Composite particle reinforced offshore steel wire for super-large heat input gas-electric vertical welding and preparation method thereof

By adding nano-sized La₂O₃ and ZrO₂ to the welding wire of marine steel, fine inclusions are formed, which solves the problems of porosity, cracks and grain coarsening in welds during ultra-high heat input welding. This achieves high strength, high toughness and defect-free welding effect, and improves the safety and service life of marine steel welded structures.

CN118744295BActive Publication Date: 2026-11-24CHINA-UKRAINE INST OF WELDING GUANGDONG ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410980588.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2026-11-24
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Under ultra-high heat input welding conditions, existing technologies are prone to porosity, cracks and inclusions in marine steel welds, and grain coarsening in the heat-affected zone, resulting in insufficient strength and toughness of the welded joint, which affects the safety and lifespan of the ship structure.

Method used

The high-energy gas-electric vertical welding wire for marine engineering steel reinforced with composite particles is made by adding nano-sized La₂O₃ and ZrO₂ to the flux core powder to form fine and dispersed La-rich and Zr-rich inclusions, which promotes the formation of acicular ferrite, refines the grains, and improves the strength and low-temperature toughness of the weld metal.

Benefits of technology

Under ultra-high heat input welding conditions, the strength and low-temperature toughness of the weld metal are significantly improved, defects are reduced, the service life of the workpiece is extended, and high-strength, high-toughness, defect-free marine steel welded structural components are obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744295B_ABST
    Figure CN118744295B_ABST
Patent Text Reader

Abstract

This invention discloses a composite particle-reinforced wire for ultra-high heat input gas-electric vertical welding of marine steel, which consists of an outer steel strip and an inner flux-cored powder. By adding nano-sized La2O3 and ZrO2 composite reinforcing particles, the strength and hardness of the cladding metal under ultra-high heat input welding (heat input ≥600kJ / cm) conditions are significantly improved. While improving the strength of the weld metal, it also has excellent low-temperature toughness, thus improving its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical fields:

[0001] This invention relates to the field of welding materials technology, specifically to a composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding and its preparation method. Background technology:

[0002] Currently, with the development of lightweight, large-scale, environmentally friendly, and economical marine engineering structures, there are higher requirements for the performance and thickness of marine structural steel. This necessitates increased steel thickness and the development of hull steel towards higher toughness, higher strength, and weldability. To effectively manufacture thick, high-quality marine structural components, high-heat welding technologies such as multi-wire submerged arc welding, gas-electric vertical welding, and electroslag welding are widely used. For example, gas-electric vertical welding can achieve a welding heat input of 600 kJ / cm, allowing for single-pass forming during the welding process. However, such ultra-high heat input also easily leads to defects such as porosity, cracks, and inclusions, and can cause severe coarsening of the heat-affected zone (HAZ) and weld metal grains. Furthermore, the slow cooling rate after welding can also lead to the formation of brittle structures such as coarse side-plate ferrite, Widmanstätten structure, and upper bainite during phase transformation, affecting the strength and toughness of the welded joint and thus threatening the safe use and service life of the ship structure. Therefore, improving the strength, low-temperature toughness, and weldability of weld microstructures under ultra-high heat input is an urgent problem that needs to be solved.

[0003] Patent publication number CN104259688B discloses a high-heat-input gas-electric vertical welding flux-cored wire and its preparation method. It abandons the traditional calcium fluoride deoxidizer and adopts sodium fluoride, which has better effects on deoxidation, arc stabilization, and slag thinning. Appropriate amounts of Al and Mg are added to the flux core to improve the alloy's deoxidation capacity and enhance slag removal during welding. The weld metal prepared using this high-heat-input gas-electric vertical welding flux-cored wire has uniform cladding and good weld formation, making it suitable for thick plate welding. However, the mechanical properties and toughness of the weld metal at high heat input are not significantly improved.

