Method for recycling waste lithium iron phosphate and use thereof

By combining wet grinding and precipitation reaction with hydrothermal aging, the problems of resource waste of iron, phosphorus and carbon slag and high energy consumption of acid leaching in the recycling of lithium iron phosphate batteries have been solved. This has enabled a highly efficient and low-cost method for the reprocessing of lithium iron phosphate, improving the recovery rate of valuable elements and product performance.

CN118754080BActive Publication Date: 2026-11-24YICHANG BRUNP RECYCLING TECH CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410839541.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2026-11-24
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

In existing lithium iron phosphate battery recycling technologies, the selective extraction efficiency of metallic lithium is low, resulting in the waste of iron, phosphorus, and carbon slag resources. Furthermore, the acid leaching process has high energy consumption, affecting production efficiency and economic benefits.

Method used

Waste lithium iron phosphate, grinding aid, and oxidant are mixed and wet-milled to separate lithium extraction liquid and iron-phosphorus-carbon slag. Lithium phosphate and ferrous phosphate are obtained through precipitation reaction. Combined with hydrothermal aging method, reprocessed lithium iron phosphate is synthesized, reducing the amount of acid and alkali used and improving the recovery rate of valuable elements.

Benefits of technology

It achieves efficient and complete recovery of valuable elements in lithium iron phosphate battery waste, reduces production costs, reduces environmental and human health hazards, and improves the purity of lithium extraction solution and the performance of lithium iron phosphate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754080B_ABST
    Figure CN118754080B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of waste resource recycling. It provides a method for reprocessing waste lithium iron phosphate and its applications. The reprocessing method involves mixing and wet-milling waste lithium iron phosphate, a grinding aid, and an oxidant to obtain a lithium extraction solution and iron-phosphorus-carbon slag. Lithium phosphate is precipitated using the lithium extraction solution, and a pure ferrous dihydrogen phosphate solution is gradually prepared using the iron-phosphorus-carbon slag, which then precipitates ferrous phosphate. Finally, the obtained lithium phosphate and ferrous phosphate can be reacted to obtain reprocessed lithium iron phosphate. This reprocessing method achieves efficient and complete recovery of valuable elements from waste lithium iron phosphate batteries. Compared to existing acid leaching technologies, it significantly reduces the amount of acid and alkali used, and the reaction process is mild and controllable, resulting in lower production costs and reduced harm to the environment and human health.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of waste resource recycling, and relates to a method for reprocessing waste lithium iron phosphate and its uses. Background Technology

[0002] With the rapid development of the global new energy vehicle industry, lithium iron phosphate (LFP) batteries have become a significant force in the electric vehicle battery market due to their superior safety performance, long cycle life, environmental friendliness, and relatively economical price. In recent years, the installed capacity of LFP batteries has surpassed that of ternary lithium batteries, demonstrating their advantages in energy storage. However, the ensuing large-scale retirement of LFP batteries not only poses a potential threat to the environment but also presents a severe challenge to resource recycling.

[0003] In recent years, the number of retired power batteries in my country has been increasing year by year. Statistics show that in 2022, the theoretical retirement volume reached 700,000 tons, while the actual recycling volume was only 330,000 tons. In 2023, the theoretical retirement volume rapidly climbed to 810,000 tons, but the actual recycling volume was only 460,000 tons, meaning that nearly half of the batteries were not effectively recycled, highlighting the imperfections of the recycling system and insufficient processing capacity. It is projected that by 2026, the retired power battery volume will reach 968,000 tons, and by 2030, it will reach a massive 3 million tons. Therefore, establishing an efficient recycling and reuse mechanism has become an urgent priority.

[0004] Currently, my country generally employs wet recycling processes for the disposal of retired lithium iron phosphate batteries. This process mainly involves multiple stages, including battery dismantling, leaching extraction, impurity removal, and material regeneration. Although wet processes have demonstrated certain efficiency in metal extraction, they face numerous challenges in practical operation. First, from a technical perspective, the selective extraction of lithium metal is the core step. The currently widely used process is acid leaching, which uses sulfuric acid combined with hydrogen peroxide or air / oxygen oxidants to achieve leaching. While these methods can effectively extract lithium, they generate a large number of bubbles during the leaching process, which not only reduces the reaction rate but also increases energy consumption, seriously affecting overall production efficiency and economic benefits. More importantly, most of the current recycling processes focus on extracting lithium, while there is often a lack of effective recovery and reuse methods for the generated iron and phosphorus resources, leading to the idleness and waste of large amounts of iron, phosphorus, and carbon slag resources.

