Composite coating, U3Si2-Al dispersion type nuclear fuel and preparation method of U3Si2-Al dispersion type nuclear fuel
Patent Information
- Application Number
- CN202410626309.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-20
- Publication Date
- 2024-10-01
Smart Images

Figure CN118726937A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of nuclear fuel technology, in particular to a composite coating, U 3 Si 2 -Al dispersed nuclear fuel and preparation method. Background Art
[0002] The design and performance research of advanced nuclear fuels have always been the primary concern of all nuclear energy system designers. 3 Si 2 -Al dispersed nuclear fuel has been highly valued due to its high thermal conductivity and good comprehensive performance. 2 In comparison, U 3 Si 2 The uranium density increases (UO 2 Uranium density 9.7g / cm 3 , U 3 Si 2 The density of uranium is 11.3 g / cm 3 ), which helps to improve the constant concentration performance of the reactor; U 3 Si 2 High thermal conductivity (15W / m / K), which can significantly reduce the core temperature, greatly reducing the risk of overheating in the core during an accident; 3 Si 2 The irradiation swelling is small and uniform, so it is considered as a potential accident-tolerant nuclear fuel (ATF). 3 Si 2 Fuel particles are fuel phase, Al is the matrix composition of U 3 Si 2 -Al dispersed nuclear fuel has been widely studied at home and abroad since the 1980s and has been used in many experimental reactors. However, a large number of studies at home and abroad have shown that when the temperature is higher than 250℃, U 3 Si 2 The interface reaction between the fuel particles and the Al matrix is likely to occur, resulting in U 3 Si 2 -Al diffused fuel elements cause damage, resulting in U 3 Si 2 -Al dispersed fuel elements can only be used below 250°C, which limits their excellent performance. 3 Si 2 Fuel particle coating, which inhibits the interface reaction between fuel particles and aluminum substrate at high temperature, has become a new method for U 3 Si 2 -Al dispersed nuclear fuel is urgently needed for application in high temperature reactors. Design and preparation of suitable U 3Si 2 The particles are coated to match the U 3 Si 2 Swelling due to radiation, maintaining integrity during service, and blocking U 3 Si 2 The interfacial reaction with Al is an important research direction of dispersed nuclear fuel.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a novel coating design and a preparation method thereof to solve the problem of U 3 Si 2 The difficulty of the interface reaction between fuel particles and aluminum substrate at high temperature is to realize U 3 Si 2 -High temperature applications of Al dispersed fuel elements.
[0005] Based on this, the present invention has the following technical solutions:
[0006] In a first aspect, the present invention first provides a composite coating, which comprises a first ceramic layer, a second ceramic layer and a metal layer which are sequentially arranged in contact with each other;
[0007] Wherein, the porosity of the first ceramic layer is greater than the porosity of the second ceramic layer; and the theoretical density TD of the second ceramic layer is greater than 98%.
[0008] In order to solve the above technical problems, the present invention provides a new coating design of "first ceramic inner layer + second ceramic middle layer + metal outer layer", wherein the porosity of the first ceramic inner layer is greater than that of the second ceramic layer; it is mainly used to absorb the swelling and deformation of particles due to radiation, and can also absorb the volume deformation caused by the different thermal expansion rates of the coating material and the nuclear fuel core, and keep the two outer dense layers from being broken by the expansion force. The second ceramic middle layer is a key component of the composite coating, which not only provides a deposition base for the outer dense metal coating, but also is used to isolate and inhibit U 3 Si 2 The present invention finds that when the density is controlled within the above range, it is beneficial to solve the problem of U 3 Si 2 The difficulty of the interface reaction between fuel particles and aluminum substrate at high temperature is to realize U 3 Si 2 -Al dispersed fuel element for high temperature applications. The metal layer is mainly used to protect the dense ceramic coating to prevent U 3 Si 2 Damage of dispersed particles during subsequent nuclear fuel assembly preparation.
[0009] Preferably, the material of the second ceramic layer is not compatible with U 3 Si 2 Ceramic materials that react with Al;
[0010] And / or, the material of the first ceramic layer is not compatible with U 3 Si 2 Reactive ceramic materials;
[0011] More preferably, the materials of the first ceramic layer and the second ceramic layer are the same or different from each other, namely, ZrC, NbC, ZrN, WC or MoC;
[0012] Further preferably, the materials of the first ceramic layer and the second ceramic layer are both ZrN.
[0013] Further preferably, the first ceramic layer and the second ceramic layer are made of the same material.
