A method for preparing a high-hardness hydrophobic SiO2 antireflection film by mixing an acid-catalyzed sol and a base-catalyzed sol

By using a mixed preparation method of acid-catalyzed and alkali-catalyzed sol, the problems of high transmittance, high hardness, and high adhesion of SiO₂ antireflective films were solved, and the preparation of high-hardness hydrophobic SiO₂ antireflective films with excellent weather resistance and self-cleaning properties was achieved.

CN118724475BActive Publication Date: 2026-11-20TIANJIN POLYTECHNIC UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202310318110.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2026-11-20
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously achieve high transmittance, high hardness, high adhesion, and hydrophobicity in SiO₂ antireflective films. In particular, alkaline catalytic films exhibit weak bonding and low porosity, while acid catalytic films demonstrate poor antireflective performance.

Method used

A mixed preparation method combining acid-catalyzed and base-catalyzed sols was adopted. By adjusting the ratio of tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and catalyst, a mixed sol was prepared, and a high-hardness hydrophobic SiO₂ antireflective film was formed on a glass substrate by dip-coating.

Benefits of technology

The transmittance increased by 5.17 percentage points in the wavelength range of 400–1100 nm, the water contact angle reached 91°, the adhesion reached level 0, the surface hardness reached 7H, and the transmittance changed by only 1.1% after 100 hours of UV irradiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HSB0000221702800000011
    Figure HSB0000221702800000011
  • Figure HSB0000221702800000012
    Figure HSB0000221702800000012
  • Figure HSB0000221702800000021
    Figure HSB0000221702800000021
Patent Text Reader

Abstract

The application discloses a preparation method of a high-hardness hydrophobic SiO2 antireflection film prepared by mixing an acid-catalyzed and base-catalyzed sol. Tetraethyl orthosilicate (TEOS) and methyl triethoxysilane (MTES) are used as precursors, anhydrous ethanol is used as a solvent, fatty alcohol polyoxyethylene ether (AEO) is used as a porogen, hydrochloric acid and ammonia are respectively used as catalysts to prepare acid-catalyzed and base-catalyzed silica sols, the two kinds of silica sols are mixed in proportion, the mixed sol is coated on glass by an immersion-drawing method, and a porous nano film is formed after drying and annealing. The average transmittance (coated glass transmittance) of the antireflection film in the range of 400-1100 nm is 92.51%, which is 5.17 percentage points higher than that of blank glass; the water contact angle of the film is 91 degrees, the pencil hardness reaches 7H, the adhesive force reaches the highest level 0, and the transmittance change is only 1.1% after 100 hours of ultraviolet irradiation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of antireflective thin film materials technology, specifically relating to a method for preparing high-hardness hydrophobic SiO2 antireflective thin films by acid-catalyzed and alkali-catalyzed sol-gel mixing. Background Technology

[0002] Anti-reflective films have a wide range of applications in the field of solar cells. Most solar panels are used outdoors or in the field, where the environment is relatively harsh. In addition to light transmittance, anti-reflective films must also have high mechanical properties (adhesion, hardness, etc.), good weather resistance (resistance to ultraviolet radiation, etc.) and a certain degree of self-cleaning ability.

[0003] Using tetraethyl orthosilicate as a precursor, silica sol can be prepared via alkaline or acid-catalyzed methods, and then coated onto glass surfaces using the dip-coating method to obtain antireflective films. Alkaline-catalyzed SiO2 films exhibit excellent antireflective properties due to their high porosity; however, the bonding between particles and between particles and the substrate is weak, making them easily damaged or detached from the substrate. Acid-catalyzed SiO2 exhibits a linear chain structure, allowing for the formation of chemical bonds between particles and between particles and the substrate, resulting in strong adhesion; however, its low porosity leads to poorer antireflective performance.