[0004] The invention disclosed in patent publication number CN109530961B is a flux-cored welding wire for gas-shielded high heat input welding, its preparation method, and its application. This invention selects low-carbon steel strip as the flux coating, with the flux core accounting for 13.0-13.5% of the total mass of the welding wire. The components of the flux core and their mass percentages in the flux-cored welding wire are as follows: TiO2: 5.0-5.6%, SiO2: 0.3-0.6%, Al2O3: 0.15-0.25%, NaF: 0.2-0.3%, Mg-Al alloy: 0.4-0.5%, Si: 0.4-0.5%, Mn: 2.0-2.5%, Ti: 0.04-0.11%, B: 0.009-0.01%, with Fe and other unavoidable impurities as the balance. The shielding gas used during welding is CO2, the welding current is 260-280A, the welding voltage is 27-28V, the heat input is 16-20kJ / cm, the interpass temperature is 135-165℃, and the yield strength ratio of the deposited metal is no higher than 0.83. This invention optimizes the composition of the flux-cored wire, thereby improving the plasticity of the weld metal, reducing crack formation at the weld, and controlling the yield strength ratio of the alloy. However, the welding heat input used in the patent is relatively low, and its effectiveness under ultra-high heat input welding conditions is unknown.

[0005] Therefore, it is necessary to design a wire for ultra-high heat input gas-electric vertical welding of marine steel, which can effectively reduce defects such as porosity, cracks and inclusions in the alloy during high heat input welding, improve the weld formation and the strength, low-temperature toughness and weldability of the weld structure under ultra-high heat input, and obtain marine steel welded structural components with high strength, high toughness and no defects. Summary of the Invention:

[0006] The purpose of this invention is to provide a composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding and its preparation method.

[0007] This invention is achieved through the following technical solutions:

[0008] A composite particle-reinforced marine steel ultra-high heat input gas-electric vertical welding wire is composed of an outer steel strip and an inner flux-cored powder. The flux-cored powder filling rate is 20-30%. The components of the flux-cored powder and their percentage by mass of the flux-cored welding wire are as follows: TiO2: 5.0-5.6%, SiO2: 0.32-0.64%, NaF: 0.18-0.3%, Al: 0.36-0.48%, Si: 0.28-0.5%, Mn: 1.3-1.7%, Ni: 2-4%, Mo: 1.8-3.6%, Ti: 0.1-0.3%, ZrO2: 0.05-0.2%, B: 0.009-0.01%, La2O3: 0.3-0.85%, with the balance being Fe and unavoidable impurities.

[0009] Preferably, the content of nano-sized ZrO2 in the core powder is 0.1-0.2%, and the content of nano-sized La2O3 is 0.36-0.82%.

[0010] Preferably, the diameter of the wire is 1.6 mm.

[0011] The addition of inexpensive nano-sized La2O3 can pin the movement of the original austenite grain boundaries during the high-temperature welding process, inhibit grain growth, and absorb impurities such as S and P in the weld metal, thus improving cleanliness. Simultaneously, the co-added ZrO2 is highly stable at high temperatures and can act as nucleation sites during weld metal cooling, inducing acicular ferrite (AF) nucleation. By co-adding nano-sized La2O3 and ZrO2 composite reinforcing particles, a large number of finely dispersed La- and Zr-rich inclusions are formed. This promotes the formation of acicular ferrite (AF) at the weld, refines the grains, reduces the tendency for welding cracks, and inhibits crack propagation during low-temperature impact. This significantly improves the strength and hardness of the cladding metal under ultra-high heat input welding conditions (heat input ≥600 kJ / cm), resulting in improved weld metal strength while also exhibiting excellent low-temperature toughness, thus extending its service life. Ultimately, this yields marine steel welded structural components that combine high strength, high toughness, and defect-free characteristics.

[0012] In the core powder, TiO2, SiO2, and NaF act as slag-forming agents, which on the one hand protect the molten pool and stabilize the electric arc, and on the other hand adjust the viscosity and alkalinity of the molten pool.

[0013] The particle size of the raw material powders in the core powder, excluding nano-sized La2O3 and nano-sized ZrO2, is 60-100 mesh.

