Preparation method of metal / nitrogen-doped spiral nano carbon wave-absorbing material

By introducing metal/nitrogen doping into the spiral carbon nanotube matrix and utilizing orbital coupling and spin polarization characteristics, a metal/nitrogen-doped spiral nanocarbon absorbing material was prepared, which solved the single absorption mode of existing microwave absorbing materials. It solves the problem of narrow bandwidth and achieves ultra-wideband electromagnetic wave absorption performance, which is suitable for a variety of scenarios and has promotion value especially in the military field.

CN118754108AActive Publication Date: 2024-10-11NANCHANG HANGKONG UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410921597.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-11
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

Existing microwave absorbing materials have problems such as single energy loss mode, high filling ratio and density, narrow microwave absorption bandwidth and single function, making them unable to be applied and promoted.

Method used

The preparation method of metal/nitrogen-doped spiral nanocarbon absorbing materials is adopted. By introducing the M-N-C configuration on the spiral carbon nanotube matrix, the orbital coupling and unique spin polarization characteristics of the 3d orbital of the metal and the 2p orbital of N are used. , enhance the absorption performance of electromagnetic waves, and increase multiple reflections and scattering through the spiral structure to form ultra-broadband absorption.

Benefits of technology

It achieves ultra-wideband electromagnetic wave absorption at low filling ratio and thin thickness, significantly improves electromagnetic wave absorption performance, has multi-functional applicability, can achieve more than 90% absorption efficiency in the entire frequency band, and has wide application prospects in the military field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754108A_ABST
    Figure CN118754108A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a metal / nitrogen-doped spiral nano carbon wave-absorbing material, and relates to a preparation method of a metal / nitrogen-doped carbon wave-absorbing material. The invention aims to solve the technical problems that the existing microwave absorbing material is single in energy loss mode, large in packing ratio and density, narrow in microwave absorbing bandwidth and single in function and cannot be applied and popularized. Metal ions are loaded into a helical carbon nanotube matrix in situ, and high-performance M / N-HCNT is prepared through an external thermal driving process, so that orbit coupling, spin polarization and cross polarization are formed by a unique atomic configuration of M-N-C and a unique geometric configuration of a helical structure, and the electromagnetic wave absorption characteristic of the material is cooperatively regulated and controlled. The material has the advantages of strong attenuation capability, broadband absorption, excellent wave-absorbing performance and the like, and has extremely high application value in both civil and military fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a metal / nitrogen doped carbon wave absorbing material. Background Art

[0002] The emergence of 5G technology and the popularization of wireless communication technology and high-power electronic devices have led to a surge in electromagnetic (EM) pollution. Although electromagnetic wave absorbing (EMWA) materials have been widely developed, their practical application remains challenging. Atomic doping strategies provide an excellent choice for the preparation of high-performance EMWA properties. This method induces lattice distortion, strain, and active point defects, generates a large number of dipole centers and in-plane topological defects, which accelerate the accumulation of electrons, trigger Maxwell polarization, and ultimately regulate the EM properties of the material. It is worth noting that the metal-nitrogen-carbon (MNC) configuration has gained widespread attention in various fields due to its high surface free energy, ultra-high atomic utilization, and quantum size effect. The orbital coupling between the 3d orbital of the metal and the 2p orbital of N induces a change in the charge arrangement, generating a new electronic state (d-band) near the Fermi level. This significantly improves the conductivity and dielectric loss. In addition, the spin polarization generated by the electron spin promotes the formation of high-spin states and enhances electromagnetic attenuation.

[0003] The geometric configuration of electromagnetic wave absorbers also plays a key role in the performance of EMWA. Helical materials have attracted research attention due to their unique symmetry and electromagnetic coupling properties. The helical structure can increase additional electromagnetic losses by simultaneously inducing electric and magnetic polarization. Notably, Zuo et al. constructed materials with helical nanotubes and studied the effect of spatial configuration on the dielectric constant, revealing additional cross-polarization and a broadband electromagnetic wave absorption with a bandwidth of 6.7 GHz (Zuo X, Zhang H, Zhou C, Zhao Y, Huang H, Wen N, Sun C, Fan Z, Pan L, Hierarchical and porous structures of carbon nanotubes-anchored MOF derivatives bridged by carbon nanocoils as lightweight and broadband microwave absorbers, Small 2023, 19: 2301992.). The results show that the helical structure effectively reduces the sensitivity of EMWA materials to frequency and is conducive to the formation of broadband absorption. In addition, Huang et al. demonstrated that the electromagnetic field is uniformly distributed along the length direction in electromagnetic simulations. However, the introduction of the helical structure destroys the original electromagnetic field distribution, causing it to redistribute along the direction of the helix (Huang L, Duan Y, Shi Y, Ma X, Pang H, Zeng Q, Che R, Chiral asymmetric polarizations generated by bioinspired helical carbon fibers to induce broadband microwave absorption and multispectral photonic manipulation, Advanced Optical Materials, 2022, 10, 220024.). This phenomenon causes a strong electromagnetic resonance, further enhancing the attenuation of electromagnetic waves EMW. Summary of the invention

