Visualizing semi-permanent release agent, its preparation method and application
A visual semi-permanent release agent was prepared by polymerizing vinyl-terminated siloxane compounds with tetrazine compounds. This solved the problems of insufficient high temperature resistance, wear resistance and impact resistance of existing release agents, and achieved efficient multiple demolding and use indication functions, thereby improving production efficiency.
Patent Information
- Application Number
- CN202411006139.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing mold release agents are insufficient in terms of high temperature resistance, wear resistance, and impact resistance, leading to frequent coating and affecting production efficiency.
A semi-permanent release agent is formed by polymerizing vinyl-terminated siloxane compounds and tetrazine compounds in an inert solvent. This agent improves rigidity and mechanical properties by increasing the density of intermolecular crosslinking and changing the interaction forces. The addition of amino silicone oil as a solvent forms a rapidly forming, high-temperature resistant, and wear-resistant release film.
It achieves rapid film formation, high temperature resistance, wear resistance, and impact resistance in the release agent, increases the number of demolding cycles, improves production efficiency, and provides usage instructions through color changes, reducing product defects.
Smart Images

Figure CN118721540B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a visual semi-permanent release agent, its preparation method and application, belonging to the field of release agent technology, and is suitable for external release systems, especially for external release systems in the production of plastic products. Background Technology
[0002] Release agents are functional substances that lie between the mold and the finished product. During the product molding process, physical or chemical adsorption can occur between the product and the mold, making it difficult to remove the molded product from the mold. The use of release agents can smoothly separate the cured product from the mold, resulting in a smooth and flat product, and ensuring that the mold can be used multiple times.
[0003] Generally, the mold release agents currently used in plastic products are mainly silicone mold release agents. Due to their low surface tension, good leveling properties, and advantages such as high temperature resistance, non-toxicity, good gloss, and non-affinity with resins, they are widely used in various applications involving plastics and rubber. To improve the mechanical abrasion resistance of silicone mold release agents, the components need to be modified.
[0004] US20180346661 discloses an organosiloxane emulsion composition, finding that by incorporating an organopolysiloxane with polyoxyalkylene residues at both ends into an organosilicone emulsion composition containing a high-viscosity organopolysiloxane and an organosiloxysilicate containing polyether groups, an emulsion with good stability in water-soluble solvents was successfully obtained. This mold release agent, through modification, improves both its release properties and emulsion stability. However, this mold release agent is easily transferred from the mold to the product, making it impossible to achieve multiple releases after a single application. Therefore, the mold release agent needs to be frequently reapplied to the mold, ultimately affecting production efficiency.
[0005] US4244912A discloses a curable siloxane composition comprising four parts: polydiorganosiloxane, xylene-soluble copolymer, methylhydropolysiloxane, and a hydrosilylation catalyst. This composition cures rapidly at low temperatures and is abrasion-resistant, making it suitable as a curable release agent, particularly useful in molding methods using "cold molding" polyurethane compositions. While this curable release agent allows for multiple releases with minimal transfer from the mold to the product, its poor heat resistance limits its applicability.
[0006] CN1671794A discloses a curable composition with release properties, comprising an ethylene polymer containing alkenyl groups, a compound containing hydrogenated silyl groups, a hydrogenated silanization catalyst, and a metal soap. This curable composition exhibits good mechanical properties, oil resistance, heat resistance, and release properties; however, its thermosetting temperature needs to be above 100°C, resulting in energy waste and complex operation.
[0007] Therefore, if a release agent that can form a film quickly, is resistant to high temperatures, wear, and impact will be developed, it will be of great significance and have broad market prospects in the field of release agents. Summary of the Invention
[0008] This invention provides a visual semi-permanent release agent, its preparation method, and its application, aiming to obtain a release agent that forms a film quickly, is resistant to high temperatures, wear, and impact, thereby increasing the number of demolding cycles and improving production efficiency.
[0009] The technical problem to be solved by this invention is achieved by the following technical solution:
[0010] A visual semi-permanent release agent, the general structural formula of which is as follows:
[0011]
[0012] Wherein: R1-R8 are independent of each other, and R1-R8 are selected from the following same or different straight-chain or branched alkyl, alkenyl, cycloalkyl or cycloalkenyl, aryl or aromatic groups, n is an integer from 1 to 30, and the sum of x+y is an integer from 1 to 1000.