[0014] The preparation steps of the composite particle-reinforced marine steel ultra-high heat input gas electric vertical welding wire include the following steps:

[0015] Step S1: After the core powder raw material is dehydrated and dried, it is sieved through an 80-mesh sieve. According to the required ratio, nano-sized La2O3, ZrO2 powder, and Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill jar for mixing. The ball milling parameters are: ball-to-material ratio of 5:1, ball milling time of 1-2 hours in forward rotation and 1-2 hours in reverse rotation, and a rotation speed of 300 r / min to obtain the ball-milled mixed powder.

[0016] Step S2: Mix TiO2, SiO2, and NaF slagging agent with the ball-milled mixed powder according to the specified ratio, put the mixture into a V-type mixer, and mix for 30 minutes to obtain a uniformly mixed core powder.

[0017] Step S3: First, dry the low-carbon steel strip, then roll the steel strip into a U-shape using forming rollers. Add the mixed flux-cored powder to the U-shaped steel strip according to the required filling rate through a powder feeding device, and then further roll it into a tube. Then, feed the tubular welding wire into the drawing die and control the drawing speed at 1.2-1.5m / min for drawing. Repeat the above operation for redrawing until the desired diameter of 1.6mm flux-cored welding wire is obtained.

[0018] This invention also protects the application of the above-mentioned welding wire in ultra-high heat input welding of thick marine steel. The ultra-high heat input welding is a double-wire gas-electric vertical welding, the base material is EH36 grade marine steel with a thickness of 50-60mm, the base material bevel is designed as a single-sided V-shaped bevel with a single-sided bevel angle of 12°, a gap of 8-10mm, a blunt edge bevel of no more than 1mm, the dry extension of the two welding wires is 35mm, the welding torch angle is 4°~8°, the distance from the rear wire to the backing is 20mm, and the spacing between the two welding wires is 19mm. The welding process parameters are as follows: the rear wire is DC positive polarity, fixed without oscillation, current 450.1-481.9A, voltage 40.2-42.3V; the front wire is DC reverse polarity, oscillation width is 15-18mm, current 473.9-501.8A, voltage 48.9-52.8A; the speed is 6-7cm / min, the heat input is 606.7-781.3kJ / cm, and the entire welding process is carried out under 100% CO2 gas protection conditions.

[0019] The beneficial effects of this invention are as follows:

[0020] 1) This invention, by combining nano-sized La2O3 and ZrO2 composite reinforcing particles, forms a large number of finely dispersed La-rich and Zr-rich inclusions. On the one hand, it promotes the formation of acicular ferrite (AF) at the weld, and on the other hand, it refines the grains, reduces the tendency of welding cracks, and inhibits the propagation of cracks during low-temperature impact. It significantly improves the strength and hardness of the cladding metal under ultra-high heat input welding (heat input ≥600kJ / cm). While improving the strength of the weld metal, it also has excellent low-temperature toughness, which improves its service life. Finally, it obtains marine steel welded structural components with high strength, high toughness and no defects.

[0021] 2) The welding wire of the present invention has the advantages of low welding spatter, high cladding speed, beautiful weld formation, and all-position welding capability. After double-wire gas-electric vertical welding, the weld formation effect is good, with no defects such as cracks, porosity, and inclusions. The weld metal obtained by using the welding wire of the present invention under ultra-high heat input welding (heat input ≥600kJ / cm) conditions can still maintain high strength and toughness, greatly increasing the service life of the workpiece and helping to save costs. Attached image description:

[0022] Figure 1This is the microstructure of the welding wire obtained in Example 1.

[0023] Figure 2 This is the microstructure of the welding wire obtained in Comparative Example 1. Detailed implementation method:

[0024] The following is a further description of the invention, but not a limitation thereof.

[0025] Example 1: A composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding, its preparation method and application.

[0026] A composite particle-reinforced marine steel high-energy gas-electric vertical welding wire for EH36 ship plate steel is composed of an outer layer of commercial H08A low-carbon steel strip and an inner layer of flux-cored powder. The components of the flux-cored powder and their percentage by mass of the flux-cored welding wire are as follows: TiO2: 5.2%, SiO2: 0.48%, NaF: 0.24%, Al: 0.42%, Si: 0.38%, Mn: 1.5%, Ni: 3.1%, Mo: 2.2%, Ti: 0.15%, B: 0.009%, La2O3: 0.8%, ZrO2: 0.1%, with the balance being Fe and some unavoidable impurities.

