High-efficiency bifunctional material for carbon capture and in-situ conversion, and preparation method and application thereof
By preparing CeO₂-NiFe-CaO bifunctional materials, the problems of high energy consumption and low product yield in in-situ capture and conversion of calcium oxide were solved, achieving efficient CO₂ capture and conversion to CO, and reducing energy consumption and cost.
Patent Information
- Application Number
- CN202410807506.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Existing technologies using calcium oxide for in-situ carbon capture and conversion suffer from high energy consumption and low product yield.
A bifunctional CeO₂-NiFe-CaO material was prepared by dispersing cerium salt and nickel ferrite in a solvent, heating at high temperature, mixing with calcium hydroxide, calcining and reducing. The synergistic effect of calcium oxide and cerium oxide-nickel alloy was utilized to promote carbonate activation and catalyze carbonate hydrogenation reaction.
This technology enables efficient capture of CO₂ and in-situ conversion into high-value-added CO, reducing adsorbent regeneration energy consumption and CO₂ compression and transportation costs, and improving the economic and environmental feasibility of carbon capture and utilization.
Smart Images

Figure CN118719075B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of carbon capture and in-situ conversion technology, and particularly relates to a highly efficient bifunctional material for achieving carbon capture and in-situ conversion, its preparation method and application. Background Technology
[0002] With the rapid advancement of global industrialization, the consumption of fossil fuels has increased dramatically, leading to excessive emissions of the greenhouse gas carbon dioxide and causing environmental problems such as the greenhouse effect and ocean acidification. These increasingly serious environmental issues have made CO2 capture and utilization a key area of discussion. Traditional CO2 capture and conversion technologies are mostly distributed, resulting in high CO2 transportation costs and high energy consumption for regeneration and conversion. To reduce the cost and energy consumption of carbon capture and utilization, carbon capture and in-situ conversion technology has emerged. This technology utilizes bifunctional materials to achieve CO2 capture and in-situ conversion by simply adjusting the reaction atmosphere, reducing compression transportation costs and related equipment, and possessing higher environmental and economic feasibility.
[0003] The reverse water gas conversion reaction (RWGS reaction) can convert CO2 captured from flue gas into CO. At the same time, by adjusting the H2 concentration, the syngas with different CO:H2 ratios can be used as raw materials for the Fischer-Tropsch reaction, and further converted into high-value-added chemical products.
[0004] The reverse water-gas conversion reaction typically occurs at high reaction temperatures, making it well-suited for carbon capture by calcium oxide adsorption. Calcium oxide is abundant, inexpensive, and exhibits rapid adsorption kinetics and high carbon capture capacity. However, due to the high activation temperature of calcium carbonate, using calcium oxide alone for in-situ capture and conversion results in high energy consumption and low product yield. Therefore, it is necessary to screen for catalytic components that are stable and active under high-temperature reducing atmospheres to promote carbonate activation, prepare highly efficient bifunctional materials, improve in-situ capture and conversion efficiency, and reduce reaction energy consumption. Summary of the Invention
[0005] Purpose of the invention: This invention provides a highly efficient bifunctional material for carbon capture and in-situ conversion, its preparation method and application, to solve the problems of high energy consumption and low product yield when using calcium oxide for in-situ capture and conversion.
[0006] Summary of the Invention: To achieve the above objectives, this invention provides a method for preparing a highly efficient bifunctional material that realizes carbon capture and in-situ conversion, the preparation method comprising:
[0007] Cerium salt and nickel ferrite are dispersed in a solvent, mixed evenly, and then heated to a solid state at high temperature. The resulting cerium oxide-nickel ferrite is ground and mixed with calcium hydroxide and calcined at high temperature. After reduction, a bifunctional material is obtained. The bifunctional material is composed of CeO2-NiFe-CaO, wherein the mass ratio of CaO to CeO2-NiFe is 4:1 to 19:1.
[0008] Under normal circumstances, the final CeO2-NiFe-CaO bifunctional material is a gray solid.
[0009] Compared to single-component catalysts, composite catalysts often exhibit superior activity and stability in CO2 hydrogenation. Fe-based catalysts show great potential in RWGS reactions due to their excellent oxygen mobility. However, during CO2 hydrogenation, Fe-based catalysts may develop carbon deposits, hindering the adsorption and activation of H2 and CO2, leading to catalyst deactivation. Therefore, it is necessary to improve the high-temperature CO2 hydrogenation stability of Fe-based catalysts by adjusting the catalyst structure and introducing other substances. Ni, due to its excellent H2 activation performance, can effectively lower the temperature required for RWGS reactions and is therefore widely used in CO2 hydrogenation research. Compared to single Fe or Ni metals, Fe-Ni alloys have higher metal dispersion, smaller particle size, stronger metal-support interactions, and more electron-rich Ni states, which facilitate CO2 adsorption and conversion, effectively improving RWGS reaction performance. Cerium oxide possesses excellent oxygen exchange capacity and anti-sintering properties; its internal oxidized Ce... 3+ and Ce 4+ Ions can exist stably and interconvert, allowing CeO2 to release or absorb O atoms, and it is often used to catalyze reverse water-gas shift reactions. Therefore, introducing CeO2 to modify Fe-Ni alloys and using iron-nickel alloy-cerium oxide support composite materials as catalytic components can effectively improve the in-situ capture-conversion performance and cycle reaction stability of the ICCC-RWGS process.