[0013] Preferably, R1-R8 are selected from C1-C6 alkyl or alkenyl groups.
[0014] Preferably, the structural formula of the release agent is as follows:
[0015]
[0016] Where x + y = 300 - 500 integers, and n is an integer between 2 and 5.
[0017] A method for preparing a visual semi-permanent release agent, the reaction process of which is shown below:
[0018]
[0019] It is prepared by polymerizing vinyl-terminated siloxane compounds and tetrazine compounds at 0-80°C, preferably at a reaction time of 60°C.
[0020] Preferably, the polymerization reaction is obtained by mixing a vinyl-terminated siloxane compound with a tetrazine compound, followed by stirring, cooling, and standing.
[0021] Furthermore, the stirring speed is 100-2000 rpm, and the stirring time is 3-15 hours.
[0022] Furthermore, the stirring speed was 1000 rpm and the stirring time was 10 hours.
[0023] Preferably, n in the tetrazine compound is an integer from 1 to 30.
[0024] Furthermore, n is between 2 and 30.
[0025] Furthermore, n can be 2-5.
[0026] Preferably, the general structural formula of the vinyl-terminated siloxane compound is as follows:
[0027]
[0028] Furthermore, the general structural formula of the vinyl-terminated siloxane compound is as follows:
[0029] ViMe2SiO(Me2SiO) x SiMe2Vi, where y = 0; or,
[0030] ViPhMeSiO(Me2SiO) x SiMePhVi, where y = 0; or,
[0031] ViMe2SiO(Me2SiO) x (ViMeSiO) y SiMe2Vi; or,
[0032] ViPhMeSiO(Me2SiO) x (ViMeSiO) y SiMePhVi;
[0033] Where: Me, Et, Ph and Vi represent methyl, ethyl, phenyl and vinyl respectively, and the sum of x+y is an integer from 1 to 1000.
[0034] Furthermore, the vinyl-terminated siloxane compounds have the following two structural formulas:
[0035] ViMe2SiO(Me2SiO) x (ViMeSiO) y SiMe2Vi, where the sum of x+y is an integer between 300 and 500; or, ViMe2SiO(Me2SiO). x SiMe2Vi, where x is an integer between 300 and 500.
[0036] The release agent composition is prepared by stirring a vinyl-terminated siloxane compound, a tetrazine compound, an amino silicone oil, and a solvent in a mass-volume ratio of 1g:0.05-0.15g:0.01-0.05g:10-100mL.
[0037] Preferably, in the method for preparing the release agent composition, the mass-volume ratio of the vinyl-terminated siloxane compound, the tetrazine compound, the amino silicone oil, and the solvent is 1g:0.1g:0.02g:100mL, and the molecular weight of the amino silicone oil is 1000-100000.
[0038] Furthermore, the solvent is one or more of the following: alcohol solvents, alcohol ether solvents, ketone solvents, ester solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, and ether solvents.
[0039] Furthermore, the alcohol solvent is one or more of ethanol, isopropanol, propylene glycol, butanol, 1,4-butanediol, 1,3-butanediol and glycerol;
[0040] The alcohol ether solvent is one or more of ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monobutyl ether;
[0041] The ketone solvent is one or more of acetone, butanone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone;
[0042] The ester solvent is one or more of methyl acetate, ethyl acetate and butyl acetate;
[0043] The aliphatic hydrocarbon solvent is one or more of n-hexane, carbon tetrachloride, petroleum ether, and isoalkanes (C8-C10);
[0044] The alicyclic hydrocarbon solvent is one or both of cyclopentane and cyclohexane;
[0045] The aromatic hydrocarbon solvent is one or both of toluene and xylene;
[0046] The ether solvent is one or more of tetrahydrofuran, diisopropyl ether, and dibutyl ether.
[0047] Preferably, during the preparation of the release agent composition, the stirring speed is 100-2000 rpm and the stirring time is 1-5 h.
[0048] Furthermore, during the preparation of the release agent composition: the stirring speed is 1000 rpm and the stirring time is 3 hours.
[0049] The above-described visual semi-permanent release agent or the above-described release agent composition is used in the preparation of external release system products.
[0050] Preferably, the external release system products are plastic products and rubber products with external release systems.
[0051] Furthermore, the plastic products include polyurethane foam products, epoxy resin products, glass fiber reinforced epoxy resin products, and unsaturated polyester products.