[0027] The specific steps for preparing composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding are as follows:

[0028] Step S1: After the core powder raw material is dehydrated and dried, it is sieved through an 80-mesh sieve. According to the required ratio, nano-sized La2O3, ZrO2 powder, and Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill jar for mixing. The ball milling parameters are: ball-to-material ratio of 5:1, ball milling time of 1 hour in the forward direction and 1 hour in the reverse direction, and rotation speed of 300 r / min to obtain the mixed powder after ball milling.

[0029] Step S2: Mix TiO2, SiO2, and NaF slag-forming agent with the ball-milled mixed powder according to the specified ratio, put the mixture into a V-type mixer, and mix for 30 minutes to obtain a uniformly mixed core powder.

[0030] Step S3: First, dry the low-carbon steel strip (commercial H08A), then roll the strip into a U-shape using forming rolls. Add the mixed flux-cored powder to the U-shaped steel strip according to the required filling rate using a powder feeding device, and then further roll it into a tube. After that, feed the tubular welding wire into the drawing die and control the drawing speed at 1.2m / min for drawing. Repeat the above operation for redrawing until the desired diameter of 1.6mm flux-cored welding wire is obtained.

[0031] The prepared flux-cored welding wires were used for dual-wire gas-electric vertical welding according to the following process parameters. The base material was EH36 grade marine steel, 60mm thick. The base material bevel design was a single-sided V-shaped bevel with a bevel angle of 12°, a gap of 8mm, and a blunt edge of 1mm. The extension length of the two welding wires was 35mm, the welding torch angle was 4°, the distance from the rear wire to the backing wire was 20mm, and the spacing between the two welding wires was 19mm. The welding process parameters were: the rear wire was DC positive polarity, fixed without oscillation, current 450.1A, voltage 40.2V; the front wire was DC reverse polarity, oscillation width 15mm, current 473.9A, voltage 48.9V; the welding speed was 6cm / min, the heat input was 606.7kJ / cm, and the entire welding process was carried out under 100% CO2 gas protection conditions.

[0032] Example 2:

[0033] This embodiment provides a composite particle-reinforced marine steel high-energy gas-electric vertical welding wire for EH36 ship plate steel. It consists of an outer layer of commercial H08A low-carbon steel strip and an inner layer of flux-cored powder. The components of the flux-cored powder and their percentage by mass of the flux-cored welding wire are as follows: TiO2: 5.0%, SiO2: 0.4%, NaF: 0.18%, Al: 0.38%, Si: 0.29%, Mn: 1.4%, Ni: 3.5%, Mo: 2.4%, Ti: 0.2%, B: 0.009%, La2O3: 0.6%, ZrO2: 0.05%, with the balance being Fe and some unavoidable impurities.

[0034] The specific steps for preparing composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding are as follows:

[0035] Step S1: After the core powder raw material is dehydrated and dried, it is sieved through an 80-mesh sieve. According to the required ratio, nano-sized La2O3, ZrO2 powder, and Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill jar for mixing. The ball milling parameters are: ball-to-material ratio of 5:1, ball milling time of 2 hours in the forward direction and 2 hours in the reverse direction, and a rotation speed of 300 r / min to obtain the mixed powder after ball milling.

[0036] Step S2: Mix TiO2, SiO2, and NaF slag-forming agent with the ball-milled mixed powder according to the specified ratio, put the mixture into a V-type mixer, and mix for 30 minutes to obtain a uniformly mixed core powder.

[0037] Step S3: First, dry the low-carbon steel strip (commercial H08A), then roll the strip into a U-shape using forming rolls. Add the mixed flux-cored powder to the U-shaped steel strip according to the required filling rate using a powder feeding device, and then further roll it into a tube. After that, feed the tubular welding wire into the drawing die and control the drawing speed at 1.5m / min for drawing. Repeat the above operation for redrawing until the desired diameter of 1.6mm flux-cored welding wire is obtained.

