or 2000–2100°C. It should be noted that the above firing temperatures refer to the holding temperature during heating (firing). The starting temperature for heating is not particularly limited and can be room temperature (e.g., 25°C). When heating begins at a temperature lower than the holding temperature, the heating rate can be, for example, 1 to 10 °C / min up to 1000 °C, and the heating rate above 1000 °C can be, for example, 0.1 to 5 °C / min.
[0060] The firing time in the decarburization crystallization process is preferably 4 hours or more, but can also be 6 hours or more, or 8 hours or more. By setting the firing time to 4 hours or more, the growth of primary particles can be more complete. The firing time in the decarburization crystallization process is preferably 40 hours or less, but can also be 30 hours or less, or 20 hours or less. By setting the firing time to 40 hours or less, the increase in manufacturing costs can be suppressed. From the above perspective, the firing time in the decarburization crystallization process can be, for example, 4–40 hours, 6–30 hours, or 8–20 hours. It should be noted that the above firing time refers to the holding time at the above firing temperature (holding temperature).
[0061] According to the inventors' research, even by changing the firing conditions in the decarburization crystallization process, the uranium content can be reduced. From the viewpoint of further reducing the uranium content, it is preferable that the firing temperature is 1800°C or higher and the firing time is 8 hours or higher, or that the firing temperature is 2000°C or higher and the firing time is 4 hours or higher, and more preferably that the firing temperature is 2000°C or higher and the firing time is 8 hours or higher.
[0062] The firing atmosphere for the decarburization crystallization process can be, for example, atmospheric or vacuum, or an inert gas atmosphere such as nitrogen or argon. The firing process can be carried out at atmospheric pressure or at pressures above atmospheric pressure. The pressure (atmosphere pressure) in the decarburization crystallization process can be, for example, 10 kPa or higher, 15 kPa or higher, or 20 kPa or higher. By maintaining the pressure at 10 kPa or higher, the removal of boron sources, carbonates, and other additives from the system can be suppressed, resulting in a more uniform reaction field for the boron nitride particles. The pressure (atmosphere pressure) in the decarburization crystallization process can be, for example, 80 kPa or lower, 60 kPa or lower, or 40 kPa or lower. By maintaining the pressure at 80 kPa or lower, the disintegration of aggregated particles can be further suppressed during the decarburization crystallization process. From the above perspective, the pressure (atmosphere pressure) in the decarburization crystallization process can be 10–80 kPa, 10–60 kPa, or 20–40 kPa. It should be noted that the above pressures refer to gauge pressure.
[0063] Boron nitride powder after the decarburization and crystallization process can be appropriately pulverized, classified, and cleaned. Pulverization can be carried out using general pulverizers or crushers such as ball mills, vibratory mills, and jet mills.
[0064] In the above-described method for manufacturing boron nitride powder, boron nitride powder containing aggregated particles formed by the aggregation of primary boron nitride particles and having an orientation index of 15 or less can be obtained. Furthermore, in the above-described method for manufacturing boron nitride powder, by using boron source and carbonate amounts of 55% by mass or more and 4% by mass or more in the decarburization crystallization process, respectively, and by acid treating boron carbide powder with an acid solution containing hydrofluoric acid, aggregated particles formed by the aggregation of primary boron nitride particles can be formed, and the uranium content can be reduced. These methods for reducing uranium content do not necessarily need to be implemented in their entirety, but by combining multiple methods, boron nitride powder with a further reduced uranium content can be provided. It should be noted that, in this specification, the orientation index of boron nitride powder refers to the value measured according to the following method.
[0065] X-ray diffraction measurements were performed on boron nitride powder to obtain its X-ray diffraction pattern. Based on this pattern, peak intensities I(002) and I(100) corresponding to the (002) and (100) planes were obtained. Using the obtained peak intensities, the orientation index [I(002) / I(100)] of the boron nitride powder was calculated. For example, the "ULTIMA-IV" (product name) manufactured by Rigaku Corporation was used as the X-ray diffraction apparatus.
