A catalytic wet oxidation catalyst, its preparation method and use
By doping noble metals with oxygen-storing metal oxides to form oxidation active sites, and doping the support and support additives to form acidic sites, a catalyst capable of catalytically oxidizing both organic matter and ammonia nitrogen was prepared. This solved the problem of the difficulty in simultaneously treating organic matter and ammonia nitrogen in existing technologies, and achieved a highly efficient wastewater treatment effect.
Patent Information
- Application Number
- CN202410681945.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-05-29
AI Technical Summary
Existing catalytic wet oxidation catalysts struggle to balance the performance of catalytic oxidation of organic matter and ammonia nitrogen when treating wastewater containing both organic pollutants and ammonia nitrogen, and there is a risk of excessive oxidation of nitrogen oxides.
A catalyst with oxygen storage and ammonia nitrogen adsorption capabilities was prepared by doping noble metals and oxygen-storing metal oxides to form oxidation active sites, and doping the support and support additives to form acidic sites. By rationally controlling the synergistic effect of the active sites, the catalyst can simultaneously remove organic matter and ammonia nitrogen through catalytic oxidation.
When treating high-concentration organic and ammonia nitrogen wastewater, the catalyst achieves a COD removal rate of over 92%, an ammonia nitrogen removal rate of over 96%, and an N₂ selectivity of over 95%, effectively preventing the generation of nitrogen oxides and possessing the potential for large-scale industrial application.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of environmental protection technology, and in particular relates to a catalytic wet oxidation catalyst, its preparation method and application. Background Technology
[0002] Catalytic wet oxidation technology is an advanced method for treating high-concentration organic industrial wastewater. This method uses precious metals (such as Au, Rh, Pd, Ru, etc.) as catalysts and air, oxygen, ozone, etc., as oxidants to oxidize and decompose pollutants such as organic matter and ammonia nitrogen in high-concentration organic wastewater into carbon dioxide and nitrogen gas in a single step, thereby enabling the wastewater to meet discharge standards or significantly improving its biodegradability. Regarding catalyst performance, for the removal of organic matter, the stronger the catalytic oxidation capacity of the catalyst, the better; however, for the removal of ammonia nitrogen, the catalyst's oxidation capacity must be moderate to avoid excessive oxidation of ammonia nitrogen, leading to the generation of nitrogen oxides and causing secondary pollution. Therefore, for wastewater containing both organic pollutants and ammonia nitrogen, the design and preparation of catalytic wet oxidation catalysts must comprehensively and rationally control the catalyst's catalytic oxidation capacity to balance the performance of catalytic oxidation of organic matter and catalytic oxidation of ammonia nitrogen. Patents CN112607905A and CN105709733B reported catalysts for the wet oxidation of organic matter or ammonia nitrogen on their own, while patent CN 109465008 B reported a catalyst for the simultaneous removal of organic matter and ammonia nitrogen. However, the oxygen storage capacity and acid site strength of the catalysts were not clearly defined.
[0003] In view of this, the present invention is hereby proposed. Summary of the Invention
[0004] The purpose of this invention is to provide a catalytic wet oxidation catalyst, its preparation method, and its application, in order to solve the above-mentioned problems.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] A catalytic wet oxidation catalyst includes a support, a support promoter, a noble metal, and an oxygen storage metal oxide;
[0007] The noble metal is doped with oxygen-storing metal oxide to form oxidation active sites;
[0008] The carrier and carrier additives are doped to form acidic sites.
[0009] Optionally, the noble metal includes any one or more of Pt, Ru, and Ag; the oxygen storage metal includes any one or more of Mn, Ti, and Ce; the support includes Al2O3; and the support additive includes MgO and / or ZrO2.
[0010] Pretreatment with noble metals and oxygen-storing metals such as Mn, Ti, and Ce can generate oxygen vacancies, providing oxygen storage capacity for the catalyst and thus enabling it to catalyze oxidation. Doping between the oxide support Al2O3 and the support promoter MgO or ZrO2 can form a solid acid, giving the catalyst the ability to adsorb NH4+. 4+ The ability to catalyze the oxidation of ammonia nitrogen is enhanced by the rational regulation and synergistic effect of the two active sites. This allows the catalyst to have oxygen storage capacity and ammonia nitrogen adsorption capacity, as well as the ability to catalyze the wet oxidation of organic matter and ammonia nitrogen.
[0011] Optionally, by weight, the noble metal in the catalyst accounts for 0.1-0.5 wt%, the oxygen storage metal accounts for 10.8-15.6 wt%, and the support and support promoter together account for 83.9-89.1 wt%; preferably, the mass ratio of the support to the support promoter is 4.1:1.0-1.2. According to the preferred formulation of the present invention, the oxygen storage capacity of the catalyst is between 320-650 μmol / g, and the acidic site concentration is between 5.3-12.8 μmol / g.
