Method for preparing cesium iodide from rubidium-cesium concentrate
Through high-temperature roasting and acidic solution treatment of the rubidium-cesium enrichment, iodide ions and bismuth oxide are combined to form a cesium iodobismuthate precipitate, and high-purity cesium iodide is obtained through thermal decomposition, which solves the difficulties and processes in the separation of rubidium and cesium in the existing technology. complex problem, enabling efficient selective recovery of cesium and process simplification.
Patent Information
- Application Number
- CN202310686398.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-06-09
Smart Images

Figure CN118724032A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of extraction technology, in particular to a method for preparing cesium iodide from rubidium and cesium enriched materials. Background Art
[0002] Cesium is an expensive and rare alkaline metal. Due to its unique physical and chemical properties, it is widely used in atomic clocks, biomedicine, electronic devices, new energy, aerospace and other fields. Rubidium and cesium are widely distributed in the earth's crust, mainly in mineral resources such as cesium garnet, lithium mica and salt lake brine. They are rarely formed as independent minerals. Among them, cesium garnet is the basic raw material for producing various cesium compounds and cesium metal, and is also the main mineral for industrial extraction of cesium. In industry, rubidium and cesium are mainly found in the post-lithium extraction liquid or waste liquid. The reserves of rubidium and cesium in salt lake brine are large but the content is low. The content of rubidium is only 10-20 mg / L, and the content of cesium is much lower than that of rubidium.
[0003] Whether in high-salt wastewater or brine, cesium usually coexists with a large amount of rubidium, potassium and sodium. In particular, the properties of rubidium and cesium are extremely similar, and they can even be used interchangeably in some applications. Therefore, the selective separation of rubidium and cesium is very difficult. Methods for extracting rubidium and cesium from solutions include precipitation separation, adsorption separation, solvent and other methods. The adsorption separation method mainly uses rubidium and cesium ions to exchange ions with adsorbents, or adsorbs rubidium and cesium ions on porous surfaces. The adsorption method has good selectivity and simple process, but the adsorbent has a relatively small adsorption capacity and is more suitable for the separation of low concentrations of rubidium and cesium. Solution extraction is a rubidium and cesium separation technology that has been studied more and developed the fastest. The solvent extraction process has a large processing capacity and can realize continuous production. However, the extractant has certain toxicity, a long process flow, and a large amount of wastewater discharge. As a traditional separation technology, the precipitation method has the advantages of simple precipitation process, convenient operation, and suitability for large-scale production, but it also has the disadvantages of forming secondary waste and low product purity. Commonly used precipitants for rubidium and cesium include vanadium salts, polyhalides, heteropoly acids and ferrocyanide.
[0004] Chinese Patent 202010712906.1 proposes a method for extracting cesium and rubidium from lithium mica, wherein a mixed alum of rubidium and cesium is calcined at high temperature to obtain a sulfate solution enriched with rubidium and cesium, and then cesium sulfate and rubidium sulfate with a purity of more than 98% are obtained through multi-stage extraction, and the total recovery rate of cesium and rubidium is more than 80%; Chinese Patent 202110474179.4 proposes a method for extracting rubidium and cesium from complex underground brine, which uses tin tetrachloride precipitation method to enrich rubidium and cesium; Chinese Patent 201710615317. X proposed a method for separating and extracting rubidium and cesium from coal, using iodine chloride to generate a precipitate containing rubidium and cesium, and then combining t-BAMBP extraction to obtain high-purity rubidium chloride and cesium chloride; China 201910583379 proposed a precipitation flotation separation system for rubidium and cesium in aqueous solution and its application, using phosphotungstate as a precipitation flotation system for the separation and purification of rubidium and cesium resources; U.S. Patent 4432893 proposed a Precipitation-adsorption process for the decontamination of nuclear waste supernates, using sodium tetraphenylborate to precipitate cesium and potassium in high-level nuclear waste to purify cesium.
[0005] In summary, most precipitants can only extract rubidium and cesium indiscriminately, and the subsequent separation of rubidium and cesium can only rely on extraction and other processes.
[0006] Therefore, the present invention provides a method for preparing cesium iodide from rubidium and cesium enriched materials. Summary of the invention
[0007] In order to make up for the deficiencies of the prior art and solve the technical problems existing in the background technology, the present invention proposes a method for preparing cesium iodide from rubidium and cesium enriched materials.