[0066] <Boron nitride powder>
[0067] One embodiment of the boron nitride powder includes aggregated particles composed of primary boron nitride particles, wherein the orientation index of the boron nitride powder is 15 or less, and the uranium content is 20 ppb or less by mass. In addition to the aggregated particles, the boron nitride powder may also contain primary particles. These primary boron nitride particles may, for example, be flake-like hexagonal boron nitride particles.
[0068] The aforementioned boron nitride powder has a uranium content of 20 ppb or less by mass, and therefore can be considered a material that does not easily emit alpha rays. Furthermore, the aforementioned boron nitride powder has an orientation index of 15 or less. Therefore, even if at least a portion of the aggregated particles disintegrate and the orientation increases during mixing with resin, large anisotropy in aspects such as heat dissipation of the resin sealing material can be suppressed. Therefore, the aforementioned boron nitride powder is suitable for use in resin sealing materials for semiconductor memory devices requiring heat dissipation.
[0069] The aforementioned boron nitride powder can be obtained, for example, by using boron source and carbonate in the decarburization crystallization process of the manufacturing method described in the above embodiments at amounts of 55% by mass and 4% by mass, respectively.
[0070] The uranium content of boron nitride powder can be, for example, 18 ppb or less by mass, 16 ppb or less by mass, 14 ppb or less by mass, 12 ppb or less by mass, 10 ppb or less by mass, 7 ppb or less by mass, or 5 ppb or less by mass. Boron nitride powder with such uranium content can be obtained, for example, by combining the implementation of an acid treatment process (first acid treatment process and / or second acid treatment process), changes in the acid treatment conditions in the acid treatment process, and changes in the calcination conditions in the decarburization crystallization process. The lower limit of uranium content can be, for example, 5 ppb by mass. Uranium content can be, for example, 5–20 ppb by mass, 5–18 ppb by mass, 5–16 ppb by mass, 5–14 ppb by mass, 5–12 ppb by mass, 5–10 ppb by mass, or 5–7 ppb by mass. It should be noted that the above contents are based on the total mass of the boron nitride powder.
[0071] The uranium content of the boron nitride powder in this specification refers to the value determined according to the following method.
[0072] According to the chemical analysis method for boron nitride powder in JCRS108, 0.5 g of the sample (boron nitride powder) was subjected to pressurized acid decomposition in a mixture of nitric acid, sulfuric acid, and hydrofluoric acid at 180°C for 18 hours. The solution obtained by pressurized acid decomposition was then dried on a hot plate to solidify it. The resulting solid component was mixed with nitric acid to prepare a mixture. Next, the solid component was dissolved by heating the mixture on a hot plate to obtain a nitric acid solution. The uranium content in this nitric acid solution was then determined using ICP-MS (inductively coupled plasma mass spectrometry). The ICP-MS determination conditions are as follows.
[0073] (ICP-MS determination conditions)
[0074] Plasma mode: Low matrix mode, Tuned mode: He, Spectrum mode, Peak pattern: 1 point, Repetition: 3, Number of scans: 100, Integration time: 1 second
[0075] From the viewpoint of further reducing the impact of the disintegration of the aforementioned aggregated particles, the orientation index can also be 12 or less, or 10 or less. The orientation index can be 3 or more, 4 or more, or 6 or more, and can be 3–15, 4–12, or 6–10. It should be noted that the orientation index of boron nitride powder can be adjusted, for example, by controlling the growth of primary particles during the manufacture of boron nitride powder.
[0076] The purity of the boron nitride powder is preferably 98.5% by mass or higher, but can also be 99% by mass or higher, or 99.5% by mass or higher. There is no particular upper limit to the purity of the boron nitride powder; it can be 100% by mass or 99.5% by mass.