[0005] In conclusion, there is still a need to develop a simple and easy-to-implement process that can efficiently recycle and reuse all components of waste lithium iron phosphate batteries. This is the key to achieving green recycling and efficient resource utilization of retired lithium iron phosphate batteries across the entire supply chain and promoting the healthy development of the new energy industry. Summary of the Invention

[0006] In view of the problems existing in the prior art, the purpose of this invention is to provide a method for reprocessing waste lithium iron phosphate and its uses. The reprocessing method involves mixing waste lithium iron phosphate, a grinding aid, and an oxidant for wet milling to obtain a lithium extraction solution and iron-phosphorus-carbon slag. Lithium phosphate is precipitated using the lithium extraction solution, and a pure ferrous dihydrogen phosphate solution is gradually prepared using the iron-phosphorus-carbon slag, which then precipitates ferrous phosphate. Finally, the obtained lithium phosphate and ferrous phosphate can be reacted to obtain reprocessed lithium iron phosphate. This reprocessing method can achieve efficient and complete recovery of valuable elements from waste lithium iron phosphate batteries. Compared with existing acid leaching technology, it can greatly reduce the amount of acid and alkali used, and the reaction process is mild and controllable, with lower production costs, while also reducing harm to the environment and human health.

[0007] To achieve this objective, the present invention adopts the following technical solution:

[0008] In a first aspect, the present invention provides a method for reprocessing waste lithium iron phosphate, comprising:

[0009] (1) Mix waste lithium iron phosphate, grinding aid and oxidant, and perform first pulping and wet grinding to obtain lithium extraction liquid and iron-phosphorus carbon slag.

[0010] (2) The lithium extraction solution is subjected to a lithium precipitation reaction to obtain lithium phosphate and mother liquor; the iron-phosphorus carbon slag is mixed with phosphoric acid and subjected to a second wet milling process to obtain iron dihydrogen phosphate solution and carbon powder slag.

[0011] (3) The ferric dihydrogen phosphate solution is mixed with iron powder and a reduction reaction is carried out to obtain a crude ferrous dihydrogen phosphate solution.

[0012] (4) The crude ferrous dihydrogen phosphate solution is subjected to an aluminum precipitation reaction to obtain aluminum product and purified ferrous dihydrogen phosphate solution.

[0013] (5) The purified ferrous dihydrogen phosphate solution is subjected to an iron precipitation reaction to obtain ferrous phosphate;

[0014] (6) The ferrous phosphate obtained in step (5) is mixed with the lithium phosphate obtained in step (2), slurryed and hydrothermally aged to obtain reconstituted lithium iron phosphate.

[0015] The reprocessing method described in this invention mixes lithium iron phosphate waste with grinding aids and oxidants, and extracts lithium through wet grinding. The process is short, simple to operate, produces a near-neutral slurry with low impurity leaching rate, and the resulting lithium extraction solution requires no purification. The grinding aid primarily shortens grinding time, saves energy, and improves grinding efficiency. During wet grinding, the collision, proximity, and attraction between molecules or particles often lead to agglomeration of the powder, resulting in a "reverse grinding" phenomenon. This means that after the material reaches a certain fineness, continued grinding results in increasingly coarser particles. Adding a grinding aid allows it to firmly adhere to the cracks in the particles and penetrate deep into the cracks. New interfaces formed during particle grinding are quickly encapsulated by the grinding aid, hindering the recombination of these new interfaces and thus accelerating the grinding process. The oxidant primarily oxidizes lithium iron phosphate during the wet process, generating iron phosphate and releasing lithium ions. This invention uses phosphoric acid instead of sulfuric acid to dissolve iron-phosphorus carbon slag, which reduces the introduction of impurity ions (S). The wet milling method significantly improves the dissolution rate of iron-phosphorus slag. The reprocessing method described in this invention uses iron powder to reduce and adjust the phosphate value of ferric dihydrogen phosphate. Simultaneously, the iron powder reduces other heavy metal impurity ions in the solution, such as copper ions. The resulting crude solution is easily separated from impurities, effectively improving the impurity removal effect. This invention synthesizes reprocessed lithium iron phosphate through hydrothermal aging of recovered lithium phosphate and ferrous phosphate. The conditions are mild, and the morphology, particle size, and specific surface area of ​​the product can be further controlled by adjusting the temperature, time, and rotation speed of the hydrothermal aging reaction, resulting in reprocessed lithium iron phosphate with excellent performance.

[0016] In this invention, based on the mass of the obtained iron-phosphorus-carbon slag as 100%, the preferred mass percentage of iron phosphate is 55% to 75%, such as 55%, 58%, 60%, 63%, 65%, 68%, 70%, 72%, or 75%, preferably around 65%; the moisture percentage is 20% to 40%, such as 20%, 23%, 25%, 28%, 30%, 32%, 35%, 38%, or 40%, preferably around 30%; the carbon powder percentage is 1% to 10%, such as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%, preferably around 5%. At this point, adding phosphoric acid, which does not react with carbon, can ensure that the product generated is ferric dihydrogen phosphate.

