Application of atomic-scale accurate gold nanocluster with photothermal effect in anti-icing and deicing aspects

CN118720123APending Publication Date: 2024-10-01UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410708215.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

Smart Images

  • Figure CN118720123A_ABST
    Figure CN118720123A_ABST
Patent Text Reader

Abstract

The invention discloses application of an atomic-scale precise gold nanocluster with a photothermal effect in anti-icing and deicing aspects, and belongs to the field of nano material application. According to the present invention, the synthesis process is simple, the rapid and efficient mass production is easily achieved, the efficient anti-icing and deicing can be achieved, the raw materials are easily available, the preparation process is simple, the rapid and efficient mass production is easily achieved, the advantages of raw material use reduction, repeated use, no pollution, no toxicity, environmental protection and the like are provided, and the method can be widely popularized to the practical application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano material applications, and in particular relates to the application of atomically precise gold nanoclusters with photothermal effects in anti-icing and de-icing. Background Art

[0002] Ice formation is a very common natural phenomenon in life. However, the accumulation of ice will have a series of adverse effects on human production and life, transportation, aviation and aerospace, etc., causing economic losses at the least and safety accidents at the worst. Therefore, efficient anti-icing and de-icing technologies and materials have attracted much attention. Traditional anti-icing and de-icing strategies include thermal melting and the use of anti-icing chemicals, but these methods consume a lot of manpower, financial resources and material resources. At present, the mainstream method of anti-icing is to use super-hydrophobic anti-icing coatings, which can not only delay the freezing time, reduce the freezing temperature and ice adhesion, but also have the advantages of environmental protection and low cost. However, it is still challenging to apply super-hydrophobic coatings to anti-icing, because long-term exposure to extreme cold conditions will lose the super-hydrophobicity of the material, so the super-hydrophobic coating can only temporarily delay ice formation. Therefore, the ideal super-hydrophobic surface should be able to both passively prevent ice and actively de-ice. The photothermal super-hydrophobic coating has both super-hydrophobic properties and photothermal effects, and is an ideal anti-icing and de-icing material. Gold nanoclusters are a new type of nanomaterials with a size (usually 1-3nm) between traditional metal nanoparticles and organometallic complexes. They are usually composed of dozens to hundreds of metal atoms as the core, and the surface is protected by ligands. Their biggest advantage is that the overall structure can be obtained through single crystal diffraction, that is, the composition and structure of the nanocluster are precisely defined at the atomic level. This feature enables atomically precise nanoclusters to reveal characteristics that cannot be "seen" on the surface of traditional nanoparticles. Moreover, the core of the nanocluster can adopt various atomic arrangement structures, rather than the single face-centered cubic structure of traditional nanoparticles. In the field of nanotechnology, the surface plasmon resonance of gold nanoparticles gives them enhanced optical properties, and strong surface plasmon resonance can convert light energy into heat energy. Due to the smaller size, nanoclusters no longer have surface plasmon resonance, but instead have multiple continuous absorption peaks, and their absorption intensity gradually weakens from the ultraviolet visible region to the near-infrared region. Therefore, synthesizing gold nanoclusters with high absorption in the near-infrared region, thereby achieving strong photothermal conversion in the near-infrared region, has a breakthrough significance for expanding new applications of nanoclusters in photothermal. The present invention synthesizes gold nanoclusters with photothermal effect and combines them with anti-icing and de-icing, which can achieve environmentally friendly and efficient anti-icing and de-icing. Summary of the invention

[0003] The problem to be solved by the present invention is to prepare an atomically precise gold nanocluster with a photothermal effect and apply it to anti-icing and de-icing. The present invention has a simple synthesis process, is easy to realize rapid and efficient mass production, and can realize efficient anti-icing and de-icing.

[0004] Technical Solution

[0005] The present invention adopts the following technical solutions:

[0006] The present invention prepares an atomically precise gold nanocluster with a photothermal effect and applies it to anti-icing and de-icing. The present invention has a simple synthesis process, is easy to realize rapid and efficient mass production, and can realize efficient anti-icing and de-icing.

[0007] (1) Synthesis of atomically precise gold nanoclusters with photothermal effect: weigh chloroaurate and tetraoctylammonium bromide and add them to a round-bottom flask, then add tetrahydrofuran solution, place the round-bottom flask on a magnetic stirrer, stir evenly for 15 minutes, the color of the solution changes from yellow to orange-red, then reduce the speed of the magnetic stirrer, slowly add 2-phenylethanethiol, continue to react for 60 minutes, the color of the solution changes from orange-red to colorless, then increase the speed of the magnetic stirrer, quickly add freshly prepared sodium borohydride aqueous solution, the solution generates a large number of bubbles, the color changes to black, continue to react for 6 hours, obtain a crude product, then wash the crude product with methanol, and finally obtain [Au 25 PET 18 ] - nanoclusters; then column chromatography was used to separate [Au 25 PET 18 ] - Oxidized to [Au 25 PET 18 ] 0 ; then [Au 25 PET 18 ] - Will be with [Au 25 PET 18 ] 0 Mix evenly, heat and evacuate in a vacuum drying oven to synthesize [Au 52 PET 33 ] 2- The crude product was then purified by column chromatography to obtain atomically precise [Au 52 PET 33 ] 2- Gold nanoclusters;