[0008] The present invention is achieved by the following technical solution: a method for preparing cesium iodide from rubidium-cesium enriched material, the method comprising the following steps:
[0009] S1: Weigh an appropriate amount of rubidium-cesium enriched material, put it into a high-temperature calcining furnace for high-temperature calcination, and obtain calcined slag;
[0010] S2: putting the roasted slag in S1 into a container filled with deionized water, so that the roasted slag is dissolved in the deionized water and allowed to stand, and after the dissolution is completed, filtering it to obtain solution A and filter residue;
[0011] S3: adding an acidic solution to solution A in S2, adjusting the pH of solution A to acidic, and at the same time, adding an amount of iodine ions calculated according to the cesium concentration, and continuously stirring to obtain a yellow solution B;
[0012] S4: weighing an appropriate amount of bismuth oxide, and then dissolving it in a container containing an appropriate amount of hydrochloric acid solution to obtain solution C;
[0013] S5: adding the solution C in S4 to the yellow solution B in S3, stirring continuously, to obtain a red solid precipitate D containing cesium and a solution E containing rubidium;
[0014] S6: performing solid-liquid separation on the red solid precipitate D containing cesium and the filtrate E containing rubidium in S5 to obtain a solid precipitate D containing cesium and a solution E containing rubidium;
[0015] S7: placing the red solid precipitate D of cesium in S6 into a thermal decomposition device for thermal decomposition treatment to obtain a volatile product, bismuth iodide, and a residual product, cesium iodide.
[0016] The rubidium-cesium enriched material in the present invention is mainly a mixture of rubidium, cesium, potassium, sodium, magnesium, and iron, and also includes non-metallic elements such as carbon and nitrogen; the contents of the main elements are shown in the following table:
[0017]
[0018] Preferably, the rubidium-cesium enriched material in S1 is calcined at a temperature of 500-600° C. in an atmospheric atmosphere. Due to the presence of carbon, rubidium-cesium potassium mainly exists in the calcined slag in the form of carbonate.
[0019] Preferably, the calcined slag and deionized water in S2 are mixed in a mass ratio of 1:4-5; the filter residue includes magnetic material and non-magnetic material; the magnetic material is Fe2O3, Fe3O4, MgFeO4; the non-magnetic material is MgO.
[0020] Preferably, the pH value of solution A in S3 is adjusted to 1-3; the amount of iodine ions added is calculated based on 100%-150% of the required amount of Cs3Bi2I9 to be formed.
[0021] Preferably, the amount of bismuth oxide added to S4 is calculated based on 100%-150% of the amount required to form Cs3Bi2I9.
[0022] Preferably, the solution C in S5 is added dropwise to the yellow solution B; the precipitation reaction equation is: 3Cs + +2Bi 3+ +9I - →Cs3Bi2I9.
[0023] Preferably, the solid-liquid separation in S6 is carried out by sedimentation filtration, and the solution is washed five times with an aqueous solution having a pH value of 1; the main purpose of the water washing is to wash away the rubidium and potassium entrained in the cesium iodine bismuthate, and the water having a pH value of 1 is used to prevent the cesium iodine bismuthate from decomposing.
[0024] Preferably, the red solid precipitate D of cesium in S7 is thermally decomposed in a vacuum environment or a protective atmosphere of nitrogen or argon at a temperature of 550-650°C; the decomposition equation is: Cs3Bi2I9→3CsI+2BiI3, the boiling point of cesium iodide is 1280°C, and the boiling point of bismuth iodide is 500°C. After thermal decomposition, the product cesium iodide is obtained, and the bismuth iodide is sublimated and collected to prepare a precipitant for recycling.
[0025] Preferably, the amount of iodide ions selected includes sodium iodide and potassium iodide.
[0026] The beneficial effects of the present invention are:
[0027] The invention uses bismuth ions and iodide ions as precipitants, adds bismuth ions and iodide ions into a solution containing rubidium and cesium potassium, and controls reaction conditions and the amount of the precipitant, so that the bismuth ions, iodide ions and cesium react to generate precipitated cesium iodide bismuthate, cesium and rubidium potassium can be separated, the rubidium content in the cesium iodide bismuthate is less than 0.2%, and the potassium and sodium contents are less than 0.1%, and the selective recovery of cesium in the rubidium and cesium potassium solution is almost achieved; in addition, cesium iodide with a purity greater than 99% can be directly obtained by thermal decomposition of the cesium iodide bismuthate, and the bismuth iodide can be recovered to continue to prepare the precipitant. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0030] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The present invention is further described according to the accompanying drawings and specific embodiments of the present invention, and the preferred implementation methods and materials described in the present invention are only for demonstration purposes.