[0010] Optionally, the cerium salt is cerium nitrate hexahydrate. Cerium nitrate is chosen because the cerium oxide-nickel ferrite formed from this precursor exhibits optimal catalytic performance.
[0011] Optionally, the solvent, as a dispersant, can be selected from methanol, ethanol, and propanol.
[0012] Optionally, the cerium salt and nickel ferrite are mixed evenly in a solvent and then stirred and heated at 300-500°C until solid.
[0013] The purpose of limiting the heating temperature is to ensure that the cerium salt is fully pyrolyzed and that the CeO2 particle size is kept small. When the heating temperature is too high, the resulting CeO2 support particles are too large, affecting the loading effect of the CeO2 support; when the heating temperature is too low, the cerium salt precursor cannot be fully pyrolyzed.
[0014] Optionally, the mass ratio of cerium oxide-nickel ferrite to calcium hydroxide is from 0.036 g:1 g to 0.144 g:1 g.
[0015] The purpose of limiting this mass ratio is to control the interfacial effect and framework support between the catalytic component and calcium oxide. If the ratio is too small, excessive calcium oxide is prone to agglomeration and sintering at high temperatures, causing deactivation of the bifunctional material; if the ratio is too large, it can easily lead to a decrease in adsorption capacity.
[0016] Optionally, the calcination temperature is 500-700℃, the time is 8-15 min, and the calcination atmosphere is N2 with a volume percentage of more than 99%.
[0017] The purpose of limiting the calcination temperature and time is to ensure that calcium hydroxide pyrolyzes to form calcium oxide and maintains the dispersion of catalytic components. When the calcination temperature is too high or the time is too long, the adverse effect is that calcium oxide and the cerium oxide-nickel ferrite composite material agglomerate and sinter, causing the active sites to be covered, thus affecting the formation of the adsorption-catalytic component interface effect and consequently impacting the capture and conversion performance of the bifunctional material. When the calcination temperature is too low or the time is too short, the adverse effect is that calcium hydroxide cannot be fully pyrolyzed to calcium oxide, causing a decrease in CO2 adsorption capacity.
[0018] Optionally, the reduction temperature is 500-700℃, the time is 8-15 min, and the reduction atmosphere is H2 / N2 with a volume ratio of 10%:90%.
[0019] The purpose of limiting the reduction temperature and time is to ensure that the precursor NiFe2O4 is fully reduced to the active Fe-Ni alloy and to maintain the dispersion of the catalytic components. When the pre-reduction temperature is too high or the time is too long, the adverse effect is the agglomeration and sintering of the calcium oxide and cerium oxide-nickel ferrite composite materials. When the pre-reduction temperature is too low or the time is too short, the NiFe2O4 precursor cannot be effectively reduced to the active Fe-Ni alloy during the synthesis process, reducing the CO2 hydrogenation conversion activity of the catalytic components.
[0020] Furthermore, the highly efficient bifunctional material prepared by the above method is applied to in-situ CO2 capture and conversion reactions, specifically integrating CO2 capture and reverse water gas conversion reactions to achieve efficient CO2 capture and in-situ hydrogenation conversion to CO.
[0021] Beneficial effects: The highly efficient bifunctional material for carbon capture and in-situ conversion, its preparation method, and its application provided by this invention have the following advantages compared with the prior art:
[0022] This invention disperses cerium salt and nickel ferrite in ethanol, mixes and heats thoroughly, and then grinds and mixes the resulting cerium oxide-nickel ferrite with calcium hydroxide. After high-temperature calcination and reduction, a bifunctional material with the composition CeO2-NiFe-CaO is obtained. Through the synergistic effect of calcium oxide and cerium oxide-nickel alloy, it achieves efficient and stable promotion of carbonate activation and catalytic hydrogenation of carbonate to CO under high-temperature conditions.
[0023] The bifunctional material prepared by this invention exhibits high CO2 adsorption capacity and product yield, thereby achieving efficient CO2 capture and in-situ conversion into high-value-added CO. This saves energy consumption for adsorbent regeneration and CO2 compression and transportation costs, promoting carbon dioxide emission reduction and economic utilization. Furthermore, the preparation method provided by this invention is simple, easy to operate, uses widely available raw materials, and has low cost. Attached Figure Description
[0024] Figure 1 This is a flowchart illustrating the preparation process of the bifunctional material in this embodiment of the invention.