[0008] (2) Using laser to irradiate atomically precise gold nanoclusters of different concentrations and blank control samples to test the photothermal conversion effect of gold nanoclusters;

[0009] (3) The gold nanoclusters are evenly spin-coated on a glass substrate, and then the contact angles of the pure glass substrate and the glass substrate coated with the gold nanoclusters are tested. The pure glass substrate and the glass substrate coated with the gold nanoclusters are then placed in a glass container, and then deionized water is added to the glass container and placed in a refrigerator to freeze. After the deionized water condenses into ice, it is taken out and irradiated with a laser for a deicing test.

[0010] A further technical solution of the present invention is that in step (1), the mass of the chloroaurate is 80 mg, the mass of tetra-n-octylammonium bromide is 129 mg, the volume of tetrahydrofuran is 15 mL, the solvent in the round-bottom flask is 50 mL, the volume of 2-phenylethanethiol is 140 uL, the mass of sodium borohydride is 77 mg, the filler used in the first column chromatography is silica gel, the eluent is dichloromethane solution, the temperature in the vacuum drying oven is set to 80° C., the reaction time is 1 hour, and the filler used in the second column chromatography is bio-beads, and the eluent is tetrahydrofuran solution.

[0011] In a further technical solution of the present invention, in step (2), the laser wavelength is 808 nm and the power is 1 W / cm 2 The concentrations of atomically precise gold nanoclusters were 1.5 mg / mL, 0.3 mg / mL, and 0.15 mg / mL, and the solvent used for the blank control sample was tetrahydrofuran.

[0012] In a further technical solution of the present invention, in step (3), the laser wavelength is 808 nm and the power is 1 W / cm 2 , the length of the glass substrate is 80 mm, the width is 20 mm, the solvent used in testing the contact angle is deionized water, the diameter of the glassware is 90 mm, the volume of deionized water is 20 mL, and the thickness of the ice is 8 mm.

[0013] An atomically precise gold nanocluster with photothermal effect obtained by the preparation method as described above can be efficiently used in anti-icing and de-icing.

[0014] Beneficial Effects

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] Compared with the existing technology, the synthesis process of the atomically precise gold nanoclusters with photothermal effect prepared by the present invention is relatively simple, and it is applicable to a variety of metal ion and alloy nanoclusters, and can achieve efficient anti-icing and de-icing in a short time. It has the advantages of easy availability of raw materials, simple preparation process, and easy to achieve fast and efficient large-scale production.

[0017] The atomically precise gold nanoclusters with photothermal effect prepared by the present invention have more advantages than traditional synthesis methods, reduce the use of raw materials, are pollution-free, non-toxic, and environmentally friendly, and can be widely promoted to practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 UV spectrum of gold nanoclusters

[0019] Figure 21. Temperature change curves of 5mg / mL, 0.3mg / mL, 0.15mg / mL gold nanoclusters and blank control samples under 808nm laser irradiation

[0020] Figure 31.5mg / mL, 0.3mg / mL, 0.15mg / mL gold nanoclusters cycle test under 808nm laser irradiation

[0021] Figure 4 Infrared thermal imaging images of the temperature changes of 1.5mg / mL, 0.3mg / mL, 0.15mg / mL gold nanoclusters and blank control samples under 808nm laser irradiation

[0022] Figure 5 Contact angle measurements of pure glass substrate and glass substrate coated with gold nanoclusters

[0023] Figure 6 Test images of the deicing process of a pure glass substrate and a glass substrate coated with gold nanoclusters DETAILED DESCRIPTION

[0024] The present invention will be further described and illustrated below in conjunction with the embodiments of the present invention.

[0025] The synthesized atomically precise gold nanoclusters were dissolved in tetrahydrofuran, and then 3 mL of the gold nanocluster solution was taken in a cuvette to test its ultraviolet spectral properties. The data showed that the synthesized gold nanoclusters had strong absorption at 820 nm and 1100 nm, indicating that gold nanoclusters with strong absorption in the near-infrared region were successfully synthesized; then the gold nanoclusters were configured into solutions with concentrations of 1.5 mg / mL, 0.3 mg / mL, and 0.15 mg / mL, respectively, and the solvent used was tetrahydrofuran, and then 100 uL was taken for photothermal testing. The laser wavelength used was 808 nm and the power was 1 W / cm 2, then turn on the infrared thermal imaging camera to record the test process. The gold nanoclusters showed an extremely fast temperature rise process, rising by about 40°C in just 2 minutes. The laser was turned off after 4 minutes, and the solution cooled to ambient temperature within 8 minutes. The blank control experiment used 100uL of pure tetrahydrofuran solvent. Under the same test conditions, the temperature of the solution remained unchanged, indicating that the gold nanoclusters have a strong photothermal conversion effect. Then the repeatability of the gold nanoclusters was tested. The laser irradiated the gold nanocluster solution for 4 minutes, then turned off the laser. After 8 minutes, the solution temperature dropped to ambient temperature, and then continued to turn on the laser and repeated the above operation. After 5 cycles, the photothermal conversion efficiency of the gold nanocluster solution remained unchanged, indicating that the gold nanoclusters not only have a high photothermal conversion effect, but also have high stability.

