High-valued treatment method of waste concrete recycled micro powder
Patent Information
- Application Number
- CN202410780390.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
Waste concrete recycled micron powder is difficult to process and the cost of capturing and solidifying carbon dioxide in cement industry exhaust is high, and carbon dioxide emissions pose a threat to the environment.
Using rapid wet carbonization technology and high value-added reuse of solid waste, through the phase separation of carbonized waste concrete regenerated micro-powder and the preparation technology of nano-silica and ultra-fine calcium carbonate, the hydration product reacts with carbon dioxide to generate calcium carbonate and Silica gel for carbon dioxide capture and storage.
It realizes the high-value treatment of waste concrete recycled micro-powder, reduces the cost of carbon dioxide capture and solidification, and is expected to realize the recycling and recovery of carbon dioxide throughout the life cycle, which has extensive economic and ecological value.
Smart Images

Figure CN118754185A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high value-added utilization of construction solid waste, and specifically relates to a method for high-value treatment of waste concrete recycled micropowder. Background Art
[0002] Concrete is the most consumed man-made material in the world due to its low cost, good mechanical strength and excellent structural performance. Nowadays, with the renewal of cities and the development of new infrastructure and housing, a large amount of construction and demolition waste is generated, including a large amount of waste concrete. The production of concrete consumes about 5 billion tons of cement each year and produces about 7% of global carbon dioxide emissions. In addition, it is not uncommon to demolish old concrete due to aging, change of use and other reasons. Waste concrete is one of the most important components of construction and demolition waste. It can be crushed and processed into recycled concrete aggregate, but the treatment of recycled concrete fine powder (RCF) is still a major problem. In addition, a large amount of CO2 is also produced in the tail gas of the cement industry, which is difficult to solidify and further utilize. With the intensification of global warming, CO2 is the main component of greenhouse gases, and reducing CO2 emissions needs to be paid more and more attention. Summary of the invention
[0003] The present invention develops a method for high-value treatment of waste concrete recycled micropowder, proposes a technical idea of rapid wet carbonization technology and high-value-added recycling of solid waste, and designs and develops preparation technology of nano-silicon dioxide and ultrafine calcium carbonate. After wet carbonization of waste concrete recycled micropowder, a large amount of hydration products and unhydrated particles can react with carbon dioxide to regenerate calcium carbonate, silica gel, etc., which can be used as excellent materials for carbon dioxide capture and storage, solving the current problem of high cost of carbon dioxide capture and solidification of cement industry tail gas, and is expected to realize circulation and recovery of carbon dioxide over its entire life cycle, which has broad economic and ecological value.
[0004] In order to achieve the above technical objectives, the present invention is implemented through the following technical solutions: a method for high-value treatment of waste concrete recycled micropowder, comprising:
[0005] By utilizing the phase separation technology of recycled micropowder from carbonized waste concrete and the preparation technology of nano-silicon dioxide, the calcium and silicon materials in the carbonization product are separated by the sodium hydroxide dissolution method, and the silicon element in the carbonized recycled micropowder is recovered. In addition, the preparation technology of ultrafine calcium carbonate and nano-silicon dioxide is developed to achieve high-value processing of recycled micropowder from waste concrete.
[0006] Furthermore, the preparation technology of ultrafine calcium carbonate comprises the following steps: first, adding waste concrete recycled micropowder and deionized water at a certain solid-liquid ratio into a reactor A, and introducing ammonium nitrate at the same time, and mechanically stirring at a certain speed at room temperature until no bubbles appear in the raw material liquid in the reactor; after the reaction is completed, filtering through a suction filter, the mother liquor in the reactor A is passed to the reactor B, 99.99% commercial carbon dioxide is injected into the reactor B at a certain flow rate, and ammonia water is introduced at the same time to induce its carbonation, and after a period of carbonation reaction, the suspended solid particles in the solution are collected by the suction filter, the main component of which is calcium carbonate-rich residue, and then the solid particles are placed in a vacuum dryer for drying, and then collected after mechanical grinding; the main carbonization reaction of the silicate phase of cement hydration in the waste concrete recycled micropowder is described by formulas (1), (2), and (3).