[0077] The purity of boron nitride powder in this specification refers to the value determined by titration as described later. First, the boron nitride powder sample is decomposed using sodium hydroxide. Ammonia is distilled from the decomposition solution using steam distillation and collected in an aqueous boric acid solution. This collected solution is then titrated using a standard sulfuric acid solution. Based on the titration results, the nitrogen (N) content in the sample is calculated. Based on the obtained nitrogen content, the boron nitride content in the sample can be determined using formula (I), and the purity of the boron nitride powder can be calculated. It should be noted that the formula weight of boron nitride is 24.818 g / mol, and the atomic weight of nitrogen is 14.006 g / mol.
[0078] The boron nitride content [mass%] in the sample = the nitrogen atom (N) content [mass%] × 1.772…(I)
[0079] From the viewpoint of preventing disintegration during compounding with resin, the aggregated particles contained in the boron nitride powder preferably have a crushing strength of 5 MPa or more. The crushing strength of the aggregated particles can also be 8 MPa or more, or 10 MPa or more. Alternatively, the crushing strength of the aggregated particles can be 20 MPa or less, 15 MPa or less, or 12 MPa or less. By setting the crushing strength of the aggregated particles to 20 MPa or less, at least a portion of the aggregated particles moderately disintegrates during compounding with resin, thus easily suppressing the formation of pores. As a result, the obtained resin sealing material has higher insulation properties. From the above viewpoint, the crushing strength of the aggregated particles can, for example, be 5–20 MPa, 8–15 MPa, or 10–12 MPa. It should be noted that the crushing strength of the aggregated particles can be adjusted, for example, by changing the firing conditions.
[0080] The crushing strength in this specification refers to the value determined according to JIS R 1639-5:2007 "Fine ceramics - Determination of particle properties - Part 5: Crushing strength of a single particle". The crushing strength σ (unit: MPa) of one aggregated particle is determined by the dimensionless number α (α = 2.48) varying according to the position within the aggregated particle, the crushing test force P (unit: N), and the particle size d (unit: μm), using the formula σ = α × P / (π × d). 2 The value was calculated by measuring more than 20 aggregated particles and determining the cumulative damage rate of 63.2%. A micro compression testing machine can be used for this measurement. For example, the "MCT-W500" (product name) manufactured by Shimadzu Corporation can be used.
[0081] The average particle size of boron nitride powder can be, for example, 90 μm or less, 80 μm or less, or 70 μm or less. By making the average particle size 90 μm or less, the sealing portion formed by the resin sealing material can be thinner. The average particle size of boron nitride powder can be, for example, 10 μm or more, 20 μm or more, or 30 μm or more. By making the average particle size 10 μm or more, the thermal conductivity of the resin sealing material can be further improved. From these viewpoints, the average particle size of boron nitride powder can be, for example, 10–90 μm, 20–80 μm, or 30–70 μm.
[0082] The average particle size in this specification refers to the 50% cumulative particle size (median particle size) in the cumulative particle size distribution on a volume basis. More specifically, it refers to the particle size (D50) at which the cumulative value in the cumulative particle size distribution on a volume basis obtained by laser diffraction scattering for powders reaches 50%. Laser diffraction scattering is performed according to the method described in ISO 13320:2009. For this measurement, a laser diffraction scattering particle size distribution measuring apparatus can be used. For example, the "LS-13 320" (product name) manufactured by BECKMAN COULTER can be used. During the measurement, no homogenization is performed; the measurement is conducted in the presence of aggregated particles.
[0083] From the perspective of the insulation properties of resin sealing materials, boron nitride powder is preferably 98.5% by mass or higher, with an average particle size of 10 to 90 μm and a crushing strength of aggregated particles of 5 MPa or higher.
[0084] <Resin Sealing Materials>
[0085] One embodiment relates to a resin sealing material for semiconductor memory, which contains the boron nitride powder described in the above embodiment.