[0017] In this invention, the hydrothermal aging reaction is mainly the hydrothermal reaction of ferrous phosphate and lithium phosphate to produce lithium iron phosphate. The aging reaction is a continuation of the hydrothermal reaction, which makes the hydrothermal reaction more thorough and the yield of lithium iron phosphate higher. At the same time, the aging reaction is also conducive to the growth of the generated lithium iron phosphate particles and the uniformity of particle size. The aging and hydrothermal reactions can be carried out continuously in one container.

[0018] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The technical objectives and beneficial effects of the present invention can be better achieved and realized through the following technical solutions.

[0019] As a preferred embodiment of the present invention, in step (1), the grinding aid includes a sulfate of at least one of sodium, potassium, and ammonium. For example, at least one of sodium sulfate, potassium sulfate, or ammonium sulfate.

[0020] Preferably, the oxidant includes at least one nitrate or hypochlorite selected from sodium, potassium, and ammonium, or at least one of hydrogen peroxide. Examples include at least one of sodium nitrate, potassium nitrate, ammonium nitrate, sodium hypochlorite, potassium hypochlorite, ammonium hypochlorite, or hydrogen peroxide.

[0021] Preferably, the mass percentage concentration of the hydrogen peroxide is 15% to 27.5%, such as 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, or 27.5%.

[0022] Preferably, the amount of the grinding aid is 0.2 to 2 times the mass of the waste lithium iron phosphate, for example, 0.2 times, 0.5 times, 0.8 times, 1 time, 1.2 times, 1.4 times, 1.6 times, 1.8 times or 2 times.

[0023] Preferably, the amount of oxidant used is 0.2 to 3 times the mass of the waste lithium iron phosphate, for example, 0.2 times, 0.5 times, 0.8 times, 1 time, 1.2 times, 1.4 times, 1.6 times, 1.8 times, 2 times, 2.2 times, 2.4 times, 2.6 times, 2.8 times, or 3 times.

[0024] Preferably, the pulping time for the first wet milling is 0.5 to 2 hours, for example, 0.5 hours, 0.8 hours, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours.

[0025] Preferably, the solid content of the slurry in the first wet milling is 10% to 30%, such as 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, or 30%.

[0026] Preferably, the feed flow rate of the first wet milling pulping process is 5% to 15% of the total pulp mass per min, such as 5% / min, 8% / min, 10% / min, 12% / min or 15% / min.

[0027] Preferably, the wet milling speed of the first pulping wet mill is 1000-3000 rpm, such as 1000 rpm, 1200 rpm, 1400 rpm, 1600 rpm, 1800 rpm, 2000 rpm, 2200 rpm, 2400 rpm, 2600 rpm, 2800 rpm or 3000 rpm, and the wet milling time is 0.5-5h, such as 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h.

[0028] As a preferred technical solution of the present invention, in step (2), the lithium extraction solution is mixed with phosphate source to carry out the lithium precipitation reaction.

[0029] Preferably, the phosphate source includes at least one phosphate selected from sodium, potassium, and ammonium. For example, at least one selected from sodium phosphate, potassium phosphate, or ammonium phosphate.

[0030] The reprocessing method described in this invention uses the phosphate source, such as sodium phosphate, mixed with lithium extraction solution to precipitate lithium and prepare lithium phosphate. The direct recovery rate of lithium is high, which facilitates the subsequent preparation of lithium iron phosphate.

[0031] Preferably, the amount of phosphate source used is 1.1 to 1.5 times the theoretical reaction amount with lithium in the lithium extraction solution, for example, 1.1 times, 1.2 times, 1.3 times, 1.4 times or 1.5 times.

[0032] Preferably, the temperature of the lithium precipitation reaction is 85-95℃, such as 85℃, 86℃, 87℃, 88℃, 89℃, 90℃, 91℃, 92℃, 93℃, 94℃ or 95℃, etc.; and the time is 0.1-2h, such as 0.1h, 0.3h, 0.5h, 0.8h, 1h, 1.2h, 1.4h, 1.6h, 1.8h or 2h, etc.

[0033] Preferably, the pH value of the lithium precipitation reaction is 12 to 13, such as 12, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9 or 13.

[0034] Preferably, after the lithium precipitation reaction, solid-liquid separation, drying, and pulverization are performed sequentially to obtain the lithium phosphate.

[0035] Preferably, the mother liquor is recycled as the grinding aid in step (1).

[0036] As a preferred technical solution of the present invention, the amount of phosphoric acid and the iron-phosphorus-carbon slag is controlled according to the ratio of the molar amount of phosphate in the phosphoric acid to the molar amount of iron in the iron-phosphorus-carbon slag (3-4.5):1, for example 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1 or 4.5:1, etc.