[0012] A method for preparing the aforementioned catalytic wet oxidation catalyst includes:
[0013] The carrier precursor compound and the carrier auxiliary agent precursor compound are dissolved in water to form solution one;
[0014] Ammonia was added to solution one to form a precipitate, which was then filtered and washed to obtain sample one.
[0015] The noble metal compound and the oxygen-storing metal compound are dissolved in water to form solution two;
[0016] The sample one was added to the solution two, and then ammonia was added to the system to form a precipitate. The precipitate was then filtered, washed, allowed to stand, dried and calcined to obtain the sample two.
[0017] The second sample was pretreated by heating in an H2 / N2 atmosphere and then cooled to room temperature to obtain the final sample.
[0018] The concentration of ammonia water is preferably 25%. Adding 25% ammonia water to a solution or suspension as a precipitant is more conducive to the efficient formation of precipitates.
[0019] Optionally, the carrier precursor compound is aluminum nitrate, and the carrier auxiliary agent precursor compound is magnesium nitrate and / or zirconium nitrate;
[0020] The noble metal compound is any one or more of chloroplatinic acid, ruthenium trichloride, and silver nitrate;
[0021] The oxygen-storing metal compound is any one or more of manganese nitrate, titanium oxysulfate, and cerium nitrate.
[0022] Optionally, the mass ratio of the carrier precursor compound to the carrier auxiliary precursor compound is 17.2:(3.2-6.4). Only when the preferred ratio of the carrier precursor compound to the carrier auxiliary precursor compound is met can the two metal oxides be fully doped to form a suitable concentration of acidic sites. Deviating from this ratio will result in an excessively low or high concentration of acidic sites, thereby affecting the overall performance of the catalyst.
[0023] Optionally, the mass ratio of the noble metal compound to the oxygen storage metal compound is (0.2-1.6):(17.0-51.6). Only by satisfying the ratio of the noble metal compound to the oxygen storage metal compound provided by this invention can the noble metal and the oxygen storage metal be fully doped; deviations from this ratio will result in ineffective doping of the noble metal and the oxygen storage metal.
[0024] Optionally, the preparation method satisfies one or more of the following conditions:
[0025] a. The settling time is 2-5 hours;
[0026] b. The drying process involves multiple drying cycles;
[0027] c. The multiple drying processes are drying at 30-50℃ for 2-5 hours and drying at 100-120℃ for 6-12 hours. Multiple drying conditions are preferred. Single drying or drying outside the temperature or time range provided by this invention will cause uneven distribution of active components and catalyst cracking during the drying process, affecting the subsequent preparation effect and even affecting the catalyst performance.
[0028] d. The calcination is carried out at 400-600℃ in air for 4-6 hours. The calcination conditions are preferred; exceeding these ranges may result in incomplete decomposition of the metal compound or aggregation of the metal oxide particles formed during calcination.
[0029] Furthermore, the preparation method also satisfies one or more of the following conditions:
[0030] e, the H2 / N2 concentration is 0.5-1.5%;
[0031] f, the H2 / N2 space velocity is 500-800 h. -1 ;
[0032] g, wherein the heating rate is 0.5-1.5℃ / min, and the target temperature is 300-500℃;
[0033] The preprocessing time is 3-5 hours.
[0034] The pretreatment conditions provided by this invention are preferred conditions for effectively pretreating metal oxides to increase oxygen vacancies. Exceeding the above pretreatment conditions will result in insufficient or excessive oxygen vacancies. The former will result in insufficient oxidation capacity of the catalyst, or excessive oxidation capacity, which will over-oxidize ammonia nitrogen into nitrogen oxides.
[0035] The present invention also provides an application of the aforementioned catalytic wet oxidation catalyst for the simultaneous removal of organic pollutants and ammonia nitrogen from wastewater.
[0036] The catalyst was placed in a fixed-bed reactor and subjected to an air space velocity of 200-500 h⁻¹. -1 Under a pressure of 4.0-8.0 MPa, the temperature is increased to the reaction temperature of 200-250℃ at a rate of 0.5-2.0℃ / min. Organic wastewater with a COD concentration of 20000-40000 mg / L and an ammonia nitrogen concentration of 3000-6000 mg / L is then reacted at a liquid hourly space velocity (LHSV) of 1.0-3.0. h-1 The feed is then introduced to initiate the reaction.
[0037] Compared with existing technologies, this invention creatively introduces acidic sites into the catalyst support and oxygen storage properties into the active sites of the catalyst, thereby enabling the catalyst to simultaneously possess the ability to catalyze the oxidation of organic matter and nitrogen. The provided catalyst can oxidize organic matter into carbon dioxide and ammonia nitrogen into nitrogen gas without excessive oxidation into nitrogen oxides, and has an excellent treatment effect on high-concentration organic and ammonia nitrogen wastewater.