[0086] As a resin included in a resin sealing material, known resins used in resin sealing materials can be used. Examples of such resins include liquid crystal polymers, fluoropolymers, silicone resins, silicone rubbers, acrylic resins, polyolefins (polyethylene, etc.), epoxy resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, polyimides, polyamide-imides, polyether-imides, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, fully aromatic polyesters, polysulfones, polyethersulfones, polycarbonates, maleimide-modified resins, ABS (acrylonitrile-butadiene-styrene) resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.
[0087] Based on the total volume of the resin sealant, the resin content can be, for example, 15% by volume or more, 20% by volume or more, or 30% by volume or more. Based on the total volume of the resin sealant, the resin content can be, for example, 60% by volume or less, 50% by volume or less, or 40% by volume or less. Based on the total volume of the resin sealant, the resin content can be, for example, 15-60% by volume, 20-50% by volume, or 30-40% by volume.
[0088] Based on the total volume of the resin sealing material, the content of boron nitride powder can be, for example, 30% by volume or more, 40% by volume or more, 50% by volume or more, or 60% by volume or more. Based on the total volume of the resin sealing material, the content of boron nitride powder can be, for example, less than 85% by volume, less than 80% by volume, or less than 70% by volume. Based on the total volume of the resin sealing material, the content of boron nitride powder can be, for example, 30–85% by volume, 40–85% by volume, 40–80% by volume, 50–80% by volume, 50–70% by volume, or 60–70% by volume.
[0089] In addition to the resin and boron nitride powder, the resin sealing material may also contain a curing agent for curing the resin. The curing agent can be appropriately selected depending on the type of resin. When the resin is an epoxy resin, examples of curing agents include phenol (Novolac), acid anhydrides, amino compounds, and imidazole compounds. The content of the curing agent relative to 100 parts by weight of the resin can be, for example, 0.5 parts by weight or more, 1 part by weight or less, 15 parts by weight or less, or 0.5 to 15 parts by weight or 1 to 10 parts by weight.
[0090] Example
[0091] The contents of this disclosure will be described in more detail with reference to the embodiments and comparative examples, but this disclosure is not limited to the following embodiments.
[0092] <Example 1>
[0093] [Preparation of boron carbide powder]
[0094] Using a Henschel mixer, 100 parts by weight of orthoboric acid manufactured by Nippon Denko Corporation and 35 parts by weight of acetylene black (trade name: HS100L) manufactured by Denka Corporation were mixed. The resulting mixture was filled into a graphite crucible and heated in an electric arc furnace at 2200°C for 6 hours under an argon atmosphere to obtain lumpy boron carbide (B4C). The lumpy material was coarsely pulverized using a jaw crusher to obtain coarse powder. The coarse powder was further pulverized using a ball mill with silicon carbide balls (diameter: 10 mm) to obtain fine powder. The ball milling was carried out at a speed of 25 rpm for 60 minutes. Then, the fine powder was classified using a vibrating sieve with a mesh size of 63 μm to produce boron carbide powder (B4C powder) with an average particle size of 20 μm. The specific surface area of the boron carbide powder is 0.4 m². 2 / g, purity 98% by mass%.
[0095] The average particle size of the boron carbide powder was determined according to ISO 13320:2009 using a laser diffraction scattering particle size distribution measuring apparatus (apparatus name: LS-13 320) manufactured by Beckman Coulter. It should be noted that the boron carbide powder was not homogenized. For the particle size distribution determination, water was used as the solvent for dispersing the boron carbide powder, and hexametaphosphate was used as the dispersant. The refractive index of water was 1.33, and the refractive index of the boron carbide powder was 2.6.
[0096] The specific surface area of the boron carbide powder was calculated using the BET single-point method with nitrogen, as described in JIS Z 8830:2013 "Method for determination of specific surface area of powders (solids) based on gas adsorption". A specific surface area measuring apparatus (device name: Quantasorb) manufactured by Yuasa Ionics Co., Ltd. was used as the measuring device. It should be noted that the measurement was performed after the boron carbide powder was dried and degassed at 300°C for 15 minutes.
[0097] The purity of boron carbide powder is calculated by the sum of its carbon and boron content. The carbon content is calculated using combustion infrared absorption spectrometry, and the boron content is calculated using ICP emission spectroscopy.