[0031] like Figure 1 As shown:
[0032] Embodiment 1
[0033] 20 g of rubidium-cesium enriched material was calcined at 520°C for 2 h in an atmospheric atmosphere to obtain 17.6 g of calcined slag, with a weight loss rate of about 12%;
[0034] The roasted slag is leached with deionized water at a solid-liquid ratio of 1:3-5, and filtered with filter paper to obtain a rubidium-cesium enriched solution and leached slag; the mass of the leached slag accounts for about one-third of the roasted slag. The magnetic substances are mainly ferric oxide, ferroferric oxide and magnesium ferrite, and the non-magnetic substances are magnesium oxide;
[0035] The contents of rubidium and cesium in the rubidium and cesium enriched solutions were 17.3 g / L and 14.5 g / L, respectively, and the contents of potassium and sodium were 5 g / L and 2 g / L;
[0036] Add hydrochloric acid to 100 mL of rubidium-cesium enriched solution until the pH is 1, and add 4.9 g of sodium iodide while stirring continuously;
[0037] Take 1.69g of bismuth oxide and add appropriate amount of hydrochloric acid until the solid is completely dissolved, add the bismuth ion solution dropwise to the rubidium-cesium enriched solution, and after the addition is completed, continue stirring for 10 minutes, then filter with fast filter paper, and wash five times with weak acid solution with pH 1;
[0038] The solid precipitate was dried in an oven at 80 °C for 4 h to obtain 5.072 g of a red solid;
[0039] 5 g of the solid precipitate was placed in a quartz crucible and placed in a vacuum environment at 550° C. for 1 h to obtain 1.66 g of solid, which was analyzed and detected to be cesium iodide with a purity of 99%; 3.3 g of bismuth iodide was obtained in the vacuum tube wall.
[0040] Embodiment 2
[0041] Take 20g of rubidium-cesium enriched material, calcine it at 520℃ for 2h in air atmosphere to obtain 18g of calcined slag, with a weight loss rate of about 10%;
[0042] The roasted slag is leached with deionized water at a solid-liquid ratio of 1:3-5, and filtered with filter paper to obtain a rubidium-cesium enriched solution and leached slag; the mass of the leached slag accounts for about one-third of the roasted slag. The magnetic substances are mainly ferric oxide, ferroferric oxide and magnesium ferrite, and the non-magnetic substances are magnesium oxide;
[0043] The contents of rubidium and cesium in the rubidium and cesium enriched solutions were 17.3 g / L and 14.5 g / L, respectively, and the contents of potassium and sodium were 5 g / L and 2 g / L;
[0044] Add hydrochloric acid to 100 mL of rubidium-cesium enriched solution until the pH is 2, and add 5.88 g of sodium iodide while stirring continuously;
[0045] Take 2.028g of bismuth oxide and add appropriate amount of hydrochloric acid until the solid is completely dissolved, add the bismuth ion solution dropwise to the rubidium-cesium enriched solution, and after the addition is completed, continue stirring for 10 minutes, then filter with fast filter paper, and wash five times with weak acid solution with pH 1;
[0046] The solid precipitate was dried in an oven at 80 °C for 4 h to obtain 6.6 g of a red solid;
[0047] 5 g of the solid precipitate was placed in a quartz crucible and placed in a vacuum environment at 580° C. for 1 h to obtain 1.65 g of solid, which was analyzed and detected to be cesium iodide with a purity of 99%; 3.4 g of bismuth iodide was obtained in the vacuum tube wall.
[0048] Embodiment 3
[0049] 100 g of rubidium-cesium enriched material was calcined at 550°C for 5 h in an atmospheric atmosphere to obtain 85 g of calcined slag, with a weight loss rate of about 15%;
[0050] The roasted slag is leached with deionized water at a solid-liquid ratio of 1:3-5. After filtering with filter paper, a rubidium-cesium enriched solution and leached slag are obtained. The mass of the leached slag accounts for about one-third of the roasted slag. The magnetic substances are mainly ferric oxide, ferroferric oxide and magnesium ferrite, and the non-magnetic substances are magnesium oxide.
[0051] The contents of rubidium and cesium in the rubidium and cesium enriched solutions were 51 g / L and 40 g / L, respectively, and the contents of potassium and sodium were 10 g / L and 3 g / L;
[0052] Add hydrochloric acid to 50 mL of rubidium-cesium enriched solution until the pH is 1, and add 8.68 g of sodium iodide and continue stirring;
[0053] Take 3g of bismuth oxide and add appropriate amount of hydrochloric acid until the solid is completely dissolved, add the bismuth ion solution dropwise to the rubidium-cesium enriched solution, and after the addition is completed, continue stirring for 10 minutes, then filter with fast filter paper, and wash five times with weak acid solution with pH 1;
[0054] The solid precipitate was dried in an oven at 80 °C for 4 h to obtain 10.66 g of a red solid;
[0055] 10 g of the solid precipitate was placed in a quartz crucible and placed in a vacuum environment at 580°C for 1 h to obtain 3.4 g of solid, which was analyzed and detected to be cesium iodide with a purity of 99%, and 6.2 g of bismuth iodide was obtained in the vacuum tube wall.