[0052] The beneficial effects of this invention are:
[0053] (1) The release agent or release agent composition prepared by the present invention has the addition of tetrazine compounds, which increases the crosslinking density between tetrazine compounds and vinyl-terminated siloxane compounds to improve the rigidity of the release agent, or adjusts its strength by changing the intermolecular forces, thereby giving the release agent certain rigid mechanical properties, enhancing its wear resistance and impact resistance, thereby increasing the number of demolding times and improving production efficiency.
[0054] (2) Through testing, the addition of tetrazine compounds improves the thermal stability of the release agent, making it more resistant to high temperatures and applicable to a wider range of conditions.
[0055] (3) In addition, tetrazine compounds are purple solids. When they react completely with vinyl-terminated siloxane compounds, the color becomes lighter to light purple. The addition of tetrazine compounds has an indicative effect on the preparation of release agents and also has an indicative effect during the use of release agents. When most of the color disappears, it is necessary to reapply.
[0056] (4) The release agent or release agent composition of the present invention has the characteristics of simple composition, rapid curing, extremely low transfer rate, good storage stability, high temperature resistance and indicator function. In addition, the release film has certain mechanical properties, which improves wear resistance and impact resistance, so as to ensure smooth production, improve production efficiency and reduce product defects. Attached Figure Description
[0057] Figure 1 The figures show the film formation of release agent compositions 1-6 on the mold surface in test 2, where (a) is release agent composition 1, (b) is release agent composition 2, (c) is release agent composition 3, (d) is release agent composition 4, (e) is release agent composition 5, and (f) is release agent composition 6.
[0058] Figure 2 The TGA graph was used to test the thermal stability of the four release agent compositions, where the horizontal axis represents temperature (°C) and the vertical axis represents weight percentage (%). Detailed Implementation
[0059] To facilitate a clear understanding of the technical means, creative features, objectives, and effects of this invention, the invention will be further described below in conjunction with specific illustrations.
[0060] The most commonly used mold release agents or combinations on the market are external mold release agents. These are applied directly to the mold surface and, after a period of time, form a smooth, dense release film, thus separating the mold from the processed material. External mold release agents must bond well to the mold surface, adhering firmly without transferring to the product, but without reacting or adhering to the product. Furthermore, because the injection of raw materials into the mold involves a certain impact force, the release film formed on the mold surface should ideally possess certain rigid mechanical properties, being impact-resistant and wear-resistant.
[0061] In this invention, the "semi-permanent release agent" refers to a release agent in which the main component forms a cross-linkable polymer in an inert solvent. The solution is applied to the surface of the mold, and after solvent evaporation and solute curing, a complete and uniform isolation film is formed on the entire surface of the mold. This isolation film has a certain rigidity and mechanical strength, which can effectively resist the damage caused by shear forces generated during the demolding process, thus enabling 15-25 demolding cycles after a single application.
[0062] "Visualization" refers to the fact that the release agent in this invention has a light purple color, which serves as an indicator during the preparation and use of the release agent. When most of the color disappears, it needs to be reapplied.
[0063] It should be noted that some of the following substances in some embodiments of the present invention were obtained by purchasing commercially available products, as detailed in Table 1.
[0064] Table 1:
[0065]
[0066]
[0067] The molds used in the following embodiments of the present invention are molds made of the following materials:
[0068] The release agent described in this invention can be applied to a molded mold by any suitable method, such as by spraying, brushing or rolling. The mold can be a metallic material, such as aluminum, nickel, stainless steel, brass, etc., or a non-metallic material, such as resin material, etc.
[0069] Example 1: Preparation of Tetraazine Compound 1
[0070] Sulfur (0.64 g, 10 mmol) was added to an aqueous solution of terephthalonitrile (1.28 g, 10 mmol) (7 mL), and hydrazine hydrate (10 mL, 164 mmol) was added to the solution that had been refluxed at 100 °C for 8 hours. The resulting yellow precipitate was washed with cold ethanol (3 × 10 mL) and allowed to stand in air for 3 hours to give a purple solid (1.32 g, 20%), which is tetrazine compound 1, with the following structural formula:
[0071] n is an integer between 2 and 5.
[0072] The mass spectrum of tetrazine compound 1 is as follows:
[0073] 546.18 (100.0%), 547.18 (32.7%), 548.18 (6.5%), 547.17 (4.4%).