[0004] The present invention aims to solve the technical problems that existing microwave absorbing materials have a single energy loss mode, a large filling ratio and density, a narrow microwave absorption bandwidth and a single function and cannot be applied and promoted, and provides a method for preparing a metal / nitrogen-doped spiral nanocarbon absorbing material.

[0005] The preparation method of the metal / nitrogen-doped helical nanocarbon absorbing material of the present invention is carried out according to the following steps:

[0006] 1. Dissolve phenylglycine and sodium hydroxide together in a mixed solution of acetone and deionized water, which is referred to as solution A.

[0007] Dissolve palmitoyl chloride in acetone, referred to as solution B;

[0008] Dissolve sodium hydroxide in deionized water, referred to as solution C;

[0009] Slowly add solution B and solution C to solution A, stir for 12h-13h, adjust the pH of the solution to 0.9-1.1, and continue stirring for 4h-4.5h; filter and dry the product, put the obtained white product in a beaker, add petroleum ether, and heat to 90℃-95℃ until the white product gradually dissolves. Stop heating when the white product reprecipitates as the petroleum ether evaporates, and then cool naturally to room temperature to obtain a purified template, which is recorded as AS;

[0010] The volume ratio of petroleum ether to acetone in solution A is 2:3;

[0011] When preparing solution A, the mass ratio of sodium hydroxide to phenylglycine is 1:(3.5-4), the volume ratio of acetone to deionized water is 1:(3-3.5), and the mass ratio of sodium hydroxide to the volume ratio of acetone is 1g:(54mL-55mL);

[0012] When preparing solution B, the volume ratio of palmitoyl chloride to acetone is 1:(7.5-8);

[0013] When preparing solution C, the mass ratio of the sodium hydroxide to the volume of deionized water is 1g:(160mL-165mL);

[0014] The mass of sodium hydroxide in solution A and solution C is the same;

[0015] The mass ratio of sodium hydroxide in solution A to the volume ratio of palmitoyl chloride in solution B is 1g:(6.5mL~7mL);

[0016] 2. Dissolve the AS and 3-aminophenol prepared in step 1 in methanol, stir well to obtain a transparent solution D;

[0017] The mass ratio of AS to 3-aminophenol is (0.01-0.1):(0.0199-1.9999);

[0018] The mass of AS and the volume ratio of methanol are 1g:(225mL-230mL);

[0019] 3. Add acetate to the transparent solution D prepared in step 2, stir thoroughly, then add deionized water, and continue stirring for 40 min to 45 min to obtain solution E;

[0020] The mass ratio of the acetate to the 3-aminophenol in step 2 is 1:(0.4-9.1);

[0021] The mass of the acetate and the volume ratio of deionized water is 1g:(124mL-2820mL);

[0022] 4. Slowly add the formaldehyde aqueous solution to the solution E prepared in step 3, heat to 62°C to 63°C and continue stirring for 3h to 3.5h, cool naturally to room temperature, and then filter and dry in sequence to obtain a yellow precursor;

[0023] The mass concentration of the formaldehyde aqueous solution is 37% to 40%, and the volume ratio of the formaldehyde aqueous solution to the deionized water added in step 3 is 1:(305 to 315);

[0024] 5. The yellow precursor prepared in step 4 is calcined under protective gas at 600° C. to 900° C. for 2 h to 3 h, and then naturally cooled to room temperature to obtain a metal / nitrogen-doped spiral nanocarbon absorbing material.