[0037] The chemical formula of the ferric dihydrogen phosphate generated in this invention is Fe(H2PO4)3. Therefore, based on the molar ratio of iron to phosphate in the ferric dihydrogen phosphate being 3:1, phosphoric acid is added in excess of 20% to 50%, preferably with a molar ratio of phosphate to iron in the iron-phosphorus carbon slag of (3 to 4.5):1. It should also be noted that this invention does not limit the specific concentration of phosphoric acid. The concentration and amount of phosphoric acid should be determined according to the specific amount of iron-phosphorus carbon slag used and the required molar ratio of iron to phosphate. Phosphoric acid with a mass percentage concentration of 20% to 85% can be reasonably selected and applied in this invention.

[0038] Preferably, the pulping time for the second wet milling is 0.5 to 2 hours, for example, 0.5 hours, 0.8 hours, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours.

[0039] Preferably, the solid content of the slurry in the second wet milling is 20% to 40%, such as 20%, 23%, 25%, 28%, 30%, 33%, 35%, 38%, or 40%.

[0040] Preferably, the feed flow rate of the second wet milling pulping process is 5% to 15% of the total pulp mass per min, such as 5% / min, 8% / min, 10% / min, 12% / min or 15% / min.

[0041] Preferably, the wet milling speed of the second pulping wet milling is 1000-3000 rpm, such as 1000 rpm, 1200 rpm, 1400 rpm, 1600 rpm, 1800 rpm, 2000 rpm, 2200 rpm, 2400 rpm, 2600 rpm, 2800 rpm or 3000 rpm, and the wet milling time is 0.5-5h, such as 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h.

[0042] As a preferred technical solution of the present invention, in step (3), the endpoint pH value of the reduction reaction is 2 to 3, for example, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3.

[0043] Preferably, the reduction reaction time is 3 to 5 hours, for example, 3 hours, 3.3 hours, 3.5 hours, 3.8 hours, 4 hours, 4.3 hours, 4.5 hours, 4.8 hours, or 5 hours.

[0044] As a preferred technical solution of the present invention, in step (4), the crude ferrous dihydrogen phosphate solution is mixed with at least one fluoride salt of sodium, potassium, or ammonium, such as at least one of sodium fluoride, potassium fluoride, or ammonium fluoride, preferably sodium fluoride, to carry out the aluminum precipitation reaction.

[0045] Preferably, the amount of the fluoride salt used is 0.5 to 2 times the theoretical reaction amount with aluminum in the crude ferrous dihydrogen phosphate solution, for example, 0.2 times, 0.4 times, 0.6 times, 0.8 times, 1 time, 1.2 times, 1.4 times, 1.6 times, 1.8 times or 2 times, etc.

[0046] When sodium fluoride is used for aluminum precipitation in this invention, the resulting aluminum product is cryolite; when potassium fluoride is used for aluminum precipitation in this invention, the resulting aluminum product is potassium cryolite; when ammonium fluoride is used for aluminum precipitation in this invention, the resulting aluminum product is ammonium hexafluoroaluminate.

[0047] Preferably, the time for the aluminum deposition reaction is 1 to 3 hours, such as 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, or 3 hours.

[0048] As a preferred technical solution of the present invention, in step (5), the purified ferrous dihydrogen phosphate solution is mixed with an alkaline source to carry out the iron precipitation reaction.

[0049] Preferably, the alkali source includes at least one carbonate and / or hydroxide of sodium, potassium, or ammonium. More preferably, it is at least one of sodium carbonate, potassium carbonate, or ammonium carbonate.

[0050] In this invention, the main function of the alkali source is to adjust the pH value. For example, sodium hydroxide, ammonia, and sodium carbonate are used. However, sodium hydroxide / potassium hydroxide is more alkaline than sodium carbonate, and local over-alkali formation of ferrous hydroxide is likely to occur during the pH adjustment process, resulting in low purity of the generated ferrous phosphate. It is preferable to use a corresponding alkali solution with a mass percentage concentration of 1% to 10%. When using ammonia, ammonia gas is easy to volatilize during the pH adjustment process, resulting in a poor operating environment. Therefore, it is further preferred to use a carbonate source, i.e., a carbonate of at least one of sodium, potassium, and ammonium.

[0051] Preferably, the pH value of the iron precipitation reaction is 5 to 7, such as 5, 5.2, 5.4, 5.6, 5.8, 6, 6.2, 6.4, 6.6, 6.8 or 7.

[0052] Preferably, the iron deposition reaction time is 1 to 3 hours, such as 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, or 3 hours.

[0053] As a preferred technical solution of the present invention, in step (6), the hydrothermal aging reaction is carried out under an inert atmosphere.

[0054] Preferably, the temperature of the hydrothermal aging reaction is 90–200°C, such as 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, or 200°C, and the time is 10–30 hours, such as 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours, or 30 hours.

[0055] Preferably, after the hydrothermal aging reaction is completed, the obtained product is dried at 80-120°C, for example, 80°C, 90°C, 100°C, 110°C or 120°C, for 4-8 hours, for example, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, to obtain the reconstituted lithium iron phosphate.

