Flame-retardant PVC power cable and preparation method thereof
By using flame retardants and coupling agents containing phosphorus and nitrogen elements in flame-retardant PVC cable materials to form porous foam structures and chemical grafting, the problem of reduced flame retardant performance in the existing technology is solved, and high efficiency and safety are achieved. Excellent flame retardant effect and excellent mechanical properties.
Patent Information
- Application Number
- CN202410934722.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-08
AI Technical Summary
The flame retardant in existing flame-retardant PVC cable materials is simply physically mixed and is easily affected by the external environment, resulting in a decrease in flame retardant performance. Increasing the amount of flame retardant will damage the mechanical properties of the material.
Using flame retardants containing phosphorus and nitrogen elements, a porous foam-like structure is formed through specific chemical reactions, combined with coupling agent modification to enhance material performance, ensuring that the flame retardants are evenly dispersed and chemically grafted with PVC resin to improve flame retardancy and toughness-enhancing properties.
It achieves efficient and safe flame retardant and smoke suppression effects and excellent mechanical properties. The flame retardant has good compatibility with other raw materials, enhances the toughness and softness of the cable material, and stably exists in the cable, improving the overall performance.
Smart Images

Figure BDA0004940944170000031 
Figure BDA0004940944170000032 
Figure BDA0004940944170000033
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electric wires and cables, and in particular relates to a flame-retardant PVC power cable and a preparation method thereof. Background Art
[0002] With the development of economy, the demand for wires and cables is increasing day by day, especially in the fields of high-rise buildings, electronic products, electrical appliances, automobiles, computers and aerospace industry products, the requirements for cable materials are getting higher and higher. Wires and cables are widely used in polyvinyl chloride materials. Polyvinyl chloride (PVC) resin is the second largest resin variety in the world after polyethylene. PVC resin has a series of advantages such as good rigidity, high strength, corrosion resistance, good electrical insulation, good processing performance, low price, cold resistance, good oil resistance, etc. It is an ideal power cable material.
[0003] However, once a fire occurs, it is difficult to extinguish the fire of wires and cables due to the concealed nature of their laying and the easy spread of fire caused by laying in bundles. More importantly, the combustion and decomposition of polyvinyl chloride produces toxic gases and a large amount of smoke, which brings difficulties to firefighting, escape, life-saving and other work. Chinese invention patent CN107619560A discloses a high-temperature flame-retardant PVC cable material, which includes the following components by weight: 120-150 parts of polyvinyl chloride, 5-10 parts of magnesium-aluminum alloy, 50-100 parts of flame retardant, 20-50 parts of dispersant and 5.2-10 parts of composite flame retardant synergist. The flame retardant in the cable material is as high as 50-100 parts. Although the flame retardant performance of the material can be significantly improved by increasing the amount of flame retardant, increasing the amount of flame retardant added will cause the mechanical properties of the material to decrease, and the flame retardant in the cable material is simply physically mixed in the cable material. Therefore, it is easy to be affected by the external environment and gradually migrate or fall out, resulting in a decrease in the flame retardant performance of the cable material. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a flame retardant PVC power cable and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a flame-retardant PVC power cable comprises the following steps:
[0007] All raw materials of the cable material are mixed evenly, then heated to 60-70°C and stirred for 20-30 minutes, then put into a twin-screw extruder for extrusion granulation, melted, extruded, coated on the side of the copper wire, cooled and solidified to obtain a flame-retardant PVC power cable.
[0008] Furthermore, the cable material includes the following raw materials in parts by weight: 100 parts of PVC resin, 50-60 parts of plasticizer, 40-50 parts of calcium carbonate, 6-10 parts of flame retardant, 5-10 parts of calcium zinc stabilizer, 1-3 parts of coupling agent, 0.8-1.2 parts of lubricant, 0.5-1 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 0.5-1 parts of colorant, and 0.01-0.02 parts of initiator.
[0009] Furthermore, the plasticizer is one or more of tricresyl phosphate, trioctyl trimellitate, dioctyl terephthalate, diisononyl cyclohexane 1,2-dicarboxylate, and dioctyl sebacate.