[0014] In the present invention, the total thickness of the composite coating is not limited. 3 Si 2 -The service requirements of Al dispersed fuel elements (including service temperature, service burnup, service conditions, etc.) are determined.
[0015] However, in the present invention, the relationship between the second ceramic layer and the total thickness of the composite coating will significantly affect the effect of the coating.
[0016] Preferably, the thickness of the second ceramic layer accounts for 30-80% of the total thickness of the composite coating.
[0017] The present invention finds that when the above thickness relationship is controlled, the second ceramic layer can play a better role in preventing the release of fission products and preventing U 3 Si 2 -Al interface reaction and providing a substrate for metal coating deposition.
[0018] Preferably, the porosity of the first ceramic layer is 30-60%. The present invention finds that when the porosity is lower than the above range, it is too loose and difficult to form a coating layer, while when the porosity is higher than the range, it is too dense and difficult to store fission products and offset radiation swelling.
[0019] In the present invention, the metal layer is not only used to block the Al substrate-core interface reaction, but also has another function that the metal coating and the Al substrate are the same metal, have similar ductility and better compatibility.
[0020] Preferably, the material of the metal layer is not 3 Si 2 Metal materials that react with Al;
[0021] More preferably, the metal layer contains the same metal element as that in the first ceramic layer and the second ceramic layer.
[0022] In a second aspect, the present invention further provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with the composite coating.
[0023] In the third aspect, the present invention provides the U 3 Si 2 -Al dispersed nuclear fuel preparation method, comprising: using fluidized bed-chemical vapor deposition method to prepare U 3 Si 2 The surface of the core particle is coated with the composite coating;
[0024] Wherein, during the coating process, the U 3 Si 2 The particle fluidization state remains stable, and the coating material can be changed only by changing the precursor gas atmosphere.
[0025] In the present invention, the fluidized bed-chemical vapor deposition process is adopted, and the fluidizing gas and temperature are maintained under the same equipment and the same environment, that is, the fluidized state is always maintained and the particle circulation does not stop; in this process, only the type and concentration of the precursor are changed to realize the continuous preparation of the loose ceramic inner layer, the dense ceramic middle layer and the dense metal outer layer, and the natural transition between the layers is conducive to obtaining a complete "loose ceramic inner layer + fine-grained dense ceramic layer + dense metal coating" composite coating barrier layer, which meets the requirement of inhibiting the interface reaction between the fuel particles and the aluminum substrate at high temperature, thereby expanding the U 3 Si 2 -Al dispersed nuclear fuel high temperature application range.
[0026] In the present invention, when preparing loose ceramic coatings and dense ceramic coatings, only the concentration is changed to achieve the change of the coating layer generation process, rather than completely replacing the precursor gas, which is conducive to the natural transition and close bonding of the coating layer.
[0027] As a preferred embodiment, the U 3 Si 2 The preparation method of -Al dispersed nuclear fuel comprises:
[0028] S1: introducing a first precursor gas, a second precursor gas and a third precursor gas to cover the first ceramic coating;
[0029] S2: changing the ratio and concentration of the first precursor gas, the second precursor gas and the third precursor gas to continue coating the second ceramic layer;
[0030] S3: changing the ratio and concentration of the first precursor gas, the second precursor gas and the third precursor gas, and continuing to coat the metal layer.
[0031] Preferably, when the material of the second ceramic layer is ZrC, the first precursor gas, the second precursor gas and the third precursor gas are zirconium salt, olefin and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (5.5-6.5); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (30-40); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-3.5): (15-20);
[0032] And / or, when the material of the second ceramic layer is NbC, the first precursor gas, the second precursor gas and the third precursor gas are niobium salt, olefin and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (3.5-5.5); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (25-35); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.0-3.5): (15-20);
[0033] And / or, when the material of the second ceramic layer is ZrN, the first precursor gas, the second precursor gas and the third precursor gas are zirconium salt, nitrogen and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (3.5-5.5); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (25-35); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-3.5): (15-20);
[0034] And / or, when the material of the second ceramic layer is WC, the first precursor gas, the second precursor gas and the third precursor gas are tungsten salt, alkyne and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (5-10); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (30-70); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-4.5): (15-20);
[0035] And / or, when the material of the second ceramic layer is MoC, the first precursor gas, the second precursor gas and the third precursor gas are molybdenum salt, alkyne and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (4-10); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (30-70); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-3.0): (15-20).