[0056] In a second aspect, the present invention provides a reconstituted lithium iron phosphate, obtained according to the reconstituted method described in the first aspect.

[0057] Thirdly, the present invention provides a lithium-ion battery containing the recycled lithium iron phosphate described in the second aspect.

[0058] Due to space limitations and to avoid redundancy, this invention does not list all point values ​​within the above numerical range, but it is not limited to the listed values ​​either; other unlisted values ​​within the above numerical range are also applicable.

[0059] Compared with existing technical solutions, the present invention has at least the following beneficial effects:

[0060] The reprocessing method described in this invention enables efficient and complete recovery of valuable elements from lithium iron phosphate battery waste. Compared to existing acid leaching technologies, it significantly reduces the amount of acid and alkali used, and the reaction process is mild and controllable, resulting in lower production costs and reduced harm to the environment and human health. The resulting reprocessed lithium iron phosphate exhibits excellent performance. Attached Figure Description

[0061] Figure 1 This is a schematic flowchart of the method for reprocessing waste lithium iron phosphate in Example 1;

[0062] Figure 2 This is the XRD pattern of the reconstituted lithium iron phosphate obtained in Example 1. Detailed Implementation

[0063] The technical solution of the present invention will be further illustrated below through specific embodiments.

[0064] Those skilled in the art will understand that the embodiments described are merely illustrative of the invention and should not be construed as limiting the invention.

[0065] Example 1

[0066] This embodiment provides a method for reprocessing waste lithium iron phosphate, such as... Figure 1 As shown, it includes:

[0067] (1) Prepare 1000g of waste lithium iron phosphate A (its composition is shown in Table 1); place the waste lithium iron phosphate A in a beaker, add 500g of grinding aid sodium sulfate (0.5 times its mass), 500g of oxidant hydrogen peroxide (mass percentage concentration of 20%) (0.5 times its mass), and pure water, and stir at room temperature for 0.5h to prepare a slurry with a solid content of 30%; add the mixed slurry to the feed hopper of the overflow wet mill using a slurry peristaltic pump, control the feed flow rate to 10% / min of the total slurry mass, and perform wet milling at 60℃. Connect the discharge pipe of the wet mill to the beaker containing the mixed slurry, and perform circulating wet milling during wet milling. Connect the condensate pipe during wet milling and pass water to the wet mill for cooling. After wet milling at 2000rpm for 5h, export all the wet milled slurry and perform solid-liquid separation to obtain lithium extraction liquid and iron-phosphorus-carbon slag;

[0068] (2) Heat the lithium extraction solution to 90°C, add a saturated solution of sodium phosphate (a source of phosphate), control the pH value to 12.6, carry out the lithium precipitation reaction for 0.5 h, and separate the solid and liquid to obtain lithium phosphate and mother liquor A (containing sodium sulfate); the obtained lithium phosphate is rinsed twice with pure water, dried and pulverized to obtain battery-grade lithium phosphate, and the obtained mother liquor A is appropriately concentrated and used as a grinding aid in step (1) for repeated recycling. 1000g of iron-phosphorus carbon slag was collected and placed in a beaker. 500g of phosphoric acid and pure water were added according to a molar ratio of phosphate to iron in the slag (3.5:1). The mixture was stirred for 0.5 hours to prepare a slurry with a solid content of 30%. The homogenized slurry was then fed into the feed hopper of an overflow wet mill using a peristaltic pump for wet milling. The discharge pipe of the wet mill was connected to the beaker containing the homogenized slurry. Circulation was performed during wet milling, and a condensate pipe was connected to cool the mill. After wet milling at 2000 rpm for 5 hours, all the wet-milled slurry was discharged and subjected to solid-liquid separation to obtain ferric dihydrogen phosphate solution and carbon powder slag.

[0069] (3) Add reduced iron powder to the ferrous dihydrogen phosphate solution and carry out the reduction reaction for 4 hours. Control the pH value at the end of the reaction to be 2.5 so as to reduce all ferric iron to ferrous iron and remove copper. Filter to obtain crude ferrous dihydrogen phosphate solution; excess reduced iron powder is washed and reused.

[0070] (4) Add sodium fluoride salt to the crude ferrous phosphate solution, and control the amount of fluoride salt to be 1.3 times the theoretical reaction amount with aluminum in the crude ferrous phosphate solution. Perform aluminum precipitation reaction for 2 hours, and separate solid and liquid to obtain crude cryolite and purified ferrous phosphate solution. Refine the crude cryolite to obtain refined cryolite.

[0071] (5) Add a saturated solution of sodium carbonate, a source of carbonate, to the purified ferrous dihydrogen phosphate solution until the pH value is 6, and carry out the iron precipitation reaction for 2 hours to obtain mother liquor B and ferrous phosphate octahydrate. Rinse the obtained ferrous phosphate octahydrate twice with deionized water.