[0026] Anti-icing and de-icing applications: Spin-coat the gold nanoclusters on the glass substrate with a spin coater, and then test the contact angles of the pure glass substrate and the glass substrate coated with gold nanoclusters. It can be found that the contact angle of the glass substrate coated with gold nanoclusters is much larger than that of the pure glass substrate, proving that the gold nanoclusters have hydrophobic properties relative to glass, so the gold nanoclusters can be applied to anti-icing. Then place the pure glass substrate and the glass substrate coated with gold nanoclusters in a glass container, add an appropriate amount of deionized water, and then place the glass container in the freezer area of ​​the refrigerator. After the deionized water condenses into ice, irradiate the sample with an 808nm laser, shoot the entire experimental process, and then record the melting of the ice at 0s, 60s, 120s, 180s, and 240s respectively. The experimental results show that the gold nanoclusters with photothermal effect have a good de-icing effect.

Claims

1. An atomically precise gold nanocluster with photothermal effect for anti-icing and de-icing, comprising the following steps: (1) Synthesis of atomically precise gold nanoclusters with photothermal effect: weigh chloroaurate and tetraoctylammonium bromide and add them to a round-bottom flask, then add tetrahydrofuran solution, place the round-bottom flask on a magnetic stirrer, stir evenly for 15 minutes, the color of the solution changes from yellow to orange-red, then reduce the speed of the magnetic stirrer, slowly add 2-phenylethanethiol, continue to react for 60 minutes, the color of the solution changes from orange-red to colorless, then increase the speed of the magnetic stirrer, quickly add freshly prepared sodium borohydride aqueous solution, the solution generates a large number of bubbles, the color changes to black, continue to react for 6 hours, obtain a crude product, then wash the crude product with methanol, and finally obtain [Au 25 PET 18 ] - nanoclusters; then column chromatography was used to separate [Au 25 PET 18 ] - Oxidized to [Au 25 PET 18 ] 0 ; then [Au 25 PET 18 ] - With [Au 25 PET 18 ] 0 Mix evenly, Heat and evacuate in a vacuum drying oven to synthesize [Au 52 PET 33 ] 2- The crude product was then purified by column chromatography to obtain atomically precise [Au 52 PET 33 ] 2- Gold nanoclusters. (2) Using laser to irradiate atomically precise gold nanoclusters of different concentrations and blank control samples to test the photothermal conversion effect of gold nanoclusters; (3) The gold nanoclusters are evenly spin-coated on a glass substrate, and then the contact angles of the pure glass substrate and the glass substrate coated with the gold nanoclusters are tested. The pure glass substrate and the glass substrate coated with the gold nanoclusters are then placed in a glass container, and then deionized water is added to the glass container and placed in a refrigerator to freeze. After the deionized water condenses into ice, it is taken out and irradiated with a laser for a deicing test.

2. The use according to claim 1, characterized in that: In step (1), the mass of the chloroaurate is 80 mg, the mass of tetraoctylammonium bromide is 129 mg, the volume of tetrahydrofuran is 15 mL, the solvent in the round-bottom flask is 50 mL, the volume of 2-phenylethanethiol is 140 uL, the mass of sodium borohydride is 77 mg, the filler used in the first column chromatography is silica gel, the eluent is dichloromethane solution, the temperature in the vacuum drying oven is set to 80° C., the reaction time is 1 hour, and the filler used in the second column chromatography is bio-beads, and the eluent is tetrahydrofuran solution.

3. The use according to claim 1, characterized in that: In step (2), the laser wavelength is 808nm and the power is 1W / cm 2 The concentrations of atomically precise gold nanoclusters were 1.5 mg / mL, 0.3 mg / mL, and 0.15 mg / mL, and the solvent used for the blank control sample was tetrahydrofuran.

4. The use according to claim 1, characterized in that: In step (3), the laser wavelength is 808nm and the power is 1W / cm 2 , the length of the glass substrate is 80 mm, the width is 20 mm, the solvent used in testing the contact angle is deionized water, the diameter of the glassware is 90 mm, the volume of deionized water is 20 mL, and the thickness of the ice is 8 mm.