[0010] Furthermore, the flame retardant is prepared by the following steps:
[0011] S1. Blow nitrogen gas into a dry three-necked flask for 30 minutes to drive away the air in the flask, then add 2-propylene glycol 1,2-dimethyl ester, 3-amino-1-propanol, DBU (1,8-diazobispiro[5.4.0]undec-7-ene) and DMSO (dimethyl sulfoxide), stir evenly and place in a 30°C oil bath to react for 1 hour. After the reaction is completed, wash the reaction product with saturated brine for 3 times, take the organic phase, dry it with anhydrous sodium sulfate, filter it, and distill the filtrate under reduced pressure to obtain intermediate 1; the dosage ratio of 2-propylene glycol 1,2-dimethyl ester, 3-amino-1-propanol, DBU and DMSO is 6.2mL:3.3mL:1.5mL:100mL;
[0012] Under the catalytic action of DBU, the molar ratio of 2-propylene glycol 1,2-diyl ester to 3-amino-1-propanol is controlled to be 1:1.05-1.1, and 2-propylene glycol 1,2-diyl ester and 3-amino-1-propanol undergo Michael addition reaction. The reaction process is as follows:
[0013]
[0014] S2. Under nitrogen protection, add intermediate 1, triethylamine and DMSO into a dry three-necked flask, stir and dissolve, slowly add tetradecane chloride, react at 80° C. for 3 h, cool to room temperature after the reaction, and distill under reduced pressure to obtain intermediate 2; the amount ratio of intermediate 1, tetradecane chloride, triethylamine and DMSO is 10.3 g:12.3 mL:8.8 mL:100 mL;
[0015] Under the action of triethylamine, the molar ratio of intermediate 1 to tetradecyl chloride is controlled to be 1:1.05-1.1, and the -NH- of intermediate 1 and the -Cl of tetradecyl chloride undergo a nucleophilic substitution reaction. The reaction process is as follows:
[0016]
[0017] S3. Blow nitrogen gas into a dry three-necked flask for 30 minutes to drive away the air in the flask, then add phenylphosphonyl dichloride, triethylamine and DMSO, cool to 15°C with ice brine, slowly add intermediate 2 while stirring, keep the temperature at 15°C with ice brine, keep the reaction for 1.5 hours, and distill under reduced pressure after the reaction to obtain a flame retardant. The dosage ratio of phenylphosphonyl dichloride, intermediate 2, triethylamine and DMSO is 2.1mL:13.8g:5.2mL:130mL.
[0018] Under the action of triethylamine, the molar ratio of phenylphosphonyl dichloride and intermediate 2 is controlled to be 1:2.05-2.1, and phenylphosphonyl dichloride and intermediate 2 can undergo the following chemical reaction, and the reaction process is shown as follows:
[0019]
[0020] The flame retardant containing phosphorus element promotes the carbonization of polymer matrix and forms a molten carbon layer on the surface of polymer matrix, while the flame retardant containing nitrogen element decomposes under heat to generate non-combustible gases such as ammonia and nitrogen, which not only dilute the concentration of oxygen and combustible gas in the flame zone, but also make the molten carbon layer formed on the surface of polymer matrix expand and foam to form a porous foam structure, and the expanded porous foam carbon layer will block the process of heat and oxygen exchange between polymer matrix and the outside world, thereby preventing the polymer material from burning and achieving the final effect of flame retardancy. The flame retardant of the present invention does not contain halogen, will not pollute the environment, and through the synergistic effect of nitrogen and phosphorus, it gives the cable material an efficient and safe flame retardant effect.
[0021] The flame retardant contains a plurality of methylene long carbon chains (14 carbons) that can stretch and rotate freely, thus increasing the toughness and softness of the cable material and providing a relatively high resilience; the lipophilic long carbon chains, ester groups and benzene rings increase the compatibility between the flame retardant and the remaining raw materials; in addition, the flame retardant contains two terminal carbon-carbon double bonds, which can react chemically with the carbon-carbon double bonds at the ends of the PVC resin under the action of an initiator, thereby being grafted onto the PVC macromolecular chain; therefore, the flame retardant of the present invention can be uniformly dispersed and stably present in the cable material, fully and stably exerting the effects of flame retardancy, smoke suppression and toughening.
[0022] Furthermore, the coupling agent is one or more of an aluminate coupling agent and a silane coupling agent.