[0072] (6) The battery-grade lithium phosphate obtained in step (2) and the washed ferrous phosphate octahydrate obtained in step (5) are mixed in equimolar amounts and slurried. The mixture is placed in a high-pressure reactor, heated to 180°C, and subjected to hydrothermal aging reaction for 20 hours. After solid-liquid separation, the mixture is rinsed twice with deionized water and dried in a nitrogen atmosphere furnace at 100°C for 6 hours to obtain reconstituted lithium iron phosphate.

[0073] Example 2

[0074] This embodiment provides a method for reprocessing waste lithium iron phosphate. The reprocessing method expands the production scale. In step (1), 5 kg of waste lithium iron phosphate A is used, and in step (2), 5 kg of iron-phosphorus carbon slag is used. The amounts of other raw materials are adjusted accordingly. Except for the above, the other conditions are exactly the same as in embodiment 1.

[0075] Example 3

[0076] This embodiment provides a method for reprocessing waste lithium iron phosphate. In step (1), another type of waste lithium iron phosphate B (whose composition is shown in Table 1) is used. Except for the above, the other conditions are exactly the same as in Example 1.

[0077] Example 4

[0078] This embodiment provides a method for reprocessing waste lithium iron phosphate. In step (1) of the reprocessing method, the oxidant is replaced by sodium nitrate instead of hydrogen peroxide. Except for the above, the other conditions are exactly the same as in Example 1.

[0079] Example 5

[0080] This embodiment provides a method for reprocessing waste lithium iron phosphate. In step (1) of the reprocessing method, the oxidant is replaced by sodium hypochlorite instead of hydrogen peroxide. Except for the above, the other conditions are exactly the same as in Example 1.

[0081] Characterization and testing:

[0082] Figure 2The image shows the XRD pattern of the reconstituted lithium iron phosphate obtained in Example 1. As can be seen from the image, the obtained reconstituted lithium iron phosphate conforms to the lithium iron phosphate phase of the PDF card.

[0083] The elemental composition of the raw materials, intermediate products and final products involved in the recycling method of waste lithium iron phosphate in Example 1 was tested, and the results are shown in Tables 1 and 2.

[0084] Table 1

[0085] Sample of Example 1 Li Fe P Cu Al Ni Co Mn Waste lithium iron phosphate A (wt%) 4.17 34.11 18.61 0.0006 0.0846 0.1383 0.0185 0.1278 Lithium extraction solution (g / L) 20.23 0.001 0.001 0.0003 0.0001 0.0001 0.0001 0.0001 Iron-phosphorus-carbon slag (wt%) 0.072 34.23 18.68 0.0007 0.085 0.140 0.019 0.13 Mother liquor A (g / L) 1.45 0.001 0.001 0.0003 0.0001 0.0001 0.0001 0.0001 Ferric dihydrogen phosphate solution (g / L) 0.11 45.23 40.1 0.23 0.45 0.01 0.003 0.01 Crude ferrous dihydrogen phosphate solution (g / L) 0.11 72.368 40.135 0.001 0.43 0.01 0.003 0.01 Ferrous dihydrogen phosphate purification solution (g / L) 0.1 71.21 39.87 0.001 0.01 0.01 0.003 0.01 Mother liquor B (g / L) 0.06 2.34 1.34 0.0001 0.0001 0.0001 0.0001 0.0001

[0086] Table 2

[0087]

[0088]

[0089] The elemental composition of the raw materials, intermediate products and final products involved in the recycling method of waste lithium iron phosphate in Example 3 was tested, and the results are shown in Tables 3 and 4.

[0090] Table 3

[0091] Sample of Example 3 Li Fe P Cu Al Ni Co Mn Waste lithium iron phosphate B (wt%) 2.8 22.4 12.4 0.8 1.1 0.15 0.04 0.23 Lithium extraction solution (g / L) 14.2 0.01 0.01 0.001 0.005 0.001 0.001 0.001 Iron-phosphorus-carbon slag (wt%) 0.09 22.38 12.38 0.08 1.09 0.15 0.04 0.23 Mother liquor A (g / L) 1.56 0.001 0.001 0.001 0.001 0.001 0.001 0.001 Ferric dihydrogen phosphate solution (g / L) 0.01 41.32 37.21 1.45 1.87 0.23 0.06 0.35 Crude ferrous dihydrogen phosphate solution (g / L) 0.01 63.34 37.21 0.001 1.85 0.22 0.06 0.35 Ferrous dihydrogen phosphate purification solution (g / L) 0.01 61.23 37.01 0.001 0.034 0.21 0.06 0.34 Mother liquor B (g / L) 0.01 2.34 1.36 0.001 0.001 0.001 0.001 0.15

[0092] Table 4

[0093] Sample of Example 3 Li P <![CDATA[PO4 3- ]]> Fe Cu Al <![CDATA[H2O]]> Li / P Fe / P Lithium phosphate (wt%) 12.33 18.25 37.6 0.01 0.001 0.001 32.3 2.99 - Ferrous phosphate octahydrate (wt%) 0.001 4.31 12.35 11.89 0.001 0.001 72.43 - 1.52 Reconstituted lithium iron phosphate (wt%) 4.40 19.56 40.32 35.12 0.001 0.001 0.11 0.99 0.99 National standard lithium iron phosphate (wt%) 4.4±1 20±1 / 35±2 / / / / /

[0094] The elemental composition of the reconstituted lithium iron phosphate obtained in Examples 2-5 was tested, and the results are shown in Table 5.