[0036] In a specific implementation process, those skilled in the art can control the thickness of the coating by adjusting the deposition time, which is not further limited here.
[0037] In the present invention, when preparing the composite coating, each precursor gas is introduced into the fluidized bed through an independent pipeline to avoid mutual interference between the precursors.
[0038] In the present invention, when preparing the composite coating, when the precursors used in each coating are switched, they are first introduced and then closed, so that the coatings have a natural transition and stratification is prevented.
[0039] Preferably, when the material of the second ceramic layer is ZrC, the coating temperature is 1200-1400°C;
[0040] and / or, when the material of the second ceramic layer is NbC, the coating temperature is 1100-1300° C.;
[0041] and / or, when the material of the second ceramic layer is ZrN, the coating temperature is 900-1300° C.;
[0042] and / or, when the material of the second ceramic layer is WC, the coating temperature is 700-1100° C.;
[0043] And / or, when the material of the second ceramic layer is MoC, the coating temperature is 1200-1500°C.
[0044] Based on the above technical solution, the beneficial effects of the present invention are:
[0045] The present invention provides a composite coating, U 3 Si 2 -Al dispersed nuclear fuel and preparation method can effectively solve the problem of U 3 Si 2 The difficulty of the interface reaction between fuel particles and aluminum substrate at high temperature is to realize U 3 Si 2 -High temperature applications of Al dispersed fuel elements. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0047] Figure 1 It is U prepared in Example 1 provided by the present invention 3 Si 2 Schematic diagram of core particle composite coating;
[0048] Figure 2 It is U prepared in Example 1 provided by the present invention 3 Si 2 -Schematic diagram of composite coating-Al matrix dispersed nuclear fuel;
[0049] Figure 3 The method of the present invention is to prepare U in Example 1 3 Si 2 Fluidized bed-chemical vapor deposition process flow diagram of core particle composite coating;
[0050] Figure 4 This is a physical picture of the multifunctional composite coating prepared in Example 1 provided by the present invention. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] Unless otherwise specified, all raw materials used in the examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.
[0053] Unless otherwise specified, the ratio of gases in the following embodiments refers to the volume ratio.
[0054] Example 1
[0055] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrC, the second ceramic layer is ZrC, and the metal layer is Zr.
[0056] The preparation method thereof comprises the following steps:
[0057] (1) Install a fluidized bed and introduce fluidizing gas Ar at a flow rate of 5.0 SLM (standard liters per minute).
[0058] (2) The reactor is heated by adjusting the power through electric heating to raise the temperature to 1000 degrees Celsius.
[0059] (3) Join U 3 Si 2 Core particles, start fluidization:
[0060] U was added from the top of the fluidized bed using a feeder 3 Si 2 The core particles are then adjusted to have a fluidizing gas of H 2 , the flow rate is 6.0SLM, making U 3 Si 2 The core particles remain in a well fluidized state.
[0061] (4) Introduce appropriate precursors respectively and coat each coating layer continuously:
[0062] The temperature was adjusted to 1200 degrees Celsius to maintain the particle fluidization state; the precursor gas ZrCl was introduced through different pipes. 4 , C 3 H 6 and H 2 , successively coated with a loose ceramic inner layer (the ratio of the three is 3:1:6), a dense ceramic layer (the ratio of the three is 3:1:38), and a dense metal coating (ZrCl 4 and H 2The ratio is 3:18) to obtain a complete composite coating;
[0063] The total thickness of the composite coating is 50 microns; the thickness of the loose ceramic inner layer is 10 microns, and the porosity of the loose ceramic inner layer is 50%; the thickness of the dense ceramic layer is 30 microns, and the density of the dense ceramic layer is 98.5% of the theoretical density; the thickness of the dense metal coating is 10 microns.
[0064] (5) Cool down and take out the coated particles:
[0065] After the coating is completed, the precursor gas pipeline is closed and the inert gas Ar is kept flowing in unchanged, that is, the fluidized state of the particles is maintained until the temperature drops to room temperature and the U3Si2 coated particles are taken out.
[0066] Example 2
[0067] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is WC, the second ceramic layer is WC, and the metal layer is W.
[0068] The preparation method thereof comprises the following steps:
[0069] (1) Install a fluidized bed and introduce fluidizing gas Ar at a flow rate of 5.0 SLM (standard liters per minute).
[0070] (2) The reactor is heated by adjusting the power through electric heating to raise the temperature to 600 degrees Celsius.