[0023] The inorganic-philic end and the organic-philic end of the coupling agent can react chemically with the surface of calcium carbonate and polyvinyl chloride resin or form entangled structures respectively, thereby enhancing the interfacial compatibility between calcium carbonate and organic resin. Therefore, modification with coupling agent can not only improve the processing performance of PVC cable materials filled with calcium carbonate, but also significantly improve the physical and mechanical properties of cable materials, reduce the water absorption rate of the product, reduce the oil absorption, and evenly disperse the filler.
[0024] Calcium carbonate can reduce the formulation cost and play a role in incremental reinforcement in PVC cable materials. In addition, calcium carbonate can adsorb ions and reduce the free mobility of conductive ions in the PVC system, which can not only improve the insulation performance of the product volume resistivity, but also improve the heat and oxygen aging resistance of the cable material, as well as its thermal deformation and mechanical properties.
[0025] Furthermore, the lubricant is one or more of butyl stearate, polyethylene wax, zinc stearate, and magnesium stearate.
[0026] Furthermore, the antioxidant is one or more of antioxidant DLTP, antioxidant 168, antioxidant 1035, antioxidant 1010, and antioxidant 1076.
[0027] Furthermore, the ultraviolet absorber is one or more of the ultraviolet absorber UV-531, 2,4,6-tris(2'-n-butoxyphenyl)-1,3,5-triazine, and light stabilizer GW-744.
[0028] Furthermore, the colorant is one or more of phthalocyanine blue, phthalocyanine green, azo yellow, azo orange, and quinacridone red.
[0029] Furthermore, the initiator is one or more of azobisisobutyronitrile, dicumyl peroxide, and dibenzoyl peroxide.
[0030] The invention also discloses a flame-retardant PVC power cable, which is prepared according to the preparation method of the flame-retardant PVC power cable.
[0031] Beneficial effects of the present invention: The flame retardant of the present invention contains halogen-free flame retardant elements phosphorus and nitrogen, and contains multiple long carbon chains (14 carbons). In addition, the flame retardant has good compatibility with other raw materials and there is a chemical reaction between the flame retardant and the polyvinyl chloride resin. Therefore, the cable of the present invention has efficient, safe and lasting flame retardant and smoke suppression effects and excellent and stable mechanical properties. The flame retardant and other raw materials work together to make the cable of the present invention have excellent comprehensive performance. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] The flame retardant is prepared in the following steps:
[0035] S1, nitrogen was blown into a dry 250mL three-necked flask for 30 minutes to drive away the air in the flask, and then 6.2mL 2-acrylic acid 1,2-ethylenediyl ester, 3.3mL 3-amino-1-propanol, 1.5mL DBU and 100mL DMSO were added, stirred evenly and placed in a 30°C oil bath for stirring and reaction for 1 hour. After the reaction was completed, the reaction product was washed 3 times with saturated brine, and the organic phase was dried with anhydrous sodium sulfate, filtered, and the filtrate was distilled under reduced pressure to obtain intermediate 1;
[0036] S2, under nitrogen protection, add 10.3 g of intermediate 1, 8.8 mL of triethylamine and 100 mL of DMSO into a dry 250 mL three-necked flask, stir to dissolve, slowly add 12.3 mL of tetradecane chloride, react at 80 °C for 3 h, cool to room temperature after the reaction, and distill under reduced pressure to obtain intermediate 2;
[0037] S3. Blow nitrogen gas into a dry 250mL three-necked flask for 30 minutes to drive away the air in the flask, then add 2.1mL phenylphosphonic dichloride, 5.2mL triethylamine and 130mL DMSO, cool to 15°C with ice brine, slowly add 13.8g intermediate 2 while stirring, and keep the temperature at 15°C with ice brine. Keep the reaction warm for 1.5 hours, and evaporate under reduced pressure after the reaction to obtain a flame retardant.
[0038] Example 2
[0039] The specific steps for preparing flame-retardant PVC power cable are as follows:
[0040] 100 parts of PVC resin, 50 parts of tricresyl phosphate, 40 parts of calcium carbonate, 6 parts of the flame retardant prepared in Example 1, 5 parts of calcium zinc stabilizer, 1 part of aluminate coupling agent DL411 produced by Hubei Maidehao Chemical Co., Ltd., 0.8 parts of butyl stearate, 0.5 parts of antioxidant 1010, 0.5 parts of ultraviolet absorber UV-531, 0.5 parts of phthalocyanine blue and 0.01 parts of azobisisobutyronitrile were mixed uniformly, heated to 60°C and stirred for 20 minutes to obtain a mixture; the mixture was put into a twin-screw extruder for extrusion granulation, and the extruder temperature was set to: 170°C for zone 1, 180°C for zone 2, and 190°C for zone 3 to obtain a cable material, the cable material was melted, extruded, coated on the side of the copper wire, cooled and solidified to obtain a flame-retardant PVC power cable.