[0074] Example 2: Preparation of tetrazine compound 2
[0075] This embodiment is basically the same as Example 1, except that in this embodiment, hydrazine hydrate (10 mL, 164 mmol) was refluxed in a solution at 100 °C for 15 h; a purple solid (2.87 g, 23%) was obtained, which is tetrazine compound 2, and its structural formula is as follows:
[0076] n is an integer between 6 and 30.
[0077] The mass spectrum of tetrazine compound 2 is as follows:
[0078] 1326.40 (100.0%), 1327.40 (76.1%), 1328.40 (37.3%), 1327.39 (11.8%), 1329.41 (7.0%), 1329.40 (3.4%), 1330.41 (1.3%), 1330.40 (1.0%).
[0079] Example 3: Preparation of Release Agent Composition 1
[0080] The chemical reaction process is as follows:
[0081]
[0082] Specifically, 5g of Polymer VS 500, 0.5g of 3,6-diphenyl-1,2,4,5-tetraazine, 10mL of ethanol, and 90mL of isodecane were added to the reactor respectively. The mixture was stirred for 10 hours at 60℃ and 1000rpm for the first stirring condition. After cooling to room temperature, 0.01g of amino silicone oil was added to the reactor, and the mixture was stirred for 3 hours at 1000rpm for the second stirring condition at room temperature. After standing, the release agent composition 1 was obtained.
[0083] Example 4: Preparation of Release Agent Composition 2
[0084] The chemical reaction process is as follows:
[0085]
[0086] This embodiment is basically the same as Example 3, except that the 3,6-diphenyl-1,2,4,5-tetraazine in Example 3 is replaced with tetrazine compound 1 prepared in Example 1 to obtain release agent composition 2.
[0087] Example 5: Preparation of release agent composition 3
[0088] The chemical reaction process is as follows:
[0089]
[0090] This embodiment is basically the same as Example 3, except that the 3,6-diphenyl-1,2,4,5-tetraazine in Example 3 is replaced with tetrazine compound 2 prepared in Example 2 to obtain release agent composition 3.
[0091] Example 6: Preparation of Release Agent Composition 4
[0092] The chemical reaction process is as follows:
[0093]
[0094] This embodiment is basically the same as embodiment 3, except that Polymer VS 500 is replaced with Polymer RV5000 to obtain release agent composition 4.
[0095] Example 7 Preparation of release agent composition 5
[0096] The chemical reaction process is as follows:
[0097]
[0098] This embodiment is basically the same as embodiment 4, except that Polymer VS 500 is replaced with Polymer RV5000 to obtain release agent composition 5.
[0099] Example 8: Preparation of Release Agent Composition 6
[0100] The chemical reaction process is as follows:
[0101]
[0102] This embodiment is basically the same as embodiment 5, except that Polymer VS 500 is replaced with Polymer RV5000 to obtain release agent composition 6.
[0103] The following tests were performed on the release agent compositions 1-6 prepared in Examples 3-8:
[0104] Test 1: Stability testing of release agent compositions 1-6
[0105] The release agent compositions 1-6 prepared in Examples 3-8 were mixed with 191 unsaturated resin and heated at 100°C for 24 hours. Compared with 191 unsaturated resin without release agent compositions 1-6, it can be seen that release agent compositions 1-6 do not react with 191 unsaturated resin.
[0106] Test 2 Storage stability of release agent compositions 1-6
[0107] The release agent compositions 1-6 prepared in Examples 3-8 were found to be stable for 12 months after being left to stand at (30±2)℃.
[0108] Test 3 Film-forming properties of release agent compositions 1-6
[0109] Take the release agent compositions 1-6 prepared in Examples 3-8, and use a degreased cotton ball to evenly apply the release agent compositions 1-6 to the clean and dry mold using a circular motion. The thickness of the application should be 0.05-5 μm, preferably 0.1-2 μm. Start timing. Stop timing when the surface of the release film is gently wiped with a dry degreased cotton ball without leaving any traces. Record the time. This time is the film-forming time of the release agent composition.
[0110] The results showed that the film-forming time of release agent compositions 1-6 on the mold was within 10 minutes, indicating that release agent compositions 1-6 could form a film in a relatively short time.
[0111] The surface of the release film was photographed with a camera to observe the film-forming state of the release agent composition. The surface of the film formed by the release agent composition is shown in the attached image. Figure 1 ; Figure 1 The results show that the release films formed on the mold by release agent compositions 1-6 all have a smooth and flat surface.