[0025] Figure 2 The XRD patterns of the bifunctional material in Example 3 of this invention before and after the reduction reaction are shown.
[0026] Figures 3a-3b All figures are test results of the cyclic capture and conversion performance of the bifunctional materials in Examples 1-4 of this invention. Detailed Implementation
[0027] To make the technical solutions of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0028] Reference Figure 1 This invention provides a highly efficient bifunctional material that achieves carbon capture and in-situ conversion, and its preparation method is as follows:
[0029] Cerium salt and nickel ferrite are dispersed in ethanol solvent, mixed evenly, and heated to solid state at high temperature. The resulting cerium oxide-nickel ferrite is ground and mixed with calcium hydroxide and calcined at high temperature. After reduction, a bifunctional material is obtained. The composition of the bifunctional material is CeO2-NiFe-CaO, wherein the mass ratio of CaO to CeO2-NiFe is 4:1 to 19:1.
[0030] The high-efficiency bifunctional material prepared by the above method can be applied to in-situ CO2 capture and conversion reactions, specifically integrating CO2 capture and reverse water gas conversion reactions to achieve efficient CO2 capture and in-situ hydrogenation conversion to CO.
[0031] Example 1:
[0032] The mass-to-volume ratio of cerium oxide-nickel ferrite to calcium hydroxide was selected as 0.036 g: 1 g;
[0033] Cerium nitrate hexahydrate and nickel ferrite were mixed evenly in ethanol solvent and then heated and stirred at 400℃ until solid. The resulting black solid was mixed with calcium hydroxide and ground. Then, it was calcined in a 99.9% N2 atmosphere at 600℃ for 10 min. Finally, it was reduced at 600℃ for 10 min in a 10%:90% H2 / N2 atmosphere to obtain the CeO2-NiFe-CaO bifunctional material, denoted as 5CNF-CaO.
[0034] Example 2:
[0035] The mass-to-volume ratio of cerium oxide-nickel ferrite to calcium hydroxide was selected as 0.072 g: 1 g;
[0036] Cerium nitrate hexahydrate and nickel ferrite were mixed evenly in ethanol solvent and heated to solidify at 400℃. The resulting black solid was mixed with calcium hydroxide and ground. Then, it was calcined at 600℃ for 10 min under a 99.9% N2 atmosphere. Finally, it was reduced at 600℃ for 10 min under a 10%:90% H2 / N2 atmosphere to obtain the CeO2-NiFe-CaO bifunctional material, denoted as 10CNF-CaO.
[0037] Example 3:
[0038] The mass-to-volume ratio of cerium oxide-nickel ferrite to calcium hydroxide is selected as 0.108 g: 1 g;
[0039] Cerium nitrate hexahydrate and nickel ferrite were mixed evenly in ethanol solvent and then heated and stirred at 400℃ until solid. The resulting black solid was mixed with calcium hydroxide and ground. Then, it was calcined in a 99.9% N2 atmosphere at 600℃ for 10 min. Finally, it was reduced at 600℃ for 10 min in a 10%:90% H2 / N2 atmosphere to obtain the CeO2-NiFe-CaO bifunctional material, denoted as 15CNF-CaO.
[0040] Example 4:
[0041] The mass-to-volume ratio of cerium oxide-nickel ferrite to calcium hydroxide was selected as 0.144 g: 1 g;
[0042] Cerium nitrate hexahydrate and nickel ferrite were mixed evenly in ethanol solvent and heated to solidify at 400℃. The resulting black solid was mixed with calcium hydroxide and ground. Then, it was calcined at 600℃ for 10 min under a 99.9% N2 atmosphere. Finally, it was reduced at 600℃ for 10 min under a 10%:90% H2 / N2 atmosphere to obtain the CeO2-NiFe-CaO bifunctional material, denoted as 20CNF-CaO.
[0043] Comparative Example 1:
[0044] 1g of calcium hydroxide was calcined in a 99.9% N2 atmosphere at a temperature of 600℃ for 10 minutes, and finally pure CaO bifunctional material was obtained, denoted as CaO.
[0045] Comparative Example 2:
[0046] Untreated pure calcium hydroxide sample.
[0047] Comparative experiment:
[0048] The CeO2-NiFe-CaO bifunctional materials prepared in Examples 1-4 and the sample materials prepared in Comparative Examples 1-2 were selected for in-situ capture and conversion performance testing. The testing method included: the CeO2-NiFe-CaO bifunctional materials prepared in Examples 1-4 and the sample materials prepared in Comparative Examples 1-2 were subjected to integrated CO2 capture and reverse water gas conversion reaction under normal pressure and 650℃.