[0025] The present invention prepares a high-performance metal / nitrogen (M / N) doped spiral nanocarbon absorber (M / N-HCNT) by introducing a unique MNC configuration on a spiral carbon nanotube matrix with special cross-polarization. The orbital coupling between the 3d orbital of the metal and the 2p orbital of N causes the local charge to rearrange, enhancing the polarization loss, while converting the electromagnetic wave into electrical energy, which is dissipated in the form of heat, increasing the conductive loss. The unique spin polarization property gives the material additional electromagnetic loss, significantly improving the electromagnetic wave absorption performance. The spiral structure can significantly increase the multiple reflections and scattering of electromagnetic waves, and the induced cross polarization can form electromagnetic coupling, thereby showing excellent electromagnetic attenuation characteristics.

[0026] The M / N-HCNT absorbing material prepared by the present invention has better dielectric and magnetic properties than a single carbon material, so that the material can be used in a variety of scenarios. At the same time, the CST electromagnetic field simulation software simulates and verifies that the material has low RCS characteristics. The material is designed as a metamaterial, achieving ultra-wideband absorption of 12.16GHz, covering 67.5% (2-18GHz) of the full frequency band, and can meet the application of special environments such as military equipment, electronic devices, and protective clothing. In particular, it is expected to replace traditional absorbing materials in stealth aircraft. At the same time, the preparation method of the present invention is simple and low in cost, and can achieve ultra-wideband absorption at a lower filling ratio and a thinner thickness, so it has great industrial production application and promotion value.

[0027] Beneficial effects of the present invention:

[0028] 1. Unique preparation method: The present invention uses the template method to prepare the helical carbon nanotube precursor (the product of step 4), introduces metal particles in situ, and calcines to prepare high-performance metal / nitrogen-doped nanocarbon absorbing materials. Through electromagnetic simulation and density functional theory calculations, it is found that due to the unique atomic configuration of MNC and the special geometric configuration of the helical structure, spin polarization, orbital coupling and cross polarization are induced, and the three synergistically enhance electromagnetic attenuation;

[0029] 2. Excellent electromagnetic wave absorption ability: The method for preparing the metal / nitrogen-doped spiral nanocarbon absorbing material of the present invention is to precisely control the electromagnetic parameters by changing the type of metal (acetate), the ratio of metal and nitrogen source (3-aminophenol) and the temperature and time of sample heat treatment (step five), thereby improving impedance matching and achieving a synergistic effect of electromagnetic loss, thereby obtaining ideal electromagnetic wave absorption performance. The obtained composite absorbing material, after being mixed with paraffin, exhibits excellent lightweight microwave absorption performance at a relatively low coating thickness, achieving an ultra-strong absorption of -63.13 dB at an ultra-thin thickness of 1.29 mm, and achieving a broadband absorption of 6.08 GHz at a thickness of 1.83 mm;

[0030] 3. Applicability in multiple scenarios: The present invention can achieve more than 90% wave absorption efficiency in the full frequency band through electromagnetic synergy; CST electromagnetic field simulation software simulates and analyzes that the maximum reduction value of radar stealth performance at 0° is 36.4dB·m 2 , which means that the obtained material has excellent radar wave attenuation characteristics, can suppress the reflection of electromagnetic waves from the PEC surface, and has broad application prospects in the military field. Through the construction of metamaterials, ultra-wideband absorption of 12.16GHz is achieved at a thickness of 5mm, which can meet most practical application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the X-ray diffraction pattern of the product obtained in step 5 of Experiments 1 to 5;

[0032] Figure 2 Scanning electron micrograph of HMC-8 prepared for Experiment 1;

[0033] Figure 3 Scanning electron micrograph of SHMC-8 prepared for Experiment 2;

[0034] Figure 4 This is a scanning electron micrograph of SMC-8 prepared in Experiment 3;

[0035] Figure 5Scanning electron micrograph of LHMC-8 prepared for Experiment 4;

[0036] Figure 6 Scanning electron micrograph of LMC-8 prepared for Experiment 5;

[0037] Figure 7 The electromagnetic reflection loss data of HMC-8 calculated by step six of experiment one;

[0038] Figure 8 This is the electromagnetic reflection loss data of SHMC-8 calculated by step six of test two;

[0039] Fig. 9 This is the electromagnetic reflection loss data of SMC-8 calculated by step six of test three;

[0040] Fig.10 This is the electromagnetic reflection loss data of LHMC-8 calculated by step six of test four;

[0041] Fig.11 This is the electromagnetic reflection loss data of LMC-8 calculated by step 6 of test 5;