[0038] The preparation method provided by this invention is simple to operate, has controllable conditions, and has the potential for large-scale industrial application.
[0039] When the catalyst provided by this invention is applied to the treatment of organic wastewater, it has the ability to catalyze the wet oxidation of organic matter and ammonia nitrogen. Experimental results show that when treating organic wastewater, the COD removal rate is greater than 92%, the ammonia nitrogen removal rate is greater than 96%, and the N2 selectivity is greater than 95%. Detailed Implementation
[0040] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0041] Example 1
[0042] The catalytic wet oxidation catalyst prepared according to the preparation method provided by the present invention comprises the following specific steps:
[0043] S1: Add 17.2g aluminum nitrate and 3.2g zirconium nitrate to 100ml deionized water to form solution one;
[0044] S2: Add 25% ammonia water as a precipitant to solution one to form a precipitate. Filter and wash the precipitate to obtain sample one.
[0045] S3: Add 0.2g of chloroplatinic acid and 20.6g of cerium nitrate to 100ml of deionized water to form solution two;
[0046] S4: Add the sample one obtained in S2 to the solution two obtained in S3 to form a suspension. Add 25% ammonia water as a precipitant to the suspension to form a precipitate. Wash the precipitate and let it stand at room temperature for 5 hours.
[0047] S5: First, dry the product obtained from S4 at 30℃ for 2 hours, and then dry it at 110℃ for 6 hours;
[0048] S6: The product obtained in S5 was calcined at 500℃ for 5 hours to obtain sample two;
[0049] S7: Sample 2 obtained in S6 was heated to 300℃ at a rate of 0.5℃ / min under an H2 / N2 atmosphere and pretreated at this temperature for 5h. The H2 / N2 space velocity was 700h. -1 .
[0050] The prepared catalyst contained 0.1 wt% Pt, 12.3 wt% CeO2, and 87.6 wt% support and support promoters, with an Al2O3 to ZrO2 mass ratio of 4.1:1.0. The catalyst had an oxygen storage capacity of 420 μmol / g and an acidic site concentration of 10.5 μmol / g.
[0051] Example 2
[0052] The difference from Example 1 is that the amount of zirconium nitrate used in step S1 is 6.4g.
[0053] Example 3
[0054] The difference from Example 1 is that the amount of cerium nitrate used in step S3 is 50.0g.
[0055] Example 4
[0056] The difference from Example 1 is that in step S5, the product obtained in S4 is first dried at 50°C for 3 hours, and then dried at 120°C for 10 hours.
[0057] Example 5
[0058] The difference from Example 1 is that in step S5, the product obtained in S4 is first dried at 40°C for 5 hours, and then dried at 110°C for 12 hours.
[0059] Example 6
[0060] The difference from Example 1 is that in step S5, the product obtained in S4 is first dried at 30°C for 5 hours, and then dried at 100°C for 6 hours.
[0061] Comparative Example 1
[0062] The difference from Example 1 is that step S5 drying is done only once, at a temperature of 110°C, for a time of 8 hours.
[0063] Comparative Example 2
[0064] The difference from Example 1 is that step S5 drying is done only once, at a temperature of 60°C for 8 hours.
[0065] Comparative Example 3
[0066] The difference from Example 1 is that the amount of cerium nitrate used in step S3 is 70.0g.
[0067] Comparative Example 4
[0068] The difference from Example 1 is that the amount of zirconium nitrate used in step S1 is 1.0g.
[0069] Performance testing:
[0070] The catalysts prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests. The test conditions were as follows: 4 ml of catalyst was placed in a fixed-bed reactor and subjected to an air space velocity of 200 h⁻¹. -1 Under a pressure of 6.0 MPa, the temperature was increased to 230℃ at a rate of 1.0℃ / min. Organic wastewater with a COD concentration of 25000 mg / L and an ammonia nitrogen concentration of 3500 mg / L was then reacted at a liquid hourly space velocity (LHSV) of 2.0 h⁻¹. -1 The feed was used for the reaction. The test results are shown in Table 1 below:
[0071] Table 1. Performance test results of the catalysts prepared in Examples 1-3 and Comparative Examples 1-4
[0072]
[0073]
[0074] As can be seen from Examples 1-6, the catalyst obtained according to the preparation method and preferred parameters provided by the present invention has a COD removal rate of greater than 92%, an ammonia nitrogen removal rate of greater than 96%, and an N2 selectivity of greater than 95% when treating organic wastewater, and its overall performance is better.
[0075] A comparison of Example 1 and Comparative Examples 1 and 2 shows that the drying temperature, number of drying cycles, and drying time all affect the catalyst's performance. Clearly, the preferred drying conditions of this invention are more conducive to the uniform distribution of the active components, significantly improving the catalyst's catalytic performance. Furthermore, the results of Examples 4-6 and Comparative Examples 1-2 also demonstrate that the preferred drying method of this invention achieves better technical results.