[0004] To achieve high mechanical and self-cleaning properties in sol-gel antireflective films, several studies have been conducted. Wang et al. [Chemical Physics Letters. 2020, 747: 137331] prepared SiO2 films with an uneven structure by mixing alkaline sols of different particle sizes. The films exhibited an average transmittance of 97.55% in the 380–1100 nm range and a contact angle of 141.38°, but their hardness and adhesion were not investigated. Zhi et al. [Applied Surface Science. 2018, 454: 239-248] synthesized a dual-scale high antireflective superhydrophobic film by introducing SiO2 nanoparticles into a nanoporous structure. This increased transmittance by 7 percentage points, achieved a contact angle of 157.9°, and a surface pencil hardness of 4H, but their adhesion was not characterized. Yuan et al. [Solar Energy. 2017, 155: 1366-1372] used ammonia to catalyze TEOS in the early stage of spherical SiO2 growth. After a period of time, hydrochloric acid was used as a catalyst to change the environment to acidic. As a result, the pencil hardness grade of the coating was 2B and the average transmittance increased by 6.3 percentage points. Then, polymethylhydrosiloxane (PMHS) was used for surface treatment, and the pencil hardness grade was further increased to 5H. The adhesion and wettability were not characterized. Ye et al. [Solar Energy Materials and Solar Cells. 2011, 95(8): 2347-2351] used tetraethyl silicate as a precursor and prepared an antireflective film with high transmittance and high wear resistance by acid / base two-step catalytic sol-gel method. Then, hexamethyldisilazane was used for surface modification. When the acid / base catalytic sol molar ratio was 0.5, the contact angle was 72.51° and the maximum transmittance at 630 nm increased by 6.5 percentage points. The hardness and adhesion of the film were not characterized.

[0005] Chinese patent CN 107863393 A discloses a method for preparing solar photovoltaic glass with a micro / nano antireflective layer. The method involves plasma etching and nanoimprinting to prepare the solar photovoltaic glass with the micro / nano antireflective layer, increasing the transmittance by 3 percentage points and achieving a contact angle of 119°. This method requires the use of photoresist and vacuum imprinting equipment. Chinese patent CN112442669 A discloses a method for preparing a self-cleaning antireflective film. First, a thin film is deposited on the glass surface using magnetron sputtering, and then etched with a specific solution to obtain a SiO2 thin film. The refractive index of the crystalline silicon dioxide film is 1.21–1.32, and the water contact angle is 137–141°. However, the hardness and adhesion of the film are not characterized, and this method is complex. Chinese patent CN 112661415 A discloses an antireflective film for photovoltaic glass and its preparation method. The antireflective film is composed of a main antireflective layer close to the glass substrate and an auxiliary antireflective layer disposed on the main antireflective layer. The transmittance of the antireflective film is increased by 3%, and the pencil hardness is 5H. However, the adhesion and contact angle are not characterized. Chinese patent CN 113387597 B discloses a superhydrophobic antireflective film and photovoltaic glass. An alkaline-catalyzed nano-SiO2 sol is coated onto the surface of K9 photovoltaic glass using an dip-coating method. The transmittance of this antireflective film is 94.7%, and the contact angle is 156.7°. However, the hardness and adhesion of the film are not studied. Chinese patent CN 109502987 B discloses a method for preparing a high-hardness antireflective film based on hollow silica. This method uses tetraethyl orthosilicate as a raw material, polyacrylic acid as a template agent, 2-isopropoxyethanol and methanol as solvents, and ammonia as a catalyst. Hollow SiO2 sol is prepared using a template method, and a coating is deposited on a glass substrate using an dip-coating method. After calcination at 550℃, the resulting film has an average transmittance of over 98% in the 400-800 nm wavelength range, but its hardness is only 4H. The adhesion and wettability of the film were not characterized. Chinese patent CN 105399340 A discloses a superhydrophobic high-transmission antireflective film and its preparation method. A hybrid sol doped with trimethylchlorosilane is prepared, and a coating is formed on the surface of a glass slide using an dip-coating method. After drying, a superhydrophobic high-transmission antireflective film is obtained, with a transmittance increase of 5.56 percentage points and a contact angle of 106°. The hardness and adhesion of the film were not tested. Summary of the Invention

[0006] The technical problem this invention aims to solve is to overcome the shortcomings of existing technologies and provide a method for preparing high-hardness, hydrophobic SiO2 antireflective films using acid-catalyzed and alkali-catalyzed sol-gel mixing. The antireflective film prepared by this invention exhibits high transmittance, high hardness, high adhesion, and hydrophobicity. The average transmittance in the wavelength range of 400–1100 nm is 92.51%, which is 5.17 percentage points higher than the average transmittance of blank glass. The water contact angle of the antireflective film can reach 91°. The film's adhesion is at the highest level (0) using the tape method, and the surface hardness reaches 7H using the pencil method. After 100 hours of ultraviolet irradiation, the transmittance changes by only 1.1%.