[0042] Fig.12 The effective absorption bandwidth diagram of HMC-8 prepared for Experiment 1;

[0043] Fig.13 A diagram of the simulation results of the electromagnetic metamaterial constructed for Experiment 7;

[0044] Fig.14 Calculation diagram of the voltage standing wave ratio of the gradient metamaterial constructed for experiment seven;

[0045] Fig.15 This is a schematic diagram of RCS calculation;

[0046] Fig.16 This is the RCS reduction value diagram for step 7 of test 2;

[0047] Fig.17 The RCS calculation results of step 7 of test 2 are shown in Figure 2. Figure 3 Vittu;

[0048] Fig.18 Structural radar diagram for RCS calculation in step seven of test two;

[0049] Fig.19 This is the structural radar diagram for the RCS calculation of step seven of test one;

[0050] Fig. 20 Structural radar diagram for the RCS calculation of step seven of experiment three. DETAILED DESCRIPTION

[0051] Specific implementation method 1: This implementation method is a method for preparing a metal / nitrogen-doped spiral nanocarbon absorbing material, which is specifically carried out in the following steps:

[0052] 1. Dissolve phenylglycine and sodium hydroxide together in a mixed solution of acetone and deionized water, which is referred to as solution A.

[0053] Dissolve palmitoyl chloride in acetone, referred to as solution B;

[0054] Dissolve sodium hydroxide in deionized water, referred to as solution C;

[0055] Slowly add solution B and solution C to solution A, stir for 12h-13h, adjust the pH of the solution to 0.9-1.1, and continue stirring for 4h-4.5h; filter and dry the product, put the obtained white product in a beaker, add petroleum ether, and heat to 90℃-95℃ until the white product gradually dissolves. Stop heating when the white product reprecipitates as the petroleum ether evaporates, and then cool naturally to room temperature to obtain a purified template, which is recorded as AS;

[0056] The volume ratio of petroleum ether to acetone in solution A is 2:3;

[0057] When preparing solution A, the mass ratio of sodium hydroxide to phenylglycine is 1:(3.5-4), the volume ratio of acetone to deionized water is 1:(3-3.5), and the mass ratio of sodium hydroxide to the volume ratio of acetone is 1g:(54mL-55mL);

[0058] When preparing solution B, the volume ratio of palmitoyl chloride to acetone is 1:(7.5-8);

[0059] When preparing solution C, the mass ratio of the sodium hydroxide to the volume of deionized water is 1g:(160mL-165mL);

[0060] The mass of sodium hydroxide in solution A and solution C is the same;

[0061] The mass ratio of sodium hydroxide in solution A to the volume ratio of palmitoyl chloride in solution B is 1g:(6.5mL~7mL);

[0062] 2. Dissolve the AS and 3-aminophenol prepared in step 1 in methanol, stir well to obtain a transparent solution D;

[0063] The mass ratio of AS to 3-aminophenol is (0.01-0.1):(0.0199-1.9999);

[0064] The mass of AS and the volume ratio of methanol are 1g:(225mL-230mL);

[0065] 3. Add acetate to the transparent solution D prepared in step 2, stir thoroughly, then add deionized water, and continue stirring for 40 min to 45 min to obtain solution E;

[0066] The mass ratio of the acetate to the 3-aminophenol in step 2 is 1:(0.4-9.1);

[0067] The mass of the acetate and the volume ratio of deionized water is 1g:(124mL-2820mL);

[0068] 4. Slowly add the formaldehyde aqueous solution to the solution E prepared in step 3, heat to 62°C to 63°C and continue stirring for 3h to 3.5h, cool naturally to room temperature, and then filter and dry in sequence to obtain a yellow precursor;

[0069] The mass concentration of the formaldehyde aqueous solution is 37% to 40%, and the volume ratio of the formaldehyde aqueous solution to the deionized water added in step 3 is 1:(305 to 315);

[0070] 5. The yellow precursor prepared in step 4 is calcined under protective gas at 600° C. to 900° C. for 2 to 3 hours, and then naturally cooled to room temperature to obtain a metal / nitrogen-doped helical nanocarbon absorbing material M / N-HCNT.

[0071] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the pH of the solution is adjusted in step 1 by adding hydrochloric acid solution. The rest is the same as specific embodiment 1.