[0007] RCF+NH4Cl→CaCl2+Si-rich(residue)+NH3·H2O+NH3 (1)
[0008] CaCl2+2 NH3·H2O+CO2→(NH4)2CO3+CaCl2+H2O (2)
[0009] (NH4)2CO3+CaCl2→CaCO3+NH4Cl (3)
[0010] Furthermore, the preparation technology of nano silicon dioxide comprises the following steps: the hydration products and unhydrated clinker C2S and C4AF in the original waste concrete regeneration micro powder are almost completely consumed after wet carbonization, and formulas (4) and (5) are the carbonization reaction formulas of clinker C2S and C4AF; the filter cake filtered by reactor A and reactor B is passed into reactor C, soaked with sodium hydroxide as a solvent, and dissolved under certain temperature and stirring speed conditions, and the sodium hydroxide reacts with the formed amorphous gel such as alumina gel and silica gel to form aqueous phase Na2SiO3 and NaAlO2, which can be expressed by formula (6); the solution obtained from reactor C is filtered through a suction filter, and the filter cake calcium carbonate is collected again, and the collected filtrate is flowed into reactor D for carbonation; the same 99.99% commercial Carbon dioxide is injected into the reaction kettle D to precipitate sodium aluminosilicate gel and silica gel; less amorphous silica gel is formed within 20 minutes before carbonation, but silica gel with a high degree of polymerization is rapidly formed between 20 minutes and 60 minutes, so the carbonation time is selected to be less than 60 minutes to ensure the formation of amorphous silica gel; during the carbonation process, the solution is stirred at a certain speed at room temperature; the amorphous silica gel can be extracted and collected by adjusting the flow rate of 99.99% commercial carbon dioxide to control its alkalinity, as shown in formula (7), and then the precipitate in the solution is collected after filtering with a suction filter; finally, the gel precipitate is washed with a diluted hydrochloric acid solution and deionized water to remove aluminum impurities, as shown in formula (8), to obtain a high-polymer amorphous silica gel with a purity of 98.8%, and then dried and collected to obtain nano-silicon dioxide.
[0011] C2S+2CO2→2CaCO3+SiO2(gel) (4)
[0012] C4AF+4CO2+3H2O→4CaCO3+SiO2(gel)+Al(OH)3(gel)+Fe(OH)3(gel) (5)
[0013] SiO2(gel)+3NaOH+Al(OH)3(gel)→Na2SiO3+NaAlO2+3 H2O (6)
[0014] 2Na2SiO3+2Na2AlO3+4CO2+2H2O→4NaHCO3+Na2SiAl2O5(gel)+SiO2(gel) (7)
[0015] Na2SiAl2O5(gel)+8HCl→2NaCl+2AlCl3+4H2O+SiO2(gel) (8)
[0016] Beneficial effects of the present invention:
[0017] The invention solves the problem of the difficulty in treating recycled micropowder of waste concrete by developing a high-value treatment method for recycled micropowder of waste concrete, proposes a rapid wet carbonization technology and a technical idea for high-value-added recycling of solid waste, and designs and develops a preparation technology of nano-silicon dioxide and ultrafine calcium carbonate, thereby enabling the recycled micropowder of waste concrete to be treated in a high-value manner and solving the current problem of high cost of capturing and solidifying carbon dioxide in cement industry tail gas. It is expected that carbon dioxide can be recycled and recovered over its entire life cycle. The invention has broad economic and ecological value. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments.
[0019] Figure 1 It is a reaction flow chart of Example 1 of the present invention. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. In addition, the technical features involved in the various embodiments described below can be combined with each other as long as they do not conflict with each other.
[0021] Example 1
[0022] See also Figure 1 As shown, a method for high-value treatment of waste concrete recycled micropowder is proposed, comprising the following steps:
[0023] In order to treat the recycled micropowder of waste concrete, we develop the phase separation technology of carbonized recycled micropowder of waste concrete and the preparation technology of nano-silicon dioxide. We use the sodium hydroxide dissolution method to separate the calcium and siliceous materials in the carbonization product and recover the silicon element in the carbonized recycled micropowder. In addition, we develop the preparation technology of ultrafine calcium carbonate and nano-silicon dioxide to achieve high-value treatment of recycled micropowder of waste concrete.