[0071] (3) Join U 3 Si 2 Core particles, start fluidization:
[0072] U was added from the top of the fluidized bed using a feeder 3 Si 2 The core particles are then adjusted to have a fluidizing gas of H 2 , the flow rate is 6.0SLM, making U 3 Si 2 The core particles remain in a well fluidized state.
[0073] (4) Introduce appropriate precursors respectively and coat each coating layer continuously:
[0074] Adjust to the appropriate temperature of 800 degrees Celsius, keep the particles in a fluidized state, and then introduce precursors, including WCl 6 , C 2 H 2 and H 2 , respectively coated with a loose ceramic inner layer (the ratio of the three is 2:1:8), a dense ceramic layer (the ratio of the three is 2:1:50), a dense metal coating (WCl 6 and H 2 The ratio is 2:50) to obtain a complete composite coating;
[0075] Among them, the total thickness of the composite coating is 55 microns; the thickness of the loose ceramic inner layer is 10 microns, and the porosity of the loose ceramic inner layer is 55%; the thickness of the dense ceramic layer is 38 microns, and the theoretical density of the dense ceramic layer is 98%; the thickness of the dense metal coating is 7 microns.
[0076] (5) Cool down and take out the coated particles:
[0077] After the coating is completed, the precursor gas pipeline is closed and the inert gas Ar is kept flowing in, that is, the particle fluidization state is maintained until the temperature drops to room temperature and the U3Si is taken out. 2 Coated particles.
[0078] Example 3
[0079] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrN, the second ceramic layer is ZrN, and the metal layer is Zr.
[0080] The preparation method thereof comprises the following steps:
[0081] (1) Install a fluidized bed and introduce fluidizing gas Ar at a flow rate of 5.0 SLM (standard liters per minute).
[0082] (2) The reactor is heated by adjusting the power through electric heating to raise the temperature to 1000 degrees Celsius.
[0083] (3) Join U 3 Si 2 Core particles, start fluidization:
[0084] U was added from the top of the fluidized bed using a feeder 3 Si 2The core particles are then adjusted to have a fluidizing gas of H 2 , the flow rate is 6SLM, so that U 3 Si 2 The core particles remain in a well fluidized state.
[0085] (4) Introduce appropriate precursors respectively and coat each coating layer continuously:
[0086] Adjust to the appropriate temperature of 1250 degrees Celsius, keep the particles in a fluidized state, and then introduce precursors, including ZrCl 4 、N 2 and H 2 , respectively coated with a loose ceramic inner layer (the ratio of the three is 2:1:4), a dense ceramic layer (the ratio of the three is 2:1:32), and a dense metal coating (ZrCl 4 and H 2 The ratio is (2.5:30) to obtain a complete composite coating;
[0087] Among them, the total thickness of the composite coating is 50 microns; the thickness of the loose ceramic inner layer is 10 microns, and the porosity of the loose ceramic inner layer is 50%; the thickness of the dense ceramic layer is 30 microns, and the density of the dense ceramic layer is 98% of the theoretical density; the thickness of the dense metal coating is 10 microns.
[0088] (5) Cool down and take out the coated particles:
[0089] After the coating is completed, the precursor gas pipeline is closed and the inert gas Ar is kept flowing in, that is, the particle fluidization state is maintained until the temperature drops to room temperature and the U 3 Si 2 Coated particles.
[0090] Example 4
[0091] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrN, the second ceramic layer is ZrN, and the metal layer is Zr.
[0092] The preparation method thereof differs from that of Example 3 only in that: in step (4), when coating the loose ceramic inner layer, ZrCl 4 、N 2 and H 2 The ratio of ZrCl is 2.5:1.0:4.0; when coated with dense ceramic layer,4 、N 2 and H 2 The ratio of ZrCl is 2:1:30; when coated with dense metal coating, 4 and H 2 The ratio is 3.5:20;
[0093] Among them, the total thickness of the composite coating is 60 microns; the thickness of the loose ceramic inner layer is 10 microns, and the porosity of the loose ceramic inner layer is 50%; the thickness of the dense ceramic layer is 40 microns, and the density of the dense ceramic layer is 98% of the theoretical density; the thickness of the dense metal coating is 10 microns.
[0094] Example 5
[0095] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrN, the second ceramic layer is ZrN, and the metal layer is Zr.
[0096] The only difference between the preparation method and Example 3 is that in step (4), the coating temperature is 1300 degrees Celsius.