[0049] The specific steps are as follows: 0.4g of the experimental material was weighed, and an in-situ capture and conversion experiment was conducted using a U-tube reactor. First, CO2 capture was performed in a gas stream with a volume ratio of CO2:N2 = 10%:90% and a flow rate of 300ml / min for 10min. Then, after 5min of nitrogen purging, the flow rate was switched to an in-situ reverse water-gas conversion stream with a flow rate of H2:N2 = 10%:90% and a flow rate of 300ml / min. The products were detected using a flue gas analyzer, and the experimental results are shown in Table 1.
[0050] Table 1
[0051] Experimental subjects CO2 adsorption capacity (mmol / g) CO yield (mmol / g) Example 1 8.68 2.55 Example 2 9.05 2.59 Example 3 9.57 2.85 Example 4 8.59 2.25 Comparative Example 1 8.06 0.73 Comparative Example 2 4.13 0.21
[0052] From the above experimental data, we can see that:
[0053] A bifunctional CeO2-NiFe-CaO material was prepared using a cerium oxide-nickel iron alloy as the catalytic component and calcium oxide as the adsorbent component. Compared with untreated calcium hydroxide and pure calcium oxide samples, the CO2 adsorption capacity and CO yield in the integrated CO2 capture and reverse water-gas conversion reaction were significantly increased. Among these, the 15CNF-CaO bifunctional material obtained at a mass-to-volume ratio of cerium oxide-nickel iron alloy to calcium hydroxide of 1.08 g:1 g exhibited the best cyclic capture and conversion performance in the integrated CO2 capture and reverse water-gas conversion reaction.
[0054] Figure 2 The figures show the XRD patterns of the bifunctional material in Example 3 of this invention before and after the reduction reaction, with the horizontal axis representing the position of the characteristic peaks and the vertical axis representing the intensity of the characteristic peaks. As can be seen from the figures, no cerium oxide-nickel ferrite phase peaks were detected in the 15CNF-CaO before the reaction, indicating that the cerium oxide-nickel ferrite particles in the bifunctional material are small and uniformly dispersed. After reduction, nickel-iron alloy phase peaks appeared, indicating that a cerium oxide-nickel-iron alloy was formed during the reduction.
[0055] Figures 3a-3b The graph shows the in-situ capture and conversion performance test results of the CeO2-NiFe-CaO bifunctional materials in Examples 1-4 of this invention at 650℃. The horizontal axis represents the number of cycles, and the vertical axis represents the CO2 adsorption capacity and CO yield, respectively. As can be seen from the graph, at a reaction temperature of 650℃, the 15CNF-CaO prepared in Example 3 has the best cyclic capture and conversion performance in the integrated CO2 capture and reverse water-gas conversion reaction, with a CO2 adsorption capacity of 9.57 mmol / g and a CO yield of 2.85 mmol / g, and maintains good capture and conversion activity in all three cycles.
[0056] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a high-efficiency bifunctional material for carbon capture and in-situ conversion, characterized in that, The preparation method includes: Cerium salt and nickel ferrite are dispersed in a solvent, mixed evenly, and then stirred and heated at 300-500℃ until solid. The resulting cerium oxide-nickel ferrite is ground and mixed with calcium hydroxide and calcined. The calcination temperature is 500-700℃, the time is 8-15 min, and the calcination atmosphere is N2 with a purity of 99% or higher. After reduction, a bifunctional material is obtained. The bifunctional material has the composition of CeO2-NiFe-CaO, wherein the mass ratio of CaO to CeO2-NiFe is 4:1 to 19:
1.
2. The production method according to claim 1, characterized by, The cerium salt is cerium nitrate hexahydrate.
3. The production method according to claim 1, characterized by, The solvent is one of methanol, ethanol, and propanol.
4. The preparation method according to claim 1, characterized in that, The mass-to-volume ratio of cerium oxide-nickel ferrite to calcium hydroxide is from 0.036 g:1 g to 0.144 g:1 g.
5. The preparation method according to claim 1, characterized in that, The reduction temperature is 500-700℃, the time is 8-15 min, and the reduction atmosphere is 10%:90% H2 / N2.
6. A highly efficient dual-functional material for achieving carbon capture and in-situ conversion, characterized in that, It is prepared by the preparation method described in any one of claims 1-5.
7. An application of the high-efficiency bifunctional material as described in claim 6, characterized in that, The high-efficiency bifunctional material is applied to in-situ CO2 capture and conversion reactions, specifically in the integration of CO2 capture and reverse water gas conversion reactions.
Citation Information
Patent Citations
Porous adsorption and catalysis bifunctional material as well as preparation method and application thereof
CN115445622A
High-temperature-stable reduction-resistant cerium oxide-nickel ferrite composite catalyst as well as preparation method and application thereof
CN116371414A
Al-NiFe composite material for preparing synthesis gas with high selectivity through ethane reforming and application of Al-NiFe composite material
CN116727674A