[0007] To solve the technical problem of this invention, the adopted technical solution is a method for preparing a high-hardness hydrophobic SiO2 antireflection film by mixing acid-catalyzed and alkali-catalyzed sols. The specific operation steps are as follows:

[0008] S1. Preparation of acid-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid in a volume ratio of 1:(0.1~3.0):10:0.3:(0.1~0.5) were added sequentially to a pre-cleaned beaker and stirred at 200-1000 r / min at room temperature for 1-5 h. The mixture was then transferred to an Erlenmeyer flask and incubated in a water bath at 50-100℃ for 1-5 h. AEO was added to the sol and mixed, wherein the volume ratio of AEO to silane (tetraethyl silicate + methyltriethoxysilane) was 0.1-45%. The mixture was aged for 1-5 days to obtain the desired acid-catalyzed silica sol.

[0009] S2. Preparation of alkaline-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, and ammonia water are added sequentially to a pre-cleaned beaker in a volume ratio of 1:(0.1~3.0):15:(0.1~0.7). The mixture is stirred at 200-1000 r / min at room temperature for 0.5~12 h and aged for 1~5 days to obtain the desired alkaline-catalyzed silica sol.

[0010] S3. Preparation of mixed sol: The alkaline catalytic silica sol is refluxed in a water bath at 50-100℃ for 6-24 hours. After cooling to room temperature, the acid catalytic silica sol is mixed with the alkaline catalytic silica sol at a volume ratio of 5-95%. The mixture is stirred at room temperature for 1-5 hours and aged for 12-72 hours to obtain the desired mixed sol.

[0011] S4. Preparation of antireflective film: The antireflective film was prepared by dip-coating at a speed of 100-3000 μm / s. The coated glass substrate was then dried in an oven at 50-80℃ for 1-5 hours, and then placed in a muffle furnace at 300-500℃ for 1-5 hours. After natural cooling, a high-hardness hydrophobic SiO2 antireflective film was prepared by mixing acid-catalyzed and alkali-catalyzed sol. Attached Figure Description

[0012] Figure 1 The transmittance spectrum (a) and average transmittance (b) of the high-hardness hydrophobic SiO2 antireflection film prepared by acid catalysis and alkali catalysis sol mixing provided in the embodiments of the present invention are shown.

[0013] Figure 2 The contact angle of the high-hardness hydrophobic SiO2 antireflective film prepared by mixing acid-catalyzed and alkali-catalyzed sols provided in this embodiment of the invention varies with the volume ratio of acid-catalyzed silica sol to alkali-catalyzed silica sol.

[0014] Figure 3 This is an adhesion diagram of the high-hardness hydrophobic SiO2 antireflective film prepared by mixing acid-catalyzed and alkali-catalyzed sols according to the embodiments of the present invention; the volume ratios of acid-catalyzed silica sol and alkali-catalyzed silica sol are (a) 0%, (b) 10%, (c) 20%, (d) 30%, and (e) 40%, respectively; the adhesion of the film was tested according to GB / T 33049-2016, and the figure shows cross-cut adhesion marks. Based on this, it can be determined that the adhesion of embodiments 2 to 5 reached level 0.

[0015] Figure 4 This is a surface hardness diagram of a high-hardness hydrophobic SiO2 antireflection film prepared by mixing acid-catalyzed and alkali-catalyzed sols according to an embodiment of the present invention. The volume ratios of acid-catalyzed silica sol and alkali-catalyzed silica sol are 0 in (a) and (b), and 30% in (c) and (d). The surface hardness of the film was tested according to (GB / T 6739-2006). The figure shows the scratch marks of an 8H pencil, which indicates that the hardness of the fourth embodiment reached 7H. Detailed Implementation

[0016] A method for preparing a high-hardness hydrophobic SiO2 antireflective film by mixing acid-catalyzed and alkali-catalyzed silica sols, wherein the SiO2 antireflective film is prepared by mixing acid-catalyzed silica sols and alkali-catalyzed silica sols.

[0017] The present invention will be further described in detail below with reference to embodiments:

[0018] Example 1:

[0019] To compare the modifying effect of acid-catalyzed silica sol, an alkaline-catalyzed SiO2 antireflection film was first prepared. The preparation method includes the following steps:

[0020] 1. Preparation of alkaline-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water, and ammonia water were added sequentially to a pre-cleaned beaker in a volume ratio of 1:1:15:0.5. The mixture was stirred at 200-1000 r / min at room temperature for 0.5-12 h and aged for 1-5 days to obtain the desired alkaline-catalyzed silica sol.