[0024] The preparation technology of ultrafine calcium carbonate includes the following steps: first, waste concrete recycled micropowder and deionized water are added into reactor A at a solid-liquid ratio of 1:10. Reactor A is equipped with a heat-insulating heating jacket, a volume of 100L, normal pressure operation, a material of 304 stainless steel, a jacket pressure bearing of 0.6MPa, a vortex propulsion agitator, a speed of 0-200rpm / min, and a matching variable frequency stirring motor. Reactor A contains a heating circulator, and the heating method is hot water circulation heating. The temperature is controlled at room temperature to 100°C, the water medium, the heating power: 8KW, the temperature control accuracy is ±1°C, and the head: 15m. At the same time, ammonium nitrate is introduced into reactor A at 50L / min, and the agitator in the reactor is set to stir at a speed of 200rpm / min until no bubbles appear. The reaction nodes are controlled to be automated, and the reaction temperature and time are adjusted to 85°C and 2h, until no bubbles appear in the raw material liquid in the kettle. The unreacted solution enters reactor A through the circulation pump. The circulation pump can realize variable frequency speed control with a flow rate of 20L / min. The solution stirred completely in reactor A is filtered through a suction filter, and the mother liquor goes to reactor B, and the filter cake goes to reactor A / reactor C. The volume of reactor B is 100L, it works at normal pressure, and is made of 304 stainless steel. The motor is a vortex propulsion agitator with a speed of 0-200rpm / min and a variable frequency stirring motor. The only difference from reactor A is that the former reactor has no heating and insulation jacket, while the latter has a jacket. After the liquid flows to reactor B, 99.99% commercial carbon dioxide is injected into reactor B at a flow rate of 0.2L / min, and ammonia water is introduced to induce carbonation. The stirrer in reactor B is set to stir at a speed of 200rpm / min, and the stirring time does not exceed 1h. The reaction node is controlled to achieve automation, and the reaction pH is adjusted to 7.5. After a period of carbonation reaction, the mother liquid is filtered through a suction filter and then sent to reactor A for wet carbonation reaction again. The suspended solid particles in the solution are collected by the suction filter, and the main component is calcium carbonate-rich residue. The solid particles are then placed in a vacuum dryer for drying, and then collected after mechanical grinding to obtain ultrafine calcium carbonate-rich materials. The main carbonization reaction of the cement hydrate silicate phase in the recycled micropowder of waste concrete can be described by formulas (1), (2), and (3).
[0025] RCF+NH4Cl→CaCl2+Si-rich(residue)+NH3·H2O+NH3 (1)
[0026] CaCl2+2 NH3·H2O+CO2→(NH4)2CO3+CaCl2+H2O (2)
[0027] (NH4)2CO3+CaCl2→CaCO3+NH4Cl (3)
[0028] The preparation technology of nano silicon dioxide comprises the following steps: the hydration products and unhydrated clinker C2S and C4AF in the original waste concrete recycled micro powder are almost completely consumed after wet carbonization, and the carbonization reaction of the clinker C2S and C4AF can be expressed by formulas (4) and (5); the filter cake filtered by reactor A and reactor B is passed into reactor C, the volume of reactor C is 200L, it works at normal pressure, it is made of 304 stainless steel, the motor is a vortex propulsion agitator, the speed is 0-200rpm / min, it is equipped with a variable frequency stirring motor, sodium hydroxide is used as a solvent for soaking, the flow rate of the metering pump of the sodium hydroxide solution is 50L / min, and stirring is performed at a stirring speed of 200r / min. The reaction node is controlled to be automated, and the reaction time is adjusted to 2h for dissolution. Sodium hydroxide reacts with the formed amorphous gels such as alumina gel and silica gel to form aqueous phase Na2SiO3 and NaAlO2, which can be expressed by formula (6). The solution obtained from reactor C is filtered through a suction filter, and the filter cake calcium carbonate is collected again. The mother liquor of reactor C that has not reacted completely flows back into reactor C through a circulation pump for alkali dissolution treatment; the circulation pump can realize variable frequency speed regulation control with a flow rate of 20L / min, and the collected filtrate flows into reactor D for carbonation. Reactor D has a volume of 200L, works at normal pressure, is made of 304 stainless steel, and has a vortex propulsion agitator with a rotation speed of 0-200rpm / min. It is equipped with a variable frequency stirring motor and performs stirring reaction at a stirring speed of 200r / min. The reaction node is controlled to be automated, and the reaction pH is adjusted to 10.5, 1h, and the stirring speed is 0.2L / min. 99.99% commercial carbon dioxide is injected into the reactor D at a flow rate to precipitate sodium aluminosilicate gel and silica gel; less amorphous silica gel is formed within 20 minutes before carbonation, but silica gel with a high degree of polymerization is rapidly formed between 20 minutes and 60 minutes, so the carbonation time is selected to be less than 60 minutes to ensure the formation of amorphous silica gel; during the carbonation process, the solution is stirred at a certain speed at room temperature; the amorphous silica gel can be extracted and collected by adjusting the flow rate of 99.99% commercial carbon dioxide to control its alkalinity, as shown in formula (7), and then the precipitate in the solution is collected after filtering with a suction filter; finally, the gel precipitate is washed with a diluted hydrochloric acid solution and deionized water to remove aluminum impurities, and the flow rate of the metering pump of the hydrochloric acid HCl flow rate is adjusted to 50L / min, as shown in formula (8), to obtain a high-polymer amorphous silica gel with a purity of 98.8%, and then dried and collected to obtain nano-silica.