[0041] Example 3
[0042] The specific steps for preparing flame-retardant PVC power cable are as follows:
[0043] 100 parts of PVC resin, 10 parts of tricresyl phosphate, 30 parts of cyclohexane 1,2-dicarboxylic acid diisononyl ester, 15 parts of dioctyl sebacate, 45 parts of calcium carbonate, 8 parts of the flame retardant prepared in Example 1, 7 parts of calcium zinc stabilizer, 2 parts of vinyl trimethoxysilane, 0.5 parts of polyethylene wax, 0.5 parts of zinc stearate, 0.4 parts of antioxidant DLTP, 0.4 parts of antioxidant 1035, 0.8 parts of 2,4,6-tri(2'-butoxy phenyl)-1,3,5-triazine, 0.8 parts of azo yellow, and 0.012 parts of diisopropylbenzene peroxide are mixed evenly, heated to 67°C and stirred for 24 minutes to obtain a mixture; the mixture is put into a twin-screw extruder for extrusion granulation, and the extruder temperature is set to: 175°C for zone one, 187°C for zone two, and 192°C for zone three to obtain a cable material, the cable material is melted, extruded, and coated on the side of the copper wire, and after cooling and solidification, a flame-retardant PVC power cable is obtained.
[0044] Example 4
[0045] The specific steps for preparing flame-retardant PVC power cable are as follows:
[0046] 100 parts of PVC resin, 10 parts of tricresyl phosphate, 20 parts of dioctyl terephthalate, 30 parts of cyclohexane 1,2-diisononyl dicarboxylate, 50 parts of calcium carbonate, 10 parts of the flame retardant prepared in Example 1, 10 parts of calcium zinc stabilizer, 3 parts of methacryloxymethyl trimethoxysilane, 0.6 parts of polyethylene wax, 0.6 parts of zinc stearate, 0.5 parts of antioxidant DLTP, 0.5 parts of antioxidant 1076, 0.5 parts of 2,4,6-tris (2'-butoxyphenyl) )-1,3,5-triazine, 0.5 parts of light stabilizer GW-744, 1 part of quinacridone red and 0.02 parts of dibenzoyl peroxide are mixed evenly, heated to 70°C and stirred for 30 minutes to obtain a mixture; the mixture is put into a twin-screw extruder for extrusion granulation, and the extruder temperature is set to: 180°C for zone one, 190°C for zone two, and 195°C for zone three to obtain a cable material, the cable material is melted, extruded, coated on the side of the copper wire, and cooled and solidified to obtain a flame-retardant PVC power cable.
[0047] Comparative Example 1
[0048] The specific steps for preparing flame-retardant PVC power cable are as follows:
[0049] The remaining steps remained unchanged, only the flame retardant in Example 4 was replaced by 5 parts of ammonium polyphosphate and 5 parts of melamine to prepare a PVC power cable.
[0050] Comparative Example 2
[0051] The specific steps for preparing flame-retardant PVC power cable are as follows:
[0052] The remaining steps remain unchanged, only the flame retardant in Example 4 is removed to prepare a PVC power cable.
[0053] Performance Testing
[0054] The cable materials obtained by extrusion granulation of Examples 2-4 and Comparative Examples 1-2 were injection molded on a micro injection molding machine to obtain standard specimens required for performance testing. The injection molding temperature was 180°C, the mold temperature was room temperature, and the elongation at break and tensile strength were tested using a UTM4204 electronic tensile testing machine according to GB / T1040.3-2006 and a tensile rate of 50 mm / min; the oxygen index was tested using the method specified in GB / T2406.2; and the fire rating was tested using UL94-2015. The test results are shown in Table 1 below:
[0055] Table 1
[0056] project Tensile strength MPa Elongation at break % Oxygen index% Example 2 14.2 403 39.8 Example 3 14.5 406 40.1 Example 4 14.7 407 40.2 Comparative Example 1 13.6 389 34.7 Comparative Example 2 13.4 386 21.9
[0057] It can be seen from Table 1 above that the cable materials obtained by extrusion granulation in Examples 2-4 of the present invention have more excellent flame retardant properties and mechanical properties.