[0021] 2. Preparation of antireflective film: The antireflective film was deposited using the dip-coating method with a coating speed of 100-3000 μm / s. The deposited glass substrate was then placed in an oven at 50-80℃ and dried for 1-5 hours. After drying, it was placed in a muffle furnace and kept at 300-500℃ for 1-5 hours. Then it was naturally cooled to obtain the alkali-catalyzed SiO2 antireflective film.

[0022] Example 2:

[0023] A method for preparing high-hardness hydrophobic SiO2 antireflective films by acid-catalyzed and base-catalyzed sol-gel mixing includes the following steps:

[0024] 1. Preparation of acid-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid in a volume ratio of 1:1:10:0.3:0.3 were added sequentially to a pre-cleaned beaker and stirred at 200-1000 r / min for 1-5 h. The mixture was then transferred to an Erlenmeyer flask and incubated in a water bath at 50-100℃ for 1-5 h. AEO was added to the sol and mixed, wherein the volume ratio of AEO to Si(TEOS+MTES) was 45%. The mixture was aged for 1-5 days to obtain the desired acid-catalyzed silica sol.

[0025] 2. Preparation of alkaline-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, and ammonia water in a volume ratio of 1:1:15:0.5 were added sequentially to a pre-cleaned beaker, stirred at 200-1000 r / min for 0.5-12 h, and aged for 1-5 days to obtain the desired alkaline-catalyzed silica sol.

[0026] 3. Preparation of mixed sol: The alkaline catalytic silica sol was refluxed in a water bath at 50-100℃ for 6-24 hours. After cooling to room temperature, the acid catalytic silica sol was mixed with the alkaline catalytic silica sol at a volume ratio of 10%. The mixture was stirred at room temperature for 1-5 hours and aged for 12-72 hours to obtain the desired mixed sol.

[0027] 4. Preparation of antireflective film: The antireflective film was prepared by dip-coating method with a coating speed of 100-3000 μm / s. The coated glass substrate was then dried in an oven at 50-80℃ for 1-5 hours, and then placed in a muffle furnace at 300-500℃ for 1-5 hours. After natural cooling, a high-hardness hydrophobic SiO2 antireflective film was prepared by mixing acid-catalyzed and alkali-catalyzed sol.

[0028] Example 3:

[0029] A method for preparing high-hardness hydrophobic SiO2 antireflective films by acid-catalyzed and base-catalyzed sol-gel mixing includes the following steps:

[0030] 1. Preparation of acid-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid in a volume ratio of 1:1:10:0.3:0.3 were added sequentially to a pre-cleaned beaker and stirred at 200-1000 r / min for 1-5 h. The mixture was then transferred to an Erlenmeyer flask and incubated in a water bath at 50-100℃ for 1-5 h. AEO was added to the sol and mixed, wherein the volume ratio of AEO to Si(TEOS+MTES) was 45%. The mixture was aged for 1-5 days to obtain the desired acid-catalyzed silica sol.

[0031] 2. Preparation of alkaline-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, and ammonia water in a volume ratio of 1:1:15:0.5 were added sequentially to a pre-cleaned beaker, stirred at 200-1000 r / min for 0.5-12 h, and aged for 1-5 days to obtain the desired alkaline-catalyzed silica sol.

[0032] 3. Preparation of mixed sol: The alkaline catalytic silica sol was refluxed in a water bath at 50-100℃ for 6-24 hours. After cooling to room temperature, the acid catalytic silica sol was mixed with the alkaline catalytic silica sol at a volume ratio of 20%. The mixture was stirred at room temperature for 1-5 hours and aged for 12-72 hours to obtain the desired mixed sol.

[0033] 4. Preparation of antireflective film: The antireflective film was deposited using the dip-coating method with a coating speed of 100-3000 μm / s. The deposited glass substrate was then dried in an oven at 50-80℃ for 1-5 hours, and then placed in a muffle furnace at 300-500℃ for 1-5 hours. After natural cooling, a high-hardness hydrophobic SiO2 antireflective film was prepared by mixing acid-catalyzed and alkali-catalyzed sol.