[0098] [Pressure nitriding process]
[0099] The prepared boron carbide powder was calcined in a carbon resistance furnace for 12 hours. The calcination atmosphere was set to nitrogen, the calcination temperature to 2050℃, and the atmosphere pressure to 0.90 MPa. This yielded boron carbonitride powder. Powder X-ray diffraction (XRD) analysis of the boron carbonitride powder confirmed the disappearance of boron carbide and the formation of hexagonal boron carbonitride.
[0100] [Decarburization and crystallization process]
[0101] Using a Henschel mixer, the calcined product (boron carbonitride powder) obtained in the above-mentioned pressure nitriding process, boric acid, and sodium carbonate were mixed to obtain a raw material mixture. Based on the total mass of the raw material mixture, the amount of boric acid used was 60% by mass, and the amount of sodium carbonate used was 5% by mass. Next, the obtained raw material mixture was filled into a boron nitride crucible and calcined in a resistance heating furnace at a calcination temperature of 1950°C and atmospheric pressure for 5 hours under a nitrogen atmosphere. Specifically, the temperature was increased from room temperature to 1000°C at a heating rate of 10°C / min, then increased from 1000°C to 1950°C at a heating rate of 2°C / min, and held at 1950°C for 5 hours. Next, the obtained powder was crushed using a Henschel mixer for 20 minutes, and the resulting pulverized material was graded through a 75μm sieve to obtain boron nitride powder of Example 1 containing aggregated particles composed of primary particles of hexagonal boron nitride. The obtained boron nitride powder has a uranium content of 19 ppb by mass, an orientation index of 7, a purity of 99% by mass, an average particle size of 40 μm, and a crushing strength of 12 MPa for aggregated particles in the boron nitride powder.
[0102] The uranium content of boron nitride powder was determined by the following method.
[0103] According to the chemical analysis method for boron nitride powder in JCRS108, 0.5 g of the sample (boron nitride powder) was subjected to pressurized acid decomposition in a mixture of nitric acid, sulfuric acid, and hydrofluoric acid at 180°C for 18 hours. The solution obtained by pressurized acid decomposition was then dried on a hot plate to solidify it. The resulting solid component was mixed with nitric acid to prepare a mixture. Next, the solid component was dissolved by heating the mixture on a hot plate to obtain a nitric acid solution. The uranium content in this nitric acid solution was then determined using ICP-MS (inductively coupled plasma mass spectrometry). The ICP-MS determination conditions are as follows.
[0104] (ICP-MS determination conditions)
[0105] Plasma mode: Low matrix mode, Tuned mode: He, Spectral mode peak pattern: 1 point, Repetition: 3, Number of scans: 100, Integration time: 1 second
[0106] The orientation index of boron nitride powder was determined based on the results of powder X-ray diffraction. First, boron nitride powder was filled into the recess of a glass sample cell with a depth of 0.2 mm, which is attached to an X-ray diffraction apparatus (manufactured by Rigaku Co., Ltd., trade name: ULTIMA-IV). The sample was then pressed using a powder sample forming machine (manufactured by Amenatech Co., Ltd., trade name: PX700) at a set pressure M, thereby adjusting the sample for measurement. If the surface of the filler pressed by the forming machine was not smooth, it was manually smoothed before measurement. After irradiating the sample with X-rays and performing baseline correction, the peak intensity ratio of the (002) plane to the (100) plane of boron nitride was calculated, and the orientation index [I(002) / I(100)] was determined based on this value.
[0107] The purity of boron nitride powder was determined by the following method. First, the boron nitride powder was decomposed using sodium hydroxide, and ammonia was distilled from the decomposition solution using steam distillation and collected in an aqueous boric acid solution. The collected solution was then titrated using a standard sulfuric acid solution. Based on the titration results, the nitrogen (N) content in the boron nitride powder was calculated. Based on the obtained nitrogen content, the boron nitride content in the boron nitride powder was determined according to equation (1), and the purity of the boron nitride powder was calculated. It should be noted that the formula weight of boron nitride was 24.818 g / mol, and the atomic weight of nitrogen was 14.006 g / mol.
