Geopolymer bonded silicon carbide refractory and method of making

By using geopolymer binders to prepare refractory materials with silicon carbide, the problems of easy oxidation and porosity of existing materials at high temperatures have been solved, realizing the preparation of low-cost, high-performance silicon carbide refractory materials with excellent oxidation resistance and thermal shock resistance.

CN118724600BActive Publication Date: 2026-11-24TAIZHOU WANGXIN REFRACTORIES CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410782843.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2026-11-24
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing silicon carbide refractory materials are prone to oxidation at high temperatures and have secondary pores or voids, which leads to a decrease in mechanical strength, thermal conductivity and erosion resistance, and also result in high production costs and complex processes.

Method used

Geopolymers are used as binders. Geopolymer sol is formed by aluminum silicate powder and phosphoric acid activator. It is then mixed with silicon carbide, pressed into shape, and sintered at low temperature in air atmosphere to generate ceramic bonding phases such as mullite, forming a core-shell structure and avoiding oxidation and pore formation.

Benefits of technology

It improves the density and strength of the material, reduces production costs, enables high-temperature sintering in an air atmosphere, has good oxidation resistance and thermal shock resistance, low apparent porosity, and excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724600B_ABST
    Figure CN118724600B_ABST
Patent Text Reader

Abstract

This invention discloses a geopolymer-bonded silicon carbide refractory material and its preparation method. The refractory material is composed of the following substances in weight percentage: 70-90 wt% silicon carbide, 7-21 wt% aluminum silicate powder, 1-3 wt% phosphoric acid activator, and 2-6 wt% water as raw materials. The beneficial effects of this invention are that it is low in cost, simple in process, feasible and efficient, and low in carbon, green and pollution-free. The prepared geopolymer-bonded silicon carbide refractory material has uniform pore distribution, excellent mechanical properties, excellent oxidation resistance and excellent thermal shock resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicon carbide refractory materials technology, specifically to a geopolymer-bonded silicon carbide refractory material and its preparation method. Background Technology

[0002] Silicon carbide (SiC) materials have excellent properties such as high mechanical strength, low coefficient of thermal expansion, strong thermal shock resistance and chemical corrosion resistance, and are widely used in metallurgy, energy and chemical industries. SiC has strong covalent bonds, making it difficult to sinter. A second phase is typically added to obtain a dense silicon carbide sintered body. The second phase of SiC refractories includes clay, silica, mullite, silicon nitride, silicon oxynitride, and silane, among others. Based on the type of bonding phase, SiC refractories can be classified into oxide-bonded silicon carbide, nitride-bonded silicon carbide, and self-bonded silicon carbide. However, existing SiC refractories have the following significant problems: ① Oxide-bonded silicon carbide refractories have a simple production process, but oxides are prone to creep at high temperatures, making them unsuitable for high-temperature applications; ② Nitride-bonded silicon carbide refractories have higher operating temperatures, but the process is complex, production costs are high, and there is thermal mismatch between nitrides and silicon carbide; ③ Self-bonded silicon carbide refractories have high synthesis temperatures, high production costs, high energy consumption, and residual carbon and free silicon degrade their high-temperature performance.

[0003] When sintered in an unprotected atmosphere or used at high temperatures, the surfaces of nitride-bonded silicon carbide and self-bonded silicon carbide refractories are easily oxidized, and it is impossible to avoid the presence of amorphous silica or cristobalite residues in the neck, which seriously affects the performance of silicon carbide products. Oxide-bonded silicon carbide can be sintered under an oxidizing atmosphere at normal pressure, with relatively low production costs, and is currently the most common bonding method for silicon carbide products. The preparation of SiC refractory products adopts coarse, medium, and fine graded batching, using silicon carbide and the bonding phase as raw materials. To ensure sufficient green strength, a temporary binder is selected, the raw materials are pressed into shape, and then fired at 1200-1400℃. Commonly used binders include organic binders such as pulp waste liquor, dextrin, resin, and polyvinyl alcohol. However, the loss of such binders during firing will generate secondary pores or voids in the material structure, resulting in a decrease in mechanical strength, thermal conductivity, erosion resistance, and wear resistance. Summary of the Invention

[0004] The purpose of this invention is to solve the above-mentioned problems by designing a geopolymer-bonded silicon carbide refractory material and its preparation method.