[0072] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the acetate in step 3 is manganese acetate, cobalt acetate or nickel acetate. The rest is the same as specific implementation method 1 or 2.

[0073] Specific embodiment 4: This embodiment is different from the first to third embodiments in that the drying in step 4 is performed at 60° C. for 12 hours. The rest is the same as the first to third embodiments.

[0074] Specific implementation mode 5: This implementation mode is different from specific implementation mode 4 in that the protective gas in step 5 is argon or nitrogen. The rest is the same as specific implementation mode 4.

[0075] The present invention is verified by the following tests:

[0076] Experiment 1: This experiment is a method for preparing a metal / nitrogen-doped spiral nanocarbon absorbing material, which is specifically carried out in the following steps:

[0077] 1. Dissolve 2.0709 g of phenylglycine and 0.55 g of sodium hydroxide in a mixed solution of 30 mL of acetone and 90 mL of deionized water, referred to as solution A.

[0078] Dissolve 3.8 mL of palmitoyl chloride in 30 mL of acetone, referred to as solution B;

[0079] Dissolve 0.55 g of sodium hydroxide in 90 mL of deionized water, referred to as solution C;

[0080] Solution B and solution C were slowly added dropwise to solution A, stirred for 12 h, hydrochloric acid was added to adjust the pH to 1, and stirred for another 4 h. The white product was filtered and dried. The obtained white product was placed in a beaker, 20 mL of petroleum ether was added, and heated to 90°C. The white product gradually dissolved. When the white product reprecipitated as the petroleum ether evaporated, the heating was stopped, and the mixture was naturally cooled to room temperature to obtain the purified template, which was recorded as AS.

[0081] 2. Dissolve 0.035 g AS and 0.1997 g 3-aminophenol in 8 mL methanol and stir well to obtain a transparent solution D.

[0082] 3: Add 0.022 g of manganese acetate to the transparent solution D, stir thoroughly, add 62 mL of deionized water, stir for 40 min, and obtain solution E.

[0083] Fourth: slowly drop 200 μL of formaldehyde aqueous solution into solution E, heat to 62°C and continue stirring for 3 hours, cool naturally to room temperature, filter, and dry at 60°C for 12 hours to obtain a yellow precursor; the mass concentration of the formaldehyde aqueous solution is 37% to 40%;

[0084] 5. Under argon protection, the yellow precursor was calcined at 800°C for 2h and then naturally cooled to room temperature to obtain HMC-8; the heating rate was 5°C / min;

[0085] Six: The prepared HMC-8 absorbing material was immersed in melted paraffin as a substrate (the mass ratio of HMC-8 to paraffin was 3:7) to form a ring, in which HMC-8 accounted for 30wt.% of the total mass of the ring. The electromagnetic parameters of HMC-8 were measured by a vector network analyzer. According to the transmission line theory, the reflection loss of the material to the electromagnetic wave was calculated by the following equation:

[0086]

[0087] 7: Use CST electromagnetic field simulation software to simulate the radar stealth performance of HMC-8, and the reduction of its radar cross-sectional area is calculated by the following formula:

[0088]

[0089] Experiment 2: The difference between this experiment and Experiment 1 is that the mass of 3-aminophenol described in step 2 is 0.0999 g;

[0090] The product obtained in step 5 is SHMC-8. Other steps are the same as those in experiment 1.

[0091] Experiment 3: The difference between this experiment and Experiment 1 is that the mass of 3-aminophenol described in step 2 is 0.0499 g;

[0092] The product obtained in step 5 is SMC-8. The rest is the same as in experiment 1.

[0093] Experiment 4: The difference between this experiment and Experiment 1 is that the mass of manganese acetate in step 3 is 0.11 g, and the product obtained in step 5 is LHMC-8. The rest is the same as Experiment 1.

[0094] Experiment 5: The difference between this experiment and Experiment 1 is that the mass of manganese acetate in step 3 is 0.22 g, and the product obtained in step 5 is LMC-8. Others are the same as Experiment 1.

[0095] Experiment 6: The difference between this experiment and Experiment 1 is that the calcination temperature in step 5 is 700°C and the product obtained in step 5 is HMC-7. The rest is the same as Experiment 1.