[0076] A comparison of Example 1 and Comparative Example 3 reveals that the ratio of noble metal to oxygen storage metal is crucial. In Example 1, under the ratio conditions provided by this invention, both noble metal and oxygen storage metal were effectively doped, resulting in a catalyst with abundant oxidation active sites. This enhanced the catalyst's catalytic oxidation capacity, leading to a higher COD removal rate. In contrast, the ratio of noble metal to oxygen storage metal in Comparative Example 3 was unsuitable, failing to achieve effective doping and thus affecting oxygen defect formation, further impacting the catalytic oxidation capacity.
[0077] By comparing Example 1 and Comparative Example 4, it can be seen that the ratio of the support precursor compound to the support auxiliary precursor compound in Example 1 meets the preferred ratio of the present invention, and the two metal oxides are fully doped to form a suitable concentration of acidic sites, resulting in a catalyst with a higher ammonia nitrogen removal rate. Comparative Example 4 deviates from this ratio, resulting in an unsuitable concentration of acidic sites, thus affecting the overall performance of the catalyst.
[0078] Please note that the technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments have been described. However, as long as the combination of these technical features does not contradict each other, it should be considered within the scope of this specification. The above embodiments only illustrate several implementation methods of this application, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the invention patent. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A method for preparing a catalytic wet oxidation catalyst, characterized in that, The catalyst includes a support, a support additive, a noble metal, and an oxygen storage metal oxide; The noble metal is doped with oxygen-storing metal oxide to form oxidation active sites; The carrier and carrier additives are doped to form acidic sites; The precious metals include any one or more of Pt, Ru, and Ag; The oxygen storage metal includes any one or more of Mn, Ti, and Ce; The carrier includes Al2O3; The carrier additives include MgO and / or ZrO2; By weight, the catalyst contains 0.1-0.5 wt% of the noble metal, 10.8-15.6 wt% of the oxygen storage metal, and the support and support additives together account for 83.9-89.1 wt%. The mass ratio of the carrier to the carrier additive is 4.1:1.0-1.2; The preparation method includes: The carrier precursor compound and the carrier auxiliary agent precursor compound are dissolved in water to form solution one; Ammonia was added to solution one to form a precipitate, which was then filtered and washed to obtain sample one. The noble metal compound and the oxygen-storing metal compound are dissolved in water to form solution two; The sample one was added to the solution two, and then ammonia was added to the system to form a precipitate. The precipitate was then filtered, washed, allowed to stand, dried and calcined to obtain the sample two. The second sample was pretreated by heating in an H2 / N2 atmosphere and then cooled to room temperature to obtain the final sample. The mass ratio of the carrier precursor compound to the carrier auxiliary agent precursor compound is 17.2:(3.2-6.4). The mass ratio of the noble metal compound to the oxygen storage metal compound is (0.2-1.6):(17.0-51.6).
2. The preparation method according to claim 1, characterized in that, The carrier precursor compound is aluminum nitrate, and the carrier auxiliary agent precursor compound is magnesium nitrate and / or zirconium nitrate; The noble metal compound is any one or more of chloroplatinic acid, ruthenium trichloride, and silver nitrate; The oxygen-storing metal compound is any one or more of manganese nitrate, titanium oxysulfate, and cerium nitrate.
3. The preparation method according to claim 1, characterized in that, The preparation method satisfies one or more of the following conditions: a. The settling time is 2-5 hours; b. The drying process involves multiple drying cycles; c. The multiple drying processes are drying at 30-50℃ for 2-5 hours and drying at 100-120℃ for 6-12 hours. d. The calcination is carried out at 400-600℃ for 4-6 hours in an air atmosphere.
4. The preparation method according to any one of claims 1-3, characterized in that, The preparation method also satisfies one or more of the following conditions: e, the H2 / N2 concentration is 0.5-1.5%; f, the H2 / N2 space velocity is 500-800 h. -1 ; g, wherein the heating rate is 0.5-1.5℃ / min, and the target temperature is 300-500℃; The preprocessing time is 3-5 hours.
5. The application of a catalytic wet oxidation catalyst prepared by the method described in any one of claims 1-4, characterized in that, It is used to remove organic pollutants and ammonia nitrogen from wastewater simultaneously.
Citation Information
Patent Citations
A noble metal catalyst for catalytic wet oxidation and its preparation method
CN105709733B
A catalytic wet oxidation catalyst, its preparation method and application
CN109465008B
Method for removing total nitrogen in organic nitrogen wastewater
CN112607905A
Catalytic wet oxidation catalyst as well as preparation method and application thereof
CN116371404A