[0108] The boron nitride (BN) content [mass%] in boron nitride powder = the nitrogen atom (N) content [mass%] × 1.772…(1)
[0109] The average particle size of the boron nitride powder was determined according to ISO 13320:2009 using a laser diffraction scattering particle size distribution measuring apparatus (apparatus name: LS-13 320) manufactured by Beckman Coulter. It should be noted that the boron nitride powder was not homogenized. For the particle size distribution determination, water was used as the solvent for dispersing the boron nitride powder, and hexametaphosphate was used as the dispersant. The refractive index of water was 1.33, and the refractive index of the boron nitride powder was 1.80.
[0110] The crushing strength of aggregated particles was determined according to JIS R 1639-5:2007 "Fine ceramics - Determination of particle characteristics - Part 5: Crushing strength of a single particle". A micro-compression testing machine (manufactured by Shimadzu Corporation, product name "MCT-W500") was used for the test. It should be noted that the test was performed on 20 or more aggregated particles, and the value was calculated when the cumulative crushing rate was 63.2%.
[0111] <Examples 2-4>
[0112] The firing temperature and / or firing time in the decarburization crystallization process were changed as shown in Table 1. Otherwise, boron nitride powders of Examples 2 to 4 were obtained in the same manner as in Example 1. In addition, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured in the same manner as in Example 1. The results are shown in Table 1.
[0113] <Example 5>
[0114] The boron nitride powder of Example 5 was obtained by grinding the boron nitride powder using a ball mill for 100 minutes at 100 rpm, followed by subsequent classification using a vibrating sieve with a mesh size of 34 μm, and then further classification after crushing using a sieve with a mesh size of 45 μm. Otherwise, the process was the same as in Example 1. Furthermore, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured as in Example 1. The results are shown in Table 1.
[0115] <Comparative Examples 1-2>
[0116] The amounts of boric acid and sodium carbonate used in the decarburization crystallization process (based on the total mass of the raw material mixture) were changed to the values shown in Table 1. Otherwise, boron nitride powders for Comparative Examples 1 and 2 were obtained in the same manner as in Example 1. Furthermore, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured in the same manner as in Example 1. The results are shown in Table 1.
[0117] [Table 1]
[0118]
[0119] <Example 6>
[0120] [Acid treatment process]
[0121] Acid treatment was performed on the boron carbide powder prepared in the same manner as in Example 1. Specifically, firstly, boron carbide powder prepared in the same manner as in Example 1 was prepared. Next, an acid solution was prepared by mixing a hydrofluoric acid solution and a hydrochloric acid solution. The acid concentration of the acid solution was 40% by mass, and the mass ratio of hydrofluoric acid to hydrochloric acid (HF to HCl mass ratio) in the acid solution was 1:1 (i.e., the concentrations of both hydrofluoric acid and hydrochloric acid in the acid solution were 20% by mass). Next, the acid solution was heated and maintained at 80°C, and boron carbide powder was added to it and stirred at 80°C for 5 hours. This brought the boron carbide powder into contact with the acid solution, thus performing acid treatment on the boron carbide powder. The operation of stirring, decantation, and adding new acid solution for acid treatment was repeated 15 times. Then, the slurry was dried to obtain acid-treated boron carbide powder. The average particle size and purity of the obtained boron carbide powder were measured by the method described in Example 1, and the results showed that the average particle size was 20 μm and the purity was 99% by mass.
[0122] Next, using the acid-treated boron carbide powder described above as boron carbide powder, the pressure nitriding and decarburization crystallization processes were performed in the same manner as in Example 1 to obtain the boron nitride powder of Example 6. Furthermore, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured in the same manner as in Example 1. The results are shown in Table 2.