[0096] Experiment seven: Construct an electromagnetic metamaterial based on HMC-7, the product of Experiment six: import the electromagnetic parameters of HMC-7 obtained by the vector network analyzer into the CST electromagnetic field simulation software, set the frequency to 2-18 GHz, set the boundary to a periodic boundary, and construct a three-layer gradient metamaterial. The side length and height of the bottom layer are 15 mm × 1 mm, the side length and height of the second layer are 13 mm × 2 mm, and the side length and height of the third layer are 11 mm × 2 mm.

[0097] Figure 1 The X-ray diffraction patterns of the products obtained in step 5 of experiments 1 to 5 are shown in Figure 1. The peaks at 34.9°, 40.5°, 58.7°, 70.2° and 73.8° observed for SMC-8 prepared in experiment 3 can be attributed to the (111), (200), (220), (311) and (222) crystal planes of MnO. The two broad characteristic peaks observed at about 23.5° and 43.8° for the other four groups of samples correspond to the (002) and (100) crystal planes of graphitized carbon, indicating that the prepared manganese / nitrogen-doped nanocarbon material products are stable and conducive to industrial production and promotion.

[0098] Figure 2 This is a scanning electron micrograph of HMC-8 prepared in Experiment 1. An obvious helical structure can be seen in the image.

[0099] Figure 3 This is a scanning electron micrograph of SHMC-8 prepared for Experiment 2. From the image, it can be seen that the helical structure and the spherical structure coexist, and the diameter of the sphere is about 171nm.

[0100] Figure 4 This is a scanning electron microscope image of SMC-8 prepared for experiment three. From the image, we can see that it is all spherical structures, and the diameter of the spheres is about 171nm.

[0101] Figure 5 Scanning electron microscope image of LHMC-8 prepared for experiment 4. From the image, it can be seen that the spiral structure coexists with the large spherical structure, and the diameter of the large sphere is about 299nm.

[0102] Figure 6 Scanning electron microscope image of LMC-8 prepared for experiment 5. From the image, we can see that they are all large spherical structures, and the diameter of the large spheres is about 299nm.

[0103] Figure 7 This is the electromagnetic reflection loss data of HMC-8 calculated by step six of experiment one. Figure 8 This is the electromagnetic reflection loss data of SHMC-8 calculated by step 6 of test 2. Fig. 9 This is the electromagnetic reflection loss data of SMC-8 calculated by step six of test three. Fig.10 This is the electromagnetic reflection loss data of LHMC-8 calculated by step 6 of test 4. Fig.11 This is the electromagnetic reflection loss data graph of LMC-8 calculated through step six of experiment five. It can be seen that when the mass filling ratio is 30%, the minimum reflection losses of HMC-8, SHMC-8, SMC-8, LHMC-8 and LMC-8 can reach -63.13dB, -26.4dB, -42.49dB, -52.43dB and -42.92dB respectively, and the matching thicknesses are 1.29mm, 1.34mm, 4.98mm, 1.67mm and 5mm respectively, all showing excellent absorbing performance.

[0104] Fig.12 This is the effective absorption bandwidth diagram of HMC-8 prepared for experiment 1. It can be seen that the effective absorption bandwidth of HMC-8 reaches an ultra-wideband absorption of 5.12 GHz when the thickness is 1.83 mm.

[0105] Fig.13 This is the simulation result of the electromagnetic metamaterial constructed in experiment seven. The metamaterial showed excellent electromagnetic wave absorption performance, exceeding 67% of the full frequency band and achieving ultra-wideband absorption of 12.16 GHz, showing potential for practical applications and prospects for military applications.

[0106] Fig.14 The voltage standing wave ratio calculation diagram of the gradient metamaterial constructed for experiment 7. The closer the voltage standing wave ratio is to 1, the better the impedance of the material. The voltage standing wave ratio of the gradient metamaterial is significantly better than that of the bulk material, showing the excellent impedance characteristics of the gradient metamaterial.

[0107] Fig.15 This is the RCS calculation diagram. Fig.16 This is the RCS reduction value diagram for step 7 of test 2. Fig.17 The RCS calculation results of step 7 of test 2 are shown in Figure 2. Figure 3 Vitu, Fig.18 This is the radar diagram of the RCS calculation structure in step 7 of test 2. It can be seen that at an angle of 0°, the RCS reduction value is greater than 30dB·m 2 , where the maximum RCS reduction value of SHMC-8 is 36.4dB·m 2 , demonstrating the excellent radar stealth performance of SHMC-8.