[0034] Example 4:

[0035] A method for preparing high-hardness hydrophobic SiO2 antireflective films by acid-catalyzed and base-catalyzed sol-gel mixing includes the following steps:

[0036] 1. Preparation of acid-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid in a volume ratio of 1:1:10:0.3:0.3 were added sequentially to a pre-cleaned beaker and stirred at 200-1000 r / min for 1-5 h. The mixture was then transferred to an Erlenmeyer flask and incubated in a water bath at 50-100℃ for 1-5 h. AEO was added to the sol and mixed, wherein the volume ratio of AEO to Si(TEOS+MTES) was 45%. The mixture was aged for 1-5 days to obtain the desired acid-catalyzed silica sol.

[0037] 2. Preparation of alkaline-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, and ammonia water in a volume ratio of 1:1:15:0.5 were added sequentially to a pre-cleaned beaker, stirred at 200-1000 r / min for 0.5-12 h, and aged for 1-5 days to obtain the desired alkaline-catalyzed silica sol.

[0038] 3. Preparation of mixed sol: The alkaline catalytic silica sol was refluxed in a water bath at 50-100℃ for 1-5 hours. After cooling to room temperature, the acid catalytic silica sol was mixed with the alkaline catalytic silica sol at a volume ratio of 30%. The mixture was stirred at room temperature for 1-5 hours and aged for 12-72 hours to obtain the desired mixed sol.

[0039] 4. Preparation of antireflective film: The antireflective film was deposited using the dip-coating method with a coating speed of 100-3000 μm / s. The deposited glass substrate was then dried in an oven at 50-80℃ for 1-5 hours, and then placed in a muffle furnace at 300-500℃ for 1-5 hours. After natural cooling, a high-hardness hydrophobic SiO2 antireflective film was prepared by mixing acid-catalyzed and alkali-catalyzed sol.

[0040] Example 5:

[0041] A method for preparing high-hardness hydrophobic SiO2 antireflective films by acid-catalyzed and base-catalyzed sol-gel mixing includes the following steps:

[0042] 1. Preparation of acid-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, deionized water and concentrated hydrochloric acid in a volume ratio of 1:1:10:0.3:0.3 were added sequentially to a pre-cleaned beaker and stirred at 200-1000 r / min for 1-5 h. The mixture was then transferred to an Erlenmeyer flask and incubated in a water bath at 50-100℃ for 1-5 h. AEO was added to the sol and mixed, wherein the volume ratio of AEO to Si(TEOS+MTES) was 45%. The mixture was aged for 1-5 days to obtain the desired acid-catalyzed silica sol.

[0043] 2. Preparation of alkaline-catalyzed silica sol: Tetraethyl silicate, methyltriethoxysilane, anhydrous ethanol, and ammonia water in a volume ratio of 1:1:15:0.5 were added sequentially to a pre-cleaned beaker, stirred at 200-1000 r / min for 0.5-12 h, and aged for 1-5 days to obtain the desired alkaline-catalyzed silica sol.

[0044] 3. Preparation of mixed sol: The alkaline catalytic silica sol was refluxed in a water bath at 50-100℃ for 1-5 hours. After cooling to room temperature, the acid catalytic silica sol was mixed with the alkaline catalytic silica sol at a volume ratio of 40%. The mixture was stirred at room temperature for 1-5 hours and aged for 12-72 hours to obtain the desired mixed sol.

[0045] 4. Preparation of antireflective film: The antireflective film was deposited using the dip-coating method with a coating speed of 100-3000 μm / s. The deposited glass substrate was then dried in an oven at 50-80℃ for 1-5 hours, and then placed in a muffle furnace at 300-500℃ for 1-5 hours. After natural cooling, a high-hardness hydrophobic SiO2 antireflective film was prepared by mixing acid-catalyzed and alkali-catalyzed sol.

[0046] Acid-catalyzed silica sol alters the transmittance of SiO2 films. With increasing acid-catalyzed silica sol concentration, more pores are formed after annealing, gradually increasing the transmittance, as shown in the attached figure. Figure 1 The transmittance spectrum of a thin film is shown.

[0047] Acid-catalyzed silica sol alters the wettability of SiO2 films. With increasing acid-catalyzed silica sol concentration, the film roughness and contact angle increase. However, with excessive acid-catalyzed silica sol, the film particles are entirely occupied by acid-catalyzed SiO2 particles, resulting in decreased roughness and a lower contact angle, as shown in the attached figure. Figure 2 A schematic diagram of the contact angle of a thin film is shown.

[0048] Acid-catalyzed silica sol alters the adhesion and hardness of SiO2 films. With increasing acid catalysis, the number of chemical bonds between particles increases, leading to improved adhesion and hardness. Figure 3 and Figure 4 .