[0038] The prepared flux-cored welding wire was used for dual-wire gas-electric vertical welding according to the process parameters described in Example 1.

[0039] Example 3:

[0040] This embodiment provides a composite particle-reinforced marine steel high-energy gas-electric vertical welding wire for EH36 ship plate steel. It consists of an outer layer of commercial H08A low-carbon steel strip and an inner layer of flux-cored powder. The components of the flux-cored powder and their percentage by mass of the flux-cored welding wire are as follows: TiO2: 5.6%, SiO2: 0.64%, NaF: 0.25%, Al: 0.39%, Si: 0.41%, Mn: 1.6%, Ni: 3.3%, Mo: 2.4%, Ti: 0.2%, B: 0.01%, La2O3: 0.3%, ZrO2: 0.06%, with the balance being Fe and some unavoidable impurities.

[0041] The preparation method of the composite particle reinforced marine steel wire for ultra-high heat input gas-electric vertical welding is the same as in Example 1.

[0042] The prepared flux-cored welding wire was used for dual-wire gas-electric vertical welding according to the process parameters described in Example 1.

[0043] Example 4:

[0044] This embodiment provides a composite particle-reinforced marine steel high-energy gas-electric vertical welding wire for EH36 ship plate steel. It consists of an outer layer of commercial H08A low-carbon steel strip and an inner layer of flux-cored powder. The components of the flux-cored powder and their percentage by mass of the flux-cored welding wire are as follows: TiO2: 5.1%, SiO2: 0.52%, NaF: 0.3%, Al: 0.39%, Si: 0.38%, Mn: 1.4%, Ni: 4%, Mo: 2.2%, Ti: 0.25%, B: 0.009%, La2O3: 0.36%, ZrO2: 0.19%, with the balance being Fe and some unavoidable impurities.

[0045] The preparation method of the composite particle reinforced marine steel wire for ultra-high heat input gas-electric vertical welding is the same as in Example 1.

[0046] The prepared flux-cored welding wire was used for dual-wire gas-electric vertical welding according to the process parameters described in Example 1.

[0047] Example 5:

[0048] This embodiment provides a composite particle-reinforced marine steel high-energy gas-electric vertical welding wire for EH36 ship plate steel. It consists of an outer layer of commercial H08A low-carbon steel strip and an inner layer of flux-cored powder. The components of the flux-cored powder and their percentage by mass of the flux-cored welding wire are as follows: TiO2: 5.3%, SiO2: 0.57%, NaF: 0.22%, Al: 0.42%, Si: 0.36%, Mn: 1.6%, Ni: 3.8%, Mo: 3.6%, Ti: 0.3%, B: 0.009%, La2O3: 0.82%, ZrO2: 0.20%, with the balance being Fe and some unavoidable impurities.

[0049] The preparation method of the composite particle reinforced marine steel wire for ultra-high heat input gas-electric vertical welding is the same as in Example 1.

[0050] The prepared flux-cored welding wire was used for dual-wire gas-electric vertical welding according to the process parameters described in Example 1.

[0051] Comparative Example 1:

[0052] Referring to Example 1, the difference is that the core powder does not contain La2O3 and ZrO2, while the other preparation processes are the same.

[0053] Comparative Example 2:

[0054] Referring to Example 1, the difference is that the core powder does not contain La2O3, but the other preparation processes are the same.

[0055] Comparative Example 3:

[0056] Referring to Example 1, the difference is that the core powder does not contain ZrO2, but the other preparation processes are the same.

[0057] The weld properties of the butt welds obtained in Examples 1-5 and Comparative Examples 1-3 were tested according to GB / T 2652 "Tension Test Method for Welds and Cladding Metals" and GB / T 2650 "Impact Test Method for Welded Joints". The impact test was conducted on an Instron Dynatup 9200 series drop hammer impact tester at a test temperature of -40℃. The results are shown in Table 1.

[0058] As can be seen from the comparison of the data of Example 1 and Comparative Examples 1-3 in Table 1, the synergistic effect of La2O3 and ZrO2 in this invention greatly improves the tensile properties and impact energy of the weld after dual-wire gas-electric vertical welding.