[0108] Fig.19 This is the radar diagram of the RCS calculation structure in step 7 of test 1. It can be seen that the maximum RCS reduction value is 35.19dB·m 2 .

[0109] Fig. 20 This is the radar diagram of the RCS calculation structure in step 7 of test 3. It can be seen that the maximum RCS reduction value is 32.04dB·m 2 .

Claims

1. A method for preparing a metal / nitrogen-doped helical nanocarbon absorbing material, characterized in that The preparation method of the metal / nitrogen doped helical nanocarbon absorbing material is carried out according to the following steps:

1. Dissolve phenylglycine and sodium hydroxide together in a mixed solution of acetone and deionized water, which is referred to as solution A. Dissolve palmitoyl chloride in acetone, referred to as solution B; Dissolve sodium hydroxide in deionized water, referred to as solution C; Slowly add solution B and solution C to solution A, stir for 12h-13h, adjust the pH of the solution to 0.9-1.1, and continue stirring for 4h-4.5h; filter and dry the product, put the obtained white product in a beaker, add petroleum ether, and heat to 90℃-95℃ until the white product gradually dissolves. Stop heating when the white product reprecipitates as the petroleum ether evaporates, and then cool naturally to room temperature to obtain a purified template, which is recorded as AS; The volume ratio of petroleum ether to acetone in solution A is 2:3; When preparing solution A, the mass ratio of sodium hydroxide to phenylglycine is 1:(3.5-4), the volume ratio of acetone to deionized water is 1:(3-3.5), and the mass ratio of sodium hydroxide to the volume ratio of acetone is 1g:(54mL-55mL); When preparing solution B, the volume ratio of palmitoyl chloride to acetone is 1:(7.5-8); When preparing solution C, the mass ratio of the sodium hydroxide to the volume of deionized water is 1g:(160mL-165mL); The mass of sodium hydroxide in solution A and solution C is the same; The mass ratio of sodium hydroxide in solution A to the volume ratio of palmitoyl chloride in solution B is 1g:(6.5mL~7mL); 2. Dissolve the AS and 3-aminophenol prepared in step 1 in methanol, stir well to obtain a transparent solution D; The mass ratio of AS to 3-aminophenol is (0.01-0.1):(0.0199-1.9999); The mass of AS and the volume ratio of methanol are 1g:(225mL-230mL); 3. Add acetate to the transparent solution D prepared in step 2, stir thoroughly, then add deionized water, and continue stirring for 40 min to 45 min to obtain solution E; The mass ratio of the acetate to the 3-aminophenol in step 2 is 1:(0.4-9.1); The mass of the acetate and the volume ratio of deionized water is 1g:(124mL-2820mL); 4. Slowly add the formaldehyde aqueous solution to the solution E prepared in step 3, heat to 62°C to 63°C and continue stirring for 3h to 3.5h, cool naturally to room temperature, and then filter and dry in sequence to obtain a yellow precursor; The mass concentration of the formaldehyde aqueous solution is 37% to 40%, and the volume ratio of the formaldehyde aqueous solution to the deionized water added in step 3 is 1:(305 to 315); 5. The yellow precursor prepared in step 4 is calcined under protective gas at 600° C. to 900° C. for 2 to 3 hours, and then naturally cooled to room temperature to obtain a metal / nitrogen-doped helical nanocarbon absorbing material M / N-HCNT.

2. The method for preparing a metal / nitrogen-doped helical nanocarbon absorbing material according to claim 1, characterized in that In step 1, the pH of the solution is adjusted by adding hydrochloric acid solution.

3. The method for preparing a metal / nitrogen-doped helical nanocarbon absorbing material according to claim 1, characterized in that The acetate described in step 3 is manganese acetate, cobalt acetate or nickel acetate.

4. The method for preparing a metal / nitrogen-doped helical nanocarbon absorbing material according to claim 1, characterized in that The drying described in step 4 is drying at 60° C. for 12 h.

5. The method for preparing a metal / nitrogen-doped helical nanocarbon absorbing material according to claim 1, characterized in that The protective gas described in step 5 is argon or nitrogen.

Citation Information

Patent Citations

  • Method for preparing single-handed helical carbon nano tube

    CN104030271A

  • HOF-derived one-dimensional Ni-doped magnetic carbon-based nanocomposite and preparation method thereof

    CN115915738A

  • Preparation method of multifunctional nitrogen-doped carbon aerogel

    CN115920790A