[0095] Table 5

[0096] Reconstituted lithium iron phosphate (wt%) Li P <![CDATA[PO4 3- ]]> Fe Cu Al <![CDATA[H2O]]> Li / P Fe / P Example 2 4.38 19.51 40.34 35.08 0.001 0.02 0.1 0.99 0.99 Example 4 4.23 18.50 40.28 35.07 0.001 0.03 0.1 1.01 1.04 Example 5 4.34 18.50 40.31 35.02 0.001 0.02 0.1 1.03 1.04 National Standard Lithium Iron Phosphate 4.4±1 20±1 / 35±2 / / / / /

[0097] Note: In Tables 1-5, "-" indicates values ​​that are too small to be considered; " / " indicates that no calculation is needed. The molar ratios Li / P and Fe / P are calculated with relative molecular masses of 7 for Li, 56 for Fe, and 31 for P.

[0098] The reconstituted lithium iron phosphate obtained in Examples 1-5 was used as the cathode material to prepare batteries for testing.

[0099] Weigh out the positive electrode material, acetylene black, and polytetrafluoroethylene (PTFE) in a mass ratio of 80:10:10. Thoroughly mix and grind the positive electrode material and acetylene black until homogeneous, then add the PTFE. Press the mixture onto a roller mill to form a positive electrode film of uniform thickness. Place the resulting positive electrode film in a vacuum drying oven and dry it at 120°C for 12 hours. Press the dried positive electrode film tightly together with aluminum foil to obtain the positive electrode sheet.

[0100] Battery assembly: The prepared and weighed positive electrode sheet was placed in an argon-filled glove box. A lithium metal sheet was used as the negative electrode. The electrolyte was 1 mol / L LiPF6 (EC+DEC, volume ratio 1:1), and the separator was a Celgard 2400 type. A CR2032 coin cell was assembled. After assembly, the battery was removed, sealed, and allowed to stand for 12 hours before testing.

[0101] The first charge specific capacity and first discharge specific capacity at 0.1C were tested with a charging cutoff voltage of 4V and a discharging cutoff voltage of 2V; the discharge specific capacity at 1C was then tested with a charging cutoff voltage of 3.75V and a discharging cutoff voltage of 2V. The results are recorded in Table 6.

[0102] Table 6

[0103]

[0104] Analysis based on Tables 1, 2, 3, 4, 5, and 6 shows that, regarding copper and aluminum impurities, iron powder is added during the reprocessing of lithium iron phosphate to remove copper and sodium fluoride to remove aluminum. Therefore, the content of copper and aluminum impurities in lithium phosphate, iron phosphate, and lithium iron phosphate is low, and their impact on the electrochemical performance of the reprocessed lithium iron phosphate material is minimal. Regarding impurities such as nickel, cobalt, and manganese, although there are no specific removal methods in the reprocessing method described in this invention, resulting in a certain amount of nickel, cobalt, and manganese in ferrous phosphate and reprocessed lithium iron phosphate, the presence of nickel, cobalt, and manganese in reprocessed lithium iron phosphate has no significant impact on the initial charge specific capacity at 0.1C, the initial discharge specific capacity, or the discharge specific capacity at 1C.

[0105] As can be seen from the above, the reprocessing method described in this invention can achieve efficient and complete recovery of valuable elements from lithium iron phosphate battery waste. Compared with existing acid leaching technology, it can greatly reduce the amount of acid and alkali used, and the reaction process is mild and controllable, with lower production costs, while also reducing harm to the environment and human health. The resulting reprocessed lithium iron phosphate possesses excellent performance.

[0106] This invention illustrates the detailed process equipment and process flow through the above embodiments. However, this invention is not limited to the detailed process equipment and process flow described above, meaning that this invention does not necessarily depend on the detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of raw materials for the product of this invention, addition of auxiliary components, and selection of specific methods, all fall within the protection scope and disclosure scope of this invention.