[0058] The PVC power cables prepared in Examples 2-4 and Comparative Examples 1-2 were made into corresponding samples according to different test standards for performance testing, and the test results are shown in Table 2 below:
[0059] Table 2
[0060] project Fire resistance test Smoke density Flame retardant grade Test standards EN 50200 GB / T 8323 IEC 60332 Example 2 pass 63 A Example 3 pass 61 A Example 4 pass 60 A Comparative Example 1 pass 73 B Comparative Example 2 Not passed 195 D
[0061] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0062] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a flame-retardant PVC power cable, It is characterized in that The following steps are involved: All raw materials of the cable material are mixed evenly, heated, stirred, and then put into a twin-screw extruder for extrusion granulation, melted, extruded, coated on the side of the copper wire, cooled and solidified to obtain a PVC power cable; The cable material comprises the following raw materials in parts by weight: 100 parts of PVC resin, 50-60 parts of plasticizer, 40-50 parts of calcium carbonate, 6-10 parts of flame retardant, 5-10 parts of calcium zinc stabilizer, 1-3 parts of coupling agent, 0.8-1.2 parts of lubricant, 0.5-1 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 0.5-1 parts of colorant, and 0.01-0.02 parts of initiator; Wherein, the flame retardant is prepared by the following steps: S1. Add 2-propylene glycol 1,2-diyl ester, 3-amino-1-propanol, DBU and DMSO under nitrogen, stir, react at 30°C for 1 hour, wash, dry, filter, and distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, add intermediate 1, triethylamine and DMSO into a flask, stir and add tetradecane chloride, react at 80°C for 3h, cool and distill under reduced pressure to obtain intermediate 2; S3. After nitrogen is blown into the flask, phenylphosphonic acid dichloride, triethylamine and DMSO are added, the mixture is cooled to 15°C, intermediate 2 is added, the mixture is reacted at 15°C for 1.5 hours, and the mixture is distilled under reduced pressure to obtain a flame retardant.
2. A method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The usage ratio of 2-propylene glycol 1,2-diyl ester, 3-amino-1-propanol, DBU and DMSO in step S1 is 6.2 mL: 3.3 mL: 1.5 mL: 100 mL; the usage ratio of intermediate 1, tetradecane chloride, triethylamine and DMSO in step S2 is 10.3 g: 12.3 mL: 8.8 mL: 100 mL; the usage ratio of phenylphosphonic dichloride, intermediate 2, triethylamine and DMSO in step S3 is 2.1 mL: 13.8 g: 5.2 mL: 130 mL.
3. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The plasticizer is one or more of tricresyl phosphate, trioctyl trimellitate, dioctyl terephthalate, diisononyl cyclohexane 1,2-dicarboxylate, and dioctyl sebacate.
4. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The coupling agent is one or more of an aluminate coupling agent and a silane coupling agent.
5. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The lubricant is one or more of butyl stearate, polyethylene wax, zinc stearate and magnesium stearate.
6. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The antioxidant is one or more of antioxidant DLTP, antioxidant 168, antioxidant 1035, antioxidant 1010, and antioxidant 1076.
7. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The ultraviolet absorber is one or more of the ultraviolet absorber UV-531, 2,4,6-tris(2'-n-butoxyphenyl)-1,3,5-triazine, and the light stabilizer GW-744.
8. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The colorant is one or more of phthalocyanine blue, phthalocyanine green, azo yellow, azo orange and quinacridone red.
9. The method for preparing a flame-retardant PVC power cable according to claim 1, It is characterized in that The initiator is one or more of azobisisobutyronitrile, dicumyl peroxide and dibenzoyl peroxide.
10. A flame retardant PVC power cable, It is characterized in that The flame-retardant PVC power cable is prepared according to the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
High-temperature-resistant flame-retardant PVC (polyvinyl chloride) cable material
CN107619560A
Cited By
Preparation method of power cable with high-performance insulator material
CN119708715A
Composite material for automotive interior skins and method of making the same
CN123004056A