[0123] <Example 7>
[0124] The firing temperature and firing time in the decarburization crystallization process were modified as shown in Table 2. Otherwise, the boron nitride powder of Example 7 was obtained in the same manner as in Example 6. Furthermore, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured in the same manner as in Example 1. The results are shown in Table 2.
[0125] <Example 8>
[0126] The concentration of the acid solution, the treatment temperature (temperature of the mixture of boron carbide powder and acid solution), and the treatment time (stirring time) in the acid treatment process were changed to the values shown in Table 2. Otherwise, boron nitride powder of Example 8 was obtained in the same manner as in Example 7. Furthermore, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured in the same manner as in Example 1. The results are shown in Table 2. It should be noted that, similar to the analysis of uranium, the thorium content was 4 ppb by mass.
[0127] <Example 9>
[0128] The concentration of the acid solution, the formulation of the acid solution, the treatment temperature (temperature of the mixture of boron carbide powder and acid solution), and the treatment time (stirring time) in the acid treatment process were changed to the values shown in Table 2. Otherwise, boron nitride powder of Example 9 was obtained in the same manner as in Example 6. Furthermore, the uranium content, orientation index, purity, average particle size, and crushing strength of aggregated particles in the boron nitride powder were measured in the same manner as in Example 1. The results are shown in Table 2.
[0129] [Table 2]
[0130]
Claims
1. A method for manufacturing boron nitride powder, comprising a decarburization and crystallization step, wherein primary boron nitride particles are generated by calcining a raw material mixture comprising boron carbonitride powder, a boron source, and a carbonate, thereby obtaining powder comprising aggregated particles composed of said primary particles. In the decarbonization crystallization process, based on the total mass of the raw material mixture, the amount of boron source used is 55% by mass or more, and based on the total mass of the raw material mixture, the amount of carbonate used is 4% by mass or more.
2. The method for manufacturing boron nitride powder as described in claim 1, wherein, The firing temperature in the decarburization and crystallization process is above 1800℃, and the firing time is above 8 hours.
3. The method for manufacturing boron nitride powder as described in claim 1, wherein, The firing temperature in the decarburization and crystallization process is above 2000℃, and the firing time is above 4 hours.
4. The method for manufacturing boron nitride powder according to any one of claims 1 to 3, further comprising a preparation step for preparing the boron carbonitride powder. The preparation process includes: An acid treatment process in which a boron carbide powder is contacted with an acid solution containing hydrofluoric acid to perform acid treatment on the boron carbide powder; and a pressure nitriding process in which the acid-treated boron carbide powder is sintered under a nitrogen pressure atmosphere.
5. The method for manufacturing boron nitride powder as described in claim 4, wherein, The acid solution is a mixed acid containing the hydrofluoric acid. Hydrofluoric acid accounts for more than 10% by mass of all acid components in the mixed acid.
6. The method for manufacturing boron nitride powder as described in claim 4, wherein, The acid treatment process is carried out at a temperature of 60°C or higher. The acid treatment process takes more than 3 hours. The acid concentration of the acid solution is 20% by mass or more.
7. Boron nitride powder, comprising aggregated particles formed by the aggregation of primary boron nitride particles. The orientation index of the boron nitride powder is below 15. The uranium content is between 1 ppb and 20 ppb.
8. The boron nitride powder as described in claim 7, having a purity of 98.5% by mass or higher and an average particle size of 10–90 μm. The crushing strength of the aggregated particles is above 5 MPa.
9. A resin sealing material for semiconductor memory elements, comprising the boron nitride powder as described in claim 7 or 8.
Citation Information
Patent Citations
Boron nitride aggregated particle, method for producing boron nitride aggregated particle, resin composition containing boron nitride aggregated particle, and molding
JP2016135731A
Aggregate boron nitride particles, boron nitride powder, production method for boron nitride powder, resin composition, and heat dissipation member
CN112334408A
Curable resin composition, dry film, cured product and printed wiring board
JP2017125173A