[0059] Table 1. Tensile properties and impact energy of welds after dual-wire gas-electric vertical welding of flux-cored welding wires in the examples and comparative examples.

[0060]

[0061] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding, characterized in that, It consists of an outer steel strip and an inner core powder, with a core powder filling rate of 20-30%. The components of the core powder and their percentage by mass of the core wire are as follows: TiO2: 5.0-5.6%, SiO2: 0.32-0.64%, NaF: 0.18-0.3%, Al: 0.36-0.48%, Si: 0.28-0.5%, Mn: 1.3-1.7%, Ni: 2-4%, Mo: 1.8-3.6%, Ti: 0.1-0.3%, ZrO2: 0.05-0.2%, B: 0.009-0.01%, La2O3: 0.3-0.85%, with the balance being Fe and unavoidable impurities. The particle size of the other raw material powders in the core powder, except for nano-sized La2O3 and nano-sized ZrO2, is 60-100 mesh.

2. The composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding according to claim 1, characterized in that, The content of nano-sized ZrO2 in the core powder is 0.1-0.2%, and the content of nano-sized La2O3 is 0.36-0.82%.

3. The composite particle-reinforced marine steel wire for ultra-high heat input gas-electric vertical welding according to claim 1, characterized in that, The diameter of the wire is 1.6 mm.

4. The preparation steps of the composite particle-reinforced marine steel ultra-high heat input gas-electric vertical welding wire according to claim 1, characterized in that, Includes the following steps: Step S1: After the core powder raw material is dehydrated and dried, it is sieved through an 80-mesh sieve. According to the required ratio, nano-sized La2O3, ZrO2 powder, and Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill jar for mixing. The ball milling parameters are: ball-to-material ratio of 5:1, ball milling time of 1-2 hours in forward rotation and 1-2 hours in reverse rotation, and rotation speed of 300 r / min to obtain the ball-milled mixed powder. Step S2: Mix TiO2, SiO2, and NaF slagging agent with the ball-milled mixed powder according to the specified ratio, put the mixture into a V-type mixer, and mix for 30 minutes to obtain a uniformly mixed core powder. Step S3: First, dry the low-carbon steel strip, then roll the steel strip into a U-shape using forming rollers. Add the mixed flux-cored powder to the U-shaped steel strip according to the required filling rate through a powder feeding device, and then further roll it into a tube. Then, feed the tubular welding wire into the drawing die and control the drawing speed at 1.2-1.5m / min for drawing. Repeat the above operation for redrawing until the desired diameter of 1.6mm flux-cored welding wire is obtained.

5. The application of the wire material according to claim 1 in ultra-high heat input welding of thick marine steel, characterized in that, The ultra-high heat input welding is a dual-wire gas-electric vertical welding method, with EH36 as the base material. Grade marine engineering steel, thickness 50-60mm, base material bevel design is single-sided V-shaped bevel, single-sided bevel angle is 12°, gap is 8-10mm, blunt edge bevel is no more than 1mm, the extension length of the two welding wires is 35mm, the welding torch angle is 4°~8°, the distance from the back wire to the backing is 20mm, and the spacing between the two welding wires is 19mm; welding process parameters are: back wire is DC positive polarity method, fixed without oscillation, current 450.1-481.9A, voltage 40.2-42.3V; front wire is DC reverse polarity method, oscillation width is 15~18mm, current 473.9-501.8A, voltage 48.9-52.8V; speed is 6-7cm / min, heat input is 606.7~781.3kJ / cm, welding is carried out under 100% CO2 gas protection conditions throughout the process.

Citation Information

Patent Citations

  • Flux-cored welding wire for large heat input gas-electric vertical welding and preparation method thereof

    CN104259688B

  • A flux-cored welding wire for high heat input welding, its preparation method and application

    CN109530961B

  • Super duplex stainless steel self-protection flux-cored wire and preparation method thereof

    CN113714682A

  • Flux-cored wire for ship plate steel ultra-large linear energy electro-gas welding and preparation method and application of flux-cored wire