[0056] Embodiment 4
[0057] 100 g of rubidium-cesium enriched material was calcined at 550°C for 5 h in an atmospheric atmosphere to obtain 85 g of calcined slag, with a weight loss rate of about 15%;
[0058] The roasted slag is leached with deionized water at a solid-liquid ratio of 1:3-5. After filtering with filter paper, a rubidium-cesium enriched solution and leached slag are obtained. The mass of the leached slag accounts for about one-third of the roasted slag. The magnetic substances are mainly ferric oxide, ferroferric oxide and magnesium ferrite, and the non-magnetic substances are magnesium oxide.
[0059] The contents of rubidium and cesium in the rubidium and cesium enriched solutions were 51 g / L and 40 g / L, respectively, and the contents of potassium and sodium were 10 g / L and 3 g / L;
[0060] Add hydrochloric acid to 300 mL of rubidium-cesium enriched solution until the pH is 1, and add 57.3 g of sodium iodide while stirring continuously;
[0061] Take 19.5g of bismuth oxide and add appropriate amount of hydrochloric acid until the solid is completely dissolved, add the bismuth ion solution dropwise to the rubidium-cesium enriched solution, and after the addition is completed, continue stirring for 10 minutes, then filter with fast filter paper, and wash five times with weak acid solution with pH 1;
[0062] The solid precipitate was dried in an oven at 80 °C for 4 h to obtain 64.38 g of a red solid;
[0063] Take 50g of the solid precipitate in a quartz crucible, place it in a vacuum environment at 580°C for 1h, and obtain 16g of solid in the quartz crucible, which is cesium iodide with a purity of 99% after analysis, and 33.8g of bismuth iodide is obtained in the vacuum tube wall.
[0064] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing cesium iodide from rubidium and cesium enriched materials, characterized in that: The method comprises the following steps: S1: Weigh an appropriate amount of rubidium-cesium enriched material, put it into a high-temperature calcining furnace for high-temperature calcination, and obtain calcined slag; S2: putting the roasted slag in S1 into a container filled with deionized water, so that the roasted slag is dissolved in the deionized water and allowed to stand, and after the dissolution is completed, filtering it to obtain solution A and filter residue; S3: adding an acidic solution to solution A in S2, adjusting the pH of solution A to acidic, and at the same time, adding an amount of iodine ions calculated according to the cesium concentration, and continuously stirring to obtain a yellow solution B; S4: weighing an appropriate amount of bismuth oxide, and then dissolving it in a container containing an appropriate amount of hydrochloric acid solution to obtain solution C; S5: adding the solution C in S4 to the yellow solution B in S3, stirring continuously, to obtain a red solid precipitate D containing cesium and a solution E containing rubidium; S6: performing solid-liquid separation on the red solid precipitate D containing cesium and the filtrate E containing rubidium in S5 to obtain a solid precipitate D containing cesium and a solution E containing rubidium; S7: placing the red solid precipitate D of cesium in S6 into a thermal decomposition device for thermal decomposition treatment to obtain a volatile product, bismuth iodide, and a residual product, cesium iodide.
2. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The rubidium-cesium enriched material in the S1 is calcined at a temperature of 500-600° C. in an atmospheric atmosphere.
3. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The calcined slag and deionized water in S2 are mixed in a mass ratio of 1:4-5; the filter residue includes magnetic material and non-magnetic material; the magnetic material is Fe2O3, Fe3O4, MgFeO4; the non-magnetic material is MgO.
4. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The pH value of solution A in S3 is adjusted to 1-3; the amount of iodine ions added is calculated based on 100%-150% of the required amount of Cs3Bi2I9 to be formed.
5. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The amount of bismuth oxide added to the S4 is calculated based on 100%-150% of the amount required to form Cs3Bi2I9.
6. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The solution C in S5 is added dropwise into the yellow solution B.
7. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The solid-liquid separation in S6 is carried out by sedimentation filtration, and the mixture is washed five times with an aqueous solution having a pH of 1.
8. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 1, characterized in that: The red solid precipitate D of cesium in the S7 is thermally decomposed in a vacuum environment or a protective atmosphere of nitrogen or argon at a temperature of 550-650°C.
9. A method for preparing cesium iodide from rubidium-cesium enriched material according to claim 4, characterized in that: The iodide ion amount can be selected from sodium iodide and potassium iodide.
Citation Information
Patent Citations
Method of separating and extracting rubidium and cesium from coal
CN107354323A
Method for separating and extracting battery-grade lithium carbonate and rubidium and cesium salts from lepidolite
CN110550644A
Method for extracting cesium and rubidium from lepidolite
CN111996392A
Method for separating rubidium and cesium from high-salt mother liquor
CN115522068A