[0097] The total thickness of the composite coating finally obtained is 50 microns; the thickness of the loose ceramic inner layer is 10 microns, and the porosity of the loose ceramic inner layer is 50%; the thickness of the dense ceramic layer is 30 microns, and the density of the dense ceramic layer is 98% of the theoretical density; the thickness of the dense metal coating is 10 microns.
[0098] Example 6
[0099] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrN, the second ceramic layer is ZrN, and the metal layer is Zr.
[0100] The preparation method thereof differs from that of Example 3 only in that: in step (4), when coating the loose ceramic inner layer, ZrCl 4 、N 2 and H 2The ratio of ZrCl is 20:1.0:4.0; when coated with dense ceramic layer, 4 、N 2 and H 2 The ratio of ZrCl is 15:1:30; when coated with dense metal coating, 4 and H 2 The ratio is 3.5:20;
[0101] Among them, the total thickness of the composite coating is 60 microns; the thickness of the loose ceramic inner layer is 10 microns, and the porosity of the loose ceramic inner layer is 80%; the thickness of the dense ceramic layer is 40 microns, and the density of the dense ceramic layer is 50% of the theoretical density; the thickness of the dense metal coating is 10 microns.
[0102] Example 7
[0103] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrN, the second ceramic layer is ZrN, and the metal layer is Zr.
[0104] The only difference between the preparation method and Example 3 is that in step (4), the coating temperature is 900 degrees Celsius.
[0105] The total thickness of the composite coating finally obtained is 30 microns; the thickness of the loose ceramic inner layer is 7 microns, and the porosity of the loose ceramic inner layer is 70%; the thickness of the dense ceramic layer is 20 microns, and the density of the dense ceramic layer is 80% of the theoretical density; the thickness of the dense metal coating is 3 microns.
[0106] Example 8
[0107] This embodiment provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; in the composite coating, the first ceramic layer is ZrN, the second ceramic layer is ZrN, and the metal layer is Zr.
[0108] The preparation method thereof differs from that of Example 3 only in that: the total thickness of the composite coating is 50 microns; the thickness of the loose ceramic inner layer is 20 microns, and the porosity of the loose ceramic inner layer is 50%; the thickness of the dense ceramic layer is 20 microns, and the density of the dense ceramic layer is 98% of the theoretical density; and the thickness of the dense metal coating is 10 microns.
[0109] Comparative Example 1
[0110] This comparative example provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is coated with a composite coating; the only difference between it and Example 3 is that the composite coating contains only a first ceramic layer ZrN (loose layer) and a metal layer Zr.
[0111] Comparative Example 2
[0112] This comparative example provides a U 3 Si 2 -Al dispersed nuclear fuel, including Al matrix and U dispersed on the Al matrix 3 Si 2 Core particle; said U 3 Si 2 The surface of the core particle is not covered with a composite coating.
[0113] Test example
[0114] The present invention further relates to the above-mentioned U 3 Si 2 -Al dispersed nuclear fuel high temperature resistance and composite coating strength were tested, the results are shown in Table 1:
[0115] Table 1
[0116]
[0117]
[0118] The present invention finds that U 3 Si 2 -Al dispersed nuclear fuel without coating can not withstand high temperature more than 400 degrees Celsius. When it exceeds 400 degrees Celsius, U 3 Si 2 The reaction between U and Al will produce U-Al phase, which will cause the entire fuel structure to be destroyed. After being coated with the composite coating, U 3 Si2 -Al are isolated, while U 3 Si 2 The irradiation expansion effect and fission gas will be absorbed by the loose layer, maintaining the integrity of the fuel structure and being able to withstand high temperatures above 1000 degrees Celsius. The bonding strength between the composite coatings can reach up to 18N. It should be noted that a bonding strength exceeding 10N is a good bonding strength, indicating that the bonding strength between the composite coatings prepared by the deposition method is very good.
[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite coating, characterized in that: It includes a first ceramic layer, a second ceramic layer and a metal layer which are sequentially arranged in contact with each other; The porosity of the first ceramic layer is greater than that of the second ceramic layer; and the theoretical density TD of the second ceramic layer is greater than 98%.
2. The composite coating according to claim 1, characterized in that: The material of the second ceramic layer is a ceramic material that does not react with U3Si2 and Al; And / or, the material of the first ceramic layer is a ceramic material that does not react with U3Si2; Preferably, the materials of the first ceramic layer and the second ceramic layer are the same or different from each other, namely, ZrC, NbC, ZrN, WC or MoC; More preferably, the first ceramic layer and the second ceramic layer are made of the same material.