[0005] To achieve the above objectives, the technical solution of the present invention is a geopolymer-bonded silicon carbide refractory material, which is composed of the following substances in weight percentage: 70-90 wt% silicon carbide, 7-21 wt% aluminum silicate powder, 1-3 wt% phosphoric acid activator and 2-6 wt% water as raw materials.

[0006] A method for preparing a geopolymer-bonded silicon carbide refractory material includes the following steps:

[0007] Step 1: First, mechanically mix aluminum silicate powder, phosphoric acid activator, and water to obtain geopolymer sol;

[0008] Step 2: Stir the sol and silicon carbide evenly; press and mold under 80-200 MPa, then dry at 110℃ for 48 hours, heat to 1200-1400℃ in air at a rate of 2-10℃ / min, hold for 2-5 hours, and cool to room temperature in the furnace.

[0009] Step 3: Prepare geopolymer-bonded silicon carbide refractory material.

[0010] As a further supplement to this technical solution, the silicon carbide contains ≥98wt% SiC and has a particle size ≤3mm.

[0011] As a further supplement to this technical solution, the aluminum silicate powder is one or more of pyrophyllite, kaolinite, sillimanite, vermiculite and mica in combination.

[0012] As a further supplement to this technical solution, the phosphoric acid activator is one or more combinations of orthophosphoric acid, phosphorous acid, metaphosphoric acid, and polyphosphoric acid.

[0013] Its beneficial effects are as follows: This invention uses geopolymers as the forming binder for silicon carbide refractory materials. Geopolymers are a type of inorganic polymer sol with a three-dimensional network structure of silicon-oxygen tetrahedra and aluminum-oxygen tetrahedra, which can avoid the secondary pores or voids generated during the firing process of traditional organic binders, effectively improving the density and strength of the product. This invention uses natural aluminum silicate minerals as raw materials to obtain geopolymer binders, which form high-temperature ceramic bonding phases such as mullite, anorthite, cordierite, and olivine in situ under calcination conditions. The small amount of alkali metal impurities in the mineral raw materials can reduce the formation temperature of the ceramic bonding phase and realize the low-temperature densification sintering of silicon carbide refractory materials. This invention forms a coating on the surface of silicon carbide particles through geopolymer sol binders. During the drying process, polymerization occurs to form a gel, providing initial strength for the green body. During the firing process, a ceramic bonding phase is generated in situ on the surface of silicon carbide, forming a uniform coating to form a core-shell structure (silicon carbide as the core and the ceramic bonding phase as the shell). This invention provides bonding strength to the material while preventing silicon carbide from contacting oxygen-containing gases, enabling the sintering of silicon carbide refractories in an air atmosphere and improving the material's oxidation resistance. The aluminosilicate raw materials used in this invention include pyrophyllite, kaolin, sillimanite, vermiculite, and mica, all commonly used raw materials in the ceramics industry. These materials are readily available and inexpensive, reducing the material's preparation cost. The geopolymer-bonded silicon carbide refractories prepared by this invention have the following characteristics: apparent porosity of 10-20%; room temperature flexural strength of 20-50 MPa; compressive strength of 150-300 MPa; residual flexural strength retention (thermal shock resistance) of 50-90% (after three water coolings at 1100℃); and good erosion and oxidation resistance. This invention is characterized by low cost, simple process, feasibility, high efficiency, and low carbon footprint with no pollution. The prepared geopolymer-bonded silicon carbide refractories exhibit uniform pore distribution, excellent mechanical properties, superior oxidation resistance, and excellent thermal shock resistance. Attached Figure Description

[0014] Figure 1 The XRD pattern of a geopolymer-bonded silicon carbide refractory material prepared according to the present invention;

[0015] Figure 2 This is a microstructure diagram of a geopolymer-bonded silicon carbide refractory material prepared according to the present invention. Detailed Implementation

[0016] To facilitate a clearer understanding of this technical solution by those skilled in the art, the technical solution of the present invention will be described in detail below with reference to embodiments:

[0017] To avoid repetition, the raw materials involved in this specific embodiment are described uniformly as follows, and will not be repeated in the examples: the silicon carbide has a SiC content ≥98wt% and a particle size ≤3mm; the aluminum silicate powder is one or more of pyrophyllite, kaolin, sillimanite, vermiculite, and mica; the phosphoric acid activator is one or more of orthophosphoric acid, phosphorous acid, metaphosphoric acid, and polyphosphoric acid; the implementation scheme will be described in detail below:

[0018] Example 1

[0019] A method for preparing a geopolymer-bonded silicon carbide refractory material uses 70-75 wt% silicon carbide, 17-21 wt% aluminum silicate powder, 1-2 wt% phosphoric acid activator, and 5-6 wt% water as raw materials. First, the aluminum silicate powder, phosphoric acid activator, and water are mechanically mixed to obtain a geopolymer sol. Then, the sol is stirred evenly with silicon carbide. The mixture is pressed into shape under 80-100 MPa conditions, dried at 110°C for 48 hours, and then heated to 1200-1300°C in air at a rate of 2-5°C / min, held at that temperature for 2-3 hours, and then cooled to room temperature in the furnace to obtain the geopolymer-bonded silicon carbide refractory material.

[0020] In this embodiment: the aluminum silicate powder is 8-9 wt% pyrophyllite and 9-12 wt% kaolin powder; the phosphoric acid is 0.5-1 wt% orthophosphoric acid and 0.5-1 wt% phosphorous acid.

[0021] The geopolymer-bonded silicon carbide refractory material prepared by this invention was tested and found to have the following characteristics: apparent porosity of 15-20%; flexural strength at room temperature of 20-30 MPa; compressive strength of 150-200 MPa; and residual flexural strength retention rate (thermal shock stability) of 50-60% (after 3 water coolings at 1100℃).

[0022] Example 2

[0023] A method for preparing a geopolymer-bonded silicon carbide refractory material, using 75-80 wt% silicon carbide, 15-19 wt% aluminum silicate powder, 1-2 wt% phosphoric acid activator, and 4-6 wt% water as raw materials; firstly, the aluminum silicate powder, phosphoric acid activator, and water are mechanically mixed to obtain a geopolymer sol; then, the sol is stirred evenly with silicon carbide; the mixture is pressed into shape under 100-150 MPa conditions, dried at 110℃ for 48 hours, heated to 1200-1300℃ in air at a rate of 2-5℃ / min, held at that temperature for 2-3 hours, and then cooled to room temperature in the furnace to obtain the geopolymer-bonded silicon carbide refractory material. Figure 1 The XRD pattern of the product in this embodiment shows that the phase composition is silicon carbide and cordierite.

[0024] In this embodiment: the aluminum silicate powder consists of 2-4 wt% kaolin, 4-5 wt% sillimanite and 9-10 wt% vermiculite powder; the phosphoric acid consists of 0.5-1 wt% orthophosphoric acid, 0.25-0.5 wt% phosphorous acid and 0.25-0.5 wt% metaphosphoric acid.

[0025] The geopolymer-bonded silicon carbide refractory material prepared by this invention was tested and found to have the following characteristics: apparent porosity of 10-15%; room temperature flexural strength of 30-40 MPa; compressive strength of 200-250 MPa; and residual flexural strength retention rate (thermal shock stability) of 60-70% (after 3 water coolings at 1100℃).

[0026] Example 3

[0027] A method for preparing a geopolymer-bonded silicon carbide refractory material, using 80-85 wt% silicon carbide, 9-15 wt% aluminum silicate powder, 2-3 wt% phosphoric acid activator, and 3-4 wt% water as raw materials; firstly, the aluminum silicate powder, phosphoric acid activator, and water are mechanically mixed to obtain a geopolymer sol; then, the sol is stirred evenly with silicon carbide; the mixture is pressed into shape under 100-150 MPa conditions, dried at 110°C for 48 hours, heated to 1300-1400°C in air at a rate of 2-5°C / min, held at that temperature for 3-5 hours, and then cooled to room temperature in the furnace to obtain the geopolymer-bonded silicon carbide refractory material. Figure 1 The XRD pattern of the product in this embodiment shows that the phase composition is silicon carbide and cordierite.