[0112] Test 4 Release agent compositions 1-6 release properties
[0113] The release agent compositions 1-6 prepared in Examples 3-8 were applied to the cleaned molds with a thickness of 0.05-5 μm, particularly preferably 0.1-2 μm. Then, 191 unsaturated resin was continuously molded on the mold. The process ended when the 191 unsaturated resin adhered to the mold or could not be easily removed from the mold. The number of consecutive demoldings of the 191 unsaturated resin on the release agent compositions 1-6 was recorded. The results are shown in Table 2.
[0114] Table 2 Number of consecutive demolding cycles with release agent
[0115] Example Release agent composition Number of consecutive demolding cycles Film-forming properties 3 1 15 whole 4 2 23 whole 5 3 19 whole 6 4 15 whole 7 5 25 whole 8 6 21 whole
[0116] As shown in Table 2, the release agent compositions 1-6 all achieved more than 15-25 consecutive demolding times on the mold. The best was release agent composition 5, which achieved 25 consecutive demolding times, which is superior to most commercially available silicone release agents.
[0117] Test 5: Thermal stability test of release agent compositions 1-6
[0118] Take the release agent compositions 1-6 from Examples 3-8 respectively, and test the thermal stability of the release agents using a thermogravimetric analyzer. The specific process is as follows:
[0119] Under a protected N2 atmosphere, release agent compositions 1-6 were placed into crucibles in a heating furnace and heated at 10°C·min. -1 The temperature was increased from 35℃ to 500℃ at a rate that allowed the release agent compositions 1-6 to experience mass loss within the 35-500℃ temperature range. The test results are shown below. Figure 2 ,from Figure 2 It can be seen that, under the condition of 340-370℃, the release agent composition 5 prepared in Example 7 has the lowest mass loss and higher thermal stability.
[0120] Figure 2 The results show that all release agent compositions 1-6 have good thermal stability.
[0121] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and various changes and modifications can be made without departing from the spirit and scope of the invention, all of which fall within the scope of the claims. The scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A visual semi-permanent release agent, characterized in that: The general structural formula of the release agent is as follows: Wherein: R1-R8 are independent of each other, and R1-R8 are selected from the same or different straight-chain or branched alkyl, alkenyl, cycloalkyl or cycloalkenyl, aryl or aromatic groups; n is an integer from 1 to 30, and the sum of x+y is an integer from 1 to 1000.
2. The visual semi-permanent release agent according to claim 1, wherein R1-R8 are selected from C1-C6 alkyl or alkenyl groups.
3. The visual semi-permanent release agent according to claim 1, characterized in that: The structural formula of the release agent is as follows: Where x + y = 300 - 500 integers, and n is an integer between 2 and 5.
4. A method for preparing a visual semi-permanent release agent according to any one of claims 1-3, characterized in that: The reaction process is as follows: It is formed by the polymerization reaction of vinyl-terminated siloxane compounds and tetrazine compounds at 0-80°C.
5. The method for preparing a visual semi-permanent release agent according to claim 4, characterized in that: In the tetrazine compounds, n is an integer from 1 to 30.
6. The method for preparing a visual semi-permanent release agent according to claim 5, characterized in that: n is an integer between 2 and 5.
7. A visual semi-permanent release agent composition, characterized in that, It includes the mold release agent and amino silicone oil as described in any one of claims 1 to 3.
8. The method for preparing the release agent composition according to claim 7, characterized in that, The product is obtained by mixing vinyl-terminated siloxane compounds, tetrazine compounds, amino silicone oil, and solvent in a mass-volume ratio of 1g:0.05-0.15g:0.01-0.05g:10-100mL.
9. The method for preparing the release agent composition according to claim 8, characterized in that, The mass-to-volume ratio of vinyl-terminated siloxane compounds, tetrazine compounds, amino silicone oil, and solvent is 1 g: 0.1 g: 0.02 g: 100 mL.
10. The use of a visual semi-permanent release agent as described in any one of claims 1-3 or the release agent composition as described in claim 7 in the preparation of external release system products.
Citation Information
Patent Citations
Organosilicone emulsion composition
US20180346661A1
Preparation method of semi-permanent organic silicon release agent
CN118269271A
Molding process using curable silicone release compositions
US4244912A