3. The composite coating according to claim 1 or 2, characterized in that: The thickness of the second ceramic layer accounts for 30-80% of the total thickness of the composite coating.
4. The composite coating according to any one of claims 1 to 3, characterized in that: The porosity of the first ceramic layer is 30-60%.
5. The composite coating according to any one of claims 1 to 4, characterized in that: The material of the metal layer is a metal material that does not react with U3Si2 and Al; More preferably, the metal layer contains the same metal element as that in the first ceramic layer and the second ceramic layer.
6. A U3Si2-Al dispersed nuclear fuel, characterized in that: It comprises an Al matrix and U3Si2 core particles dispersed on the Al matrix; the surface of the U3Si2 core particles is coated with the composite coating according to any one of claims 1 to 5.
7. The method for preparing the U3Si2-Al dispersed nuclear fuel according to claim 6, characterized in that: The composite coating is coated on the surface of the U3Si2 core particles by a fluidized bed-chemical vapor deposition method; In the coating process, the fluidized state of the U3Si2 particles is kept stable and unchanged, and the coating material is changed only by changing the precursor gas atmosphere.
8. The method for preparing U3Si2-Al dispersed nuclear fuel according to claim 7, characterized in that: include: S1: introducing a first precursor gas, a second precursor gas and a third precursor gas to cover the first ceramic coating; S2: changing the ratio and concentration of the first precursor gas, the second precursor gas and the third precursor gas to continue coating the second ceramic layer; S3: changing the ratio and concentration of the first precursor gas, the second precursor gas and the third precursor gas, and continuing to coat the metal layer.
9. The method for preparing U3Si2-Al dispersed nuclear fuel according to claim 8, characterized in that: When the material of the second ceramic layer is ZrC, the first precursor gas, the second precursor gas and the third precursor gas are zirconium salt, olefin and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (5.5-6.5); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (30-40); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-3.5): (15-30); And / or, when the material of the second ceramic layer is NbC, the first precursor gas, the second precursor gas and the third precursor gas are niobium salt, olefin and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (3.5-5.5); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (2.5-3.5): (0.5-1.5): (25-35); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.0-3.5): (15-30); And / or, when the material of the second ceramic layer is ZrN, the first precursor gas, the second precursor gas and the third precursor gas are zirconium salt, nitrogen and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (3.5-5.5); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (25-35); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-3.5): (15-20); And / or, when the material of the second ceramic layer is WC, the first precursor gas, the second precursor gas and the third precursor gas are tungsten salt, alkyne and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (5-10); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (30-70); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-4.5): (15-50); And / or, when the material of the second ceramic layer is MoC, the first precursor gas, the second precursor gas and the third precursor gas are molybdenum salt, alkyne and hydrogen respectively; in S1, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (4-10); in S2, the volume ratio of the first precursor gas, the second precursor gas and the third precursor gas is (1.5-2.5): (0.5-1.5): (30-70); in S3, the introduction of the second precursor gas is stopped, and the volume ratio of the first precursor gas to the third precursor gas is (2.5-3.0): (15-40).
10. The method for preparing U3Si2-Al dispersed nuclear fuel according to claim 8 or 9, characterized in that: When the material of the second ceramic layer is ZrC, the coating temperature is 1200-1400°C; and / or, when the material of the second ceramic layer is NbC, the coating temperature is 1100-1300° C.; and / or, when the material of the second ceramic layer is ZrN, the coating temperature is 900-1300° C.; and / or, when the material of the second ceramic layer is WC, the coating temperature is 700-1100° C.; And / or, when the material of the second ceramic layer is MoC, the coating temperature is 1200-1500°C.
Citation Information
Patent Citations
Full ceramic type covering fuel particle, preparation method of full ceramic type covering fuel particle and fuel element
CN105185418A
Coated fuel particles containing composite carbide coating layer and preparation method thereof
CN111489837A
Coated fuel particle containing carbide-refractory metal coating layer and preparation method of coated fuel particle
CN111584100A
Dispersion Ceramic Micro-encapsulated (DCM) Nuclear Fuel and Related Methods
US20170040069A1
Nuclear reactor fuel
US20240145105A1
Cited By
U3Si2-Cu dispersion type nuclear fuel with stable interface at high temperature and simulation construction method
CN121545603A
U3Si2-cu dispersion type nuclear fuel with stable interface at high temperature and simulation construction method
CN121545603B