[0028] In this embodiment: the aluminum silicate powder consists of 2-3 wt% kaolin, 2-3 wt% sillimanite, 4-7 wt% vermiculite, and 1-2 wt% mica powder; the phosphoric acid consists of 1-1.5 wt% orthophosphoric acid, 0.5-0.75 wt% phosphorous acid, and 0.5-0.75 wt% metaphosphoric acid.

[0029] The geopolymer-bonded silicon carbide refractory material prepared by this invention was tested and found to have the following characteristics: apparent porosity of 10-15%; room temperature flexural strength of 30-40 MPa; compressive strength of 200-250 MPa; and residual flexural strength retention rate (thermal shock stability) of 70-80% (after 3 water coolings at 1100℃).

[0030] Example 4

[0031] A method for preparing a geopolymer-bonded silicon carbide refractory material, comprising: 85-90 wt% silicon carbide, 7-10 wt% pyrophyllite, kaolin, sillimanite, vermiculite and mica powder, 2-3 wt% orthophosphoric acid, phosphorous acid, metaphosphoric acid and polyphosphoric acid activator, and 2-3 wt% water as raw materials; firstly, mechanically mixing aluminosilicate powder, phosphoric acid activator and water to obtain a geopolymer sol; then, stirring the sol with silicon carbide until uniform; pressing and molding under 150-200 MPa, then drying at 110℃ for 48 hours, heating to 1300-1400℃ in air at a rate of 5-10℃ / min, holding at that temperature for 3-5 hours, and then cooling to room temperature in the furnace to obtain the geopolymer-bonded silicon carbide refractory material.

[0032] In this embodiment: the aluminum silicate powder consists of 1.5–2 wt% pyrophyllite, 0.5–1 wt% kaolin, 1.5–2 wt% sillimanite, 3–4 wt% vermiculite, and 0.5–1 wt% mica powder; the phosphoric acid consists of 1–1.25 wt% orthophosphoric acid, 0.25–0.5 wt% phosphorous acid, 0.25–0.5 wt% metaphosphoric acid, and 0.5–0.75 wt% polyphosphoric acid;

[0033] The geopolymer-bonded silicon carbide refractory material prepared by this invention was tested and found to have the following characteristics: apparent porosity of 10-15%; room temperature flexural strength of 40-50 MPa; compressive strength of 250-300 MPa; and residual flexural strength retention rate (thermal shock stability) of 80-90% (after 3 water coolings at 1100℃).

[0034] The above technical solutions only embody the preferred technical solutions of the present invention. Any modifications that may be made by those skilled in the art to certain parts thereof embody the principles of the present invention and fall within the protection scope of the present invention.

Claims

1. A geopolymer-bonded silicon carbide refractory material, characterized in that, It is composed of the following substances in weight percentage: 70-90 wt% silicon carbide, 7-21 wt% aluminum silicate powder, 1-3 wt% phosphoric acid activator and 2-6 wt% water as raw materials; Its preparation method includes the following steps: Step 1: First, mechanically mix aluminum silicate powder, phosphoric acid activator, and water to obtain geopolymer sol; Step 2: Stir the sol and silicon carbide evenly; press and mold under 80~200 MPa, then dry at 110℃ for 48 hours, heat to 1200~1400℃ in air at a rate of 2~10℃ / min, hold for 2~5 hours, and cool to room temperature in the furnace. Step 3: Obtaining geopolymer-bonded silicon carbide refractory material; The silicon carbide contains ≥98 wt% SiC and has a particle size ≤3 mm. The aluminum silicate powder is one or more of pyrophyllite, kaolin, sillimanite, vermiculite and mica; The phosphoric acid activator is one or more combinations of orthophosphoric acid, phosphorous acid, metaphosphoric acid, and polyphosphoric acid.

Citation Information

Patent Citations

  • Preparation method of oxide combined SiC porous ceramic

    CN104072142A

  • Method for preparing porous oxide microspheres by using geopolymer as binder

    CN112321297A