[0107] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0108] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0109] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A method for reprocessing waste lithium iron phosphate, characterized in that, include: (1) Waste lithium iron phosphate, grinding aid and oxidant are mixed and subjected to first pulping and wet grinding to obtain lithium extraction liquid and iron-phosphorus carbon slag; the grinding aid includes at least one sulfate of sodium, potassium and ammonium; (2) The lithium extraction solution is subjected to a lithium precipitation reaction to obtain lithium phosphate and mother liquor; the iron-phosphorus carbon slag is mixed with phosphoric acid and subjected to a second wet milling process to obtain iron dihydrogen phosphate solution and carbon powder slag. (3) The ferric dihydrogen phosphate solution is mixed with iron powder and a reduction reaction is carried out to obtain a crude ferrous dihydrogen phosphate solution; (4) The crude ferrous dihydrogen phosphate solution is subjected to an aluminum precipitation reaction to obtain aluminum product and purified ferrous dihydrogen phosphate solution; (5) The purified ferrous dihydrogen phosphate solution is subjected to an iron precipitation reaction to obtain ferrous phosphate; (6) The ferrous phosphate obtained in step (5) is mixed with the lithium phosphate obtained in step (2), slurryed and hydrothermally aged to obtain reconstituted lithium iron phosphate.

2. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The oxidant includes at least one of sodium, potassium, or ammonium nitrates, hypochlorite, or hydrogen peroxide.

3. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The amount of the grinding aid is 0.2 to 2 times the mass of the waste lithium iron phosphate.

4. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The amount of oxidant used is 0.2 to 3 times the mass of the waste lithium iron phosphate.

5. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The pulping time for the first wet milling process is 0.5 to 2 hours.

6. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The solid content of the pulp from the first wet milling process is 10% to 30%.

7. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The feed flow rate of the first wet milling pulping process is 5%~15% / min of the total pulp mass.

8. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The wet milling speed of the first pulping process is 1000~3000 rpm, and the wet milling time is 0.5~5h.

9. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, In step (2), the lithium extraction solution is mixed with phosphate source to carry out the lithium precipitation reaction.

10. The method for reprocessing waste lithium iron phosphate according to claim 9, characterized in that, The phosphate source includes at least one phosphate selected from sodium, potassium, and ammonium.

11. The method for reprocessing waste lithium iron phosphate according to claim 9, characterized in that, The amount of phosphate source used is 1.1 to 1.5 times the theoretical reaction amount with lithium in the lithium extraction solution.

12. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The lithium precipitation reaction is carried out at a temperature of 85~95℃ for a time of 0.1~2h.

13. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The pH value of the lithium precipitation reaction is 12-13.

14. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, After the lithium precipitation reaction, solid-liquid separation, drying and pulverization are carried out in sequence to obtain the lithium phosphate.

15. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The mother liquor is recycled as the grinding aid in step (1).

16. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, In step (2), the amount of phosphoric acid and the iron-phosphorus-carbon slag is controlled according to the ratio of the molar amount of phosphate in the phosphoric acid to the molar amount of iron in the iron-phosphorus-carbon slag (3~4.5):

1.

17. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The pulping time for the second wet milling process is 0.5 to 2 hours.

18. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The solid content of the pulp from the second wet milling process is 20% to 40%.

19. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The feed flow rate of the second wet milling pulping process is 5%~15% / min of the total pulp mass.

20. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The second wet milling process involves a milling speed of 1000~3000 rpm and a milling time of 0.5~5 h.

21. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, In step (3), the endpoint pH value of the reduction reaction is 2~3.

22. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The reduction reaction takes 3 to 5 hours.

23. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, In step (4), the crude ferrous dihydrogen phosphate solution is mixed with at least one fluoride salt of sodium, potassium, or ammonium to carry out the aluminum precipitation reaction.

24. The method for reprocessing waste lithium iron phosphate according to claim 23, characterized in that, The amount of the fluoride salt used is 0.5 to 2 times the theoretical reaction amount with aluminum in the crude ferrous dihydrogen phosphate solution.

25. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The time for the aluminum deposition reaction is 1 to 3 hours.

26. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, In step (5), the purified ferrous dihydrogen phosphate solution is mixed with an alkaline source to carry out the iron precipitation reaction.

27. The method for reprocessing waste lithium iron phosphate according to claim 26, characterized in that, The alkali source includes at least one carbonate and / or hydroxide of sodium, potassium, and ammonium.

28. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The pH value of the iron precipitation reaction is 5-7.

29. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The iron deposition reaction takes 1 to 3 hours.

30. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, In step (6), the hydrothermal aging reaction is carried out under an inert atmosphere.

31. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, The hydrothermal aging reaction is carried out at a temperature of 90~200℃ for a time of 10~30h.

32. The method for reprocessing waste lithium iron phosphate according to claim 1, characterized in that, After the hydrothermal aging reaction is completed, the resulting product is dried at 80~120℃ for 4~8h to obtain the reconstituted lithium iron phosphate.

Citation Information

Patent Citations

  • Method for preparing lithium iron phosphate positive electrode material in directional recycling manner from waste lithium iron phosphate battery

    WO2024082544A1