[0049] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high-hardness hydrophobic SiO2 antireflective film by mixing acid-catalyzed and base-catalyzed sols, characterized in that, Acid-catalyzed silica sol and alkali-catalyzed silica sol were prepared using tetraethyl silicate (TEOS) and methyltriethoxysilane (MTES) as precursors and anhydrous ethanol as solvent, respectively, with hydrochloric acid and ammonia as catalysts. Fatty alcohol polyoxyethylene ether (AEO) was added as a pore-forming agent to the acid-catalyzed silica sol. The alkali sol was refluxed in a water bath, and the acid-catalyzed silica sol and alkali-catalyzed silica sol were mixed at a volume ratio of 5-95% to prepare a mixed sol. The mixed sol was then coated onto glass using the dip-coating method. During annealing, the AEO inside the coating volatilized to form a micro-nano porous structure. After annealing, a high-hardness, hydrophobic, and UV-resistant SiO2 antireflective film was obtained.

2. The method for preparing a high-hardness hydrophobic SiO2 antireflective film by mixing acid-catalyzed and alkali-catalyzed sols as described in claim 1, characterized in that, The preparation method of the acid-catalyzed and base-catalyzed mixed sol is as follows: S1. Preparation of acid-catalyzed silica sol: TEOS, MTES, anhydrous ethanol, deionized water and concentrated hydrochloric acid in a volume ratio of 1:(0.1~3.0):10:0.3:(0.1~0.5) were added to a pre-cleaned beaker and stirred at 200-1000 r / min for 1~5 h. Then the mixture was transferred to an Erlenmeyer flask and heated in a water bath at 50~100℃ for 1~5 h. AEO was added to the sol and mixed, wherein the volume ratio of AEO to silane (TEOS+MTES) was 0.1-45%. The mixture was aged for 1~5 days to obtain the desired acid-catalyzed silica sol. S2. Preparation of alkaline-catalyzed silica sol: TEOS, MTES, anhydrous ethanol, and ammonia water in a volume ratio of 1:(0.1~3.0):15:(0.1~0.7) are added to a pre-cleaned beaker, stirred at 200-1000 r / min for 0.5~12 h, and aged for 1~5 days to obtain the desired alkaline-catalyzed silica sol; S3. Preparation of mixed sol: The alkaline catalytic silica sol is refluxed in a water bath at 50-100℃ for 6-24h and cooled to room temperature. Then, the acid catalytic silica sol and the alkaline catalytic silica sol are mixed at a volume ratio of 5-95%, stirred at room temperature for 1-5h, and aged for 12-72h to obtain the desired mixed sol.

3. The method for preparing a high-hardness hydrophobic SiO2 antireflective film by mixing acid-catalyzed and alkali-catalyzed sols as described in claim 1, characterized in that, The mixed sol was coated onto glass using an dip-coating method at a speed of 10–3000 μm / s. The coated glass substrate was then placed in an oven at 50–80 °C and dried for 1–5 h. After drying, it was placed in a muffle furnace and annealed at 200–500 °C for 1–5 h to obtain a high-hardness hydrophobic SiO2 antireflective film prepared by mixing acid-catalyzed and alkali-catalyzed sols.

4. The method for preparing a high-hardness hydrophobic SiO2 antireflective film by mixing acid-catalyzed and alkali-catalyzed sols as described in claim 1, characterized in that, The film exhibits excellent antireflection performance in the visible light range (400–1100 nm), with an average transmittance of 92.51% in the 400–1100 nm wavelength range, which is 5.17 percentage points higher than that of blank glass. The antireflection film also has a certain degree of hydrophobic self-cleaning function, with a water contact angle of 91°. It has good mechanical properties, with adhesion at the highest level of 0 using the tape method and a surface hardness of 7H using the pencil method. After 100 hours of strong ultraviolet irradiation, the transmittance changes by only 1.1%.

Citation Information

Patent Citations

  • Super-hydrophobic high-transmittance SiO2 anti-reflecting thin film and preparation method thereof

    CN105399340A

  • Preparation method of solar photovoltaic glass with micro-nano antireflection layer

    CN107863393A

  • A method for preparing high-hardness antireflective films based on hollow silica

    CN109502987B

  • Preparation method for self-cleaning antireflection film

    CN112442669A

  • Antireflection film layer for photovoltaic glass, preparation method of antireflection film layer and solar cell module

    CN112661415A