[0029] C2S+2CO2→2CaCO3+SiO2(gel) (4)
[0030] C4AF+4CO2+3H2O→4CaCO3+SiO2(gel)+Al(OH)3(gel)+Fe(OH)3(gel) (5)
[0031] SiO2(gel)+3NaOH+Al(OH)3(gel)→Na2SiO3+NaAlO2+3 H2O (6)
[0032] 2Na2SiO3+2Na2AlO3+4CO2+2H2O→4NaHCO3+Na2SiAl2O5(gel)+SiO2(gel) (7)
[0034] Na2SiAl2O5(gel)+8HCl→2NaCl+2AlCl3+4H2O+SiO2(gel) (8)
[0035] The process equipment used in the above process is shown in Table 1.
[0036] Table 1 Process auxiliary equipment
[0037]
[0038]
[0039] During the whole treatment process, reactor A, reactor B, reactor C, and reactor D will all generate some waste gas. In this embodiment, a water ring vacuum pump is used to remove the waste gas generated during the reaction process. Considering that there are only carbon dioxide and ammonia, they can be collected and then dissolved in water. The ammonia waste gas generated by reactor A is collected and passed into the ammonia raw material tank of reactor B for water dissolution and recycling.
[0040] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific embodiments described. Obviously, many modifications and changes can be made according to the content of this specification.
Claims
1. A method for high-value treatment of waste concrete recycled micropowder, characterized by: Carbonized waste concrete recycled micropowder phase separation and nano-silicon dioxide preparation technology, use sodium hydroxide dissolution method technology to separate the calcium and silicon materials in the carbonization product, and recover the silicon element in the carbonized recycled micropowder. In addition, develop ultrafine calcium carbonate preparation technology and nano-silicon dioxide preparation technology to achieve high-value processing of waste concrete recycled micropowder.
2. The method for high-value treatment of recycled fine powder from waste concrete according to claim 1 is characterized by: The preparation steps of the ultrafine calcium carbonate include: adding waste concrete recycled micro powder and deionized water into a reactor A at a certain solid-liquid ratio, introducing ammonium nitrate at the same time, and mechanically stirring at a certain speed until no bubbles appear in the raw material liquid in the reactor; after the reaction is completed, filtering through a suction filter, passing the mother liquid in the reactor A to the reactor B, injecting carbon dioxide into the reactor B, and introducing ammonia water to induce carbonation, and after a period of carbonation reaction, collecting suspended solid particles in the solution through a suction filter, and then putting the solid particles into a vacuum dryer for drying, and then collecting them after mechanical grinding.
3. The method for high-value treatment of waste concrete recycled micropowder according to claim 1 is characterized by: The preparation steps of the nano silicon dioxide include: after wet carbonization, the filter cake filtered by the reactor A and the reactor B is passed into the reactor C, soaked with sodium hydroxide as a solvent, after dissolution reaction, the sodium hydroxide reacts with the formed amorphous gel such as alumina gel and silica gel to form aqueous phase Na2SiO3 and NaAlO2, the solution obtained by the reactor C is filtered by a suction filter, the filter cake calcium carbonate is collected again, and the collected filtrate is passed into the reactor D for carbonation; carbon dioxide is injected into the reactor D to precipitate sodium aluminosilicate gel and silica gel, the carbonation time is selected to be 20min to 60min, and during the carbonation process, the solution is stirred at a certain speed at room temperature; the amorphous silica gel is extracted and collected by adjusting the flow rate of carbon dioxide to control its alkalinity, and then the precipitate in the solution is collected after filtering by a suction filter; finally, the gel precipitate is washed with a diluted hydrochloric acid solution and deionized water to remove aluminum impurities to obtain a high-polymer amorphous silica gel with a purity of 98.8%, and then dried and collected.
Citation Information
Cited By
Adsorption and immobilization method for heavy metal ions in water and geopolymer cementing material
CN119841388A
Sandy soil improvement liquid combining microorganisms and waste concrete, preparation method and improvement method
CN119875650A
Microorganism and waste concrete sand soil improvement liquid, preparation method and improvement method
CN119875650B