Photocurable 3D printing silicon-based ceramic core paste, preparation method and application thereof

By using photopolymerization 3D printing technology and silicon-based ceramic core slurry with a specific composition, the problems of long manufacturing cycle and shrinkage deformation of ceramic cores have been solved, enabling high-precision and high-performance manufacturing of the inner cavity of high-temperature alloy blades.

CN118754707BActive Publication Date: 2026-11-20AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410736228.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2026-11-20
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

Existing technologies for manufacturing ceramic cores for aero-engine blades suffer from problems such as long mold design and manufacturing cycles and high costs. In addition, ceramic cores are prone to shrinkage and deformation at high temperatures, which affects the dimensional accuracy and physical properties of the blade's internal cavity.

Method used

Using photopolymerization 3D printing technology, a silicon-based ceramic core slurry containing quartz glass powder, nano-alumina, and acrylate photosensitive resin is used to prepare the silicon-based ceramic core through photopolymerization 3D printing, debinding, and sintering. Nano-alumina modifier is used to suppress shrinkage.

Benefits of technology

It significantly reduces the sintering and casting shrinkage of ceramic cores, improves mechanical strength at room temperature and high temperature, meets the casting requirements of high-temperature alloy blades, and ensures the dimensional accuracy and physical properties of the blade cavity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004881841960000111
    Figure BDA0004881841960000111
  • Figure BDA0004881841960000112
    Figure BDA0004881841960000112
  • Figure BDA0004881841960000121
    Figure BDA0004881841960000121
Patent Text Reader

Abstract

The present application relates to the technical field of additive manufacturing, and particularly relates to a light-cured 3D printing silicon-based ceramic core slurry, a preparation method and application thereof. The light-cured 3D printing silicon-based ceramic core slurry comprises: ceramic powder 55wt%-65wt%; acrylate photosensitive resin 32wt%-42wt%; dispersing agent 3wt%-5wt%; the sum of the amounts of the above components is 100%; the ceramic powder comprises: quartz glass powder 89wt%-98wt%; mineralizer 0.2wt%-10wt%; nano-alumina 0.1wt%-2wt%; the sum of the amounts of the above components in the ceramic powder is 100%. The light-cured 3D printing silicon-based ceramic core slurry uses nano-alumina as a modifier, can be well combined with other components, and the physical properties and use performance of the obtained light-cured 3D printing silicon-based ceramic core are relatively optimal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of additive manufacturing technology, and in particular to a photopolymerizable 3D printing silicon-based ceramic core slurry, its preparation method and application. Background Technology

[0002] The internal structure of blades used in aero-engines is a ceramic core, which must withstand various complex and harsh environments. Therefore, the ceramic core must have excellent performance in terms of size, strength and surface roughness.

[0003] However, with the continuous development of aero-engine technology, the technical requirements for high-temperature alloy turbine blades are constantly increasing, and the blade structure is becoming more complex. Ceramic cores, as the inner cavity of the blade, are usually manufactured using traditional hot-pressing molding methods. Cores have disadvantages such as long mold design and manufacturing cycles, and high costs. Photopolymer 3D printing technology utilizes the core model to form a three-dimensional solid layer by layer, which has advantages such as no need for molds and short production cycles.

[0004] Ceramic cores undergo sintering shrinkage during fabrication. For 3D-printed ceramic cores, the dimensions in the three-dimensional direction can be adjusted using a digital model, ultimately reducing the sintering shrinkage rate in these directions. However, the core also experiences varying degrees of casting shrinkage during directional solidification, a process that cannot be reduced by adjusting the digital model. The significant shrinkage deformation of the ceramic core during use ultimately affects the dimensional accuracy of the blade's internal cavity. Furthermore, during high-temperature casting, the ceramic core must withstand the impact and immersion in molten metal at 1500–1600°C, placing extremely high demands on its high-temperature strength, toughness, and chemical stability. Therefore, to achieve high dimensional accuracy and excellent performance in ceramic cores and blades, reducing the sintering / casting shrinkage rate and improving the physical properties and chemical stability during fabrication and service are pressing issues that need to be addressed. Summary of the Invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a photocurable 3D printing silicon-based ceramic core slurry, its preparation method and application. The photocurable 3D printing silicon-based ceramic core obtained by using the photocurable 3D printing silicon-based ceramic core slurry of the present invention has superior physical and performance properties.

[0006] This invention provides a photopolymerizable 3D printing silicon-based ceramic core slurry, comprising:

[0007] Ceramic powder 55wt%~65wt%;

[0008] Acrylic photosensitive resin 32wt%~42wt%;

[0009] Dispersant 3wt%~5wt%;

[0010] The sum of the amounts of the above components is 100%;

[0011] The ceramic powder includes:

[0012] Quartz glass powder 89wt%~98wt%;

[0013] Mineralizing agent 0.2wt%~10wt%;

[0014] Nano-alumina 0.1wt%~2wt%;

[0015] In the ceramic powder, the sum of the amounts of the above components is 100%.

[0016] Preferably, the median particle size of the quartz glass powder is 6–8 μm.

[0017] Preferably, the mineralizer is at least one of alumina powder, silicon carbide powder, zirconium silicate powder, zirconium oxide powder, mullite powder, cristobalite, metallic silicon powder, silicon micro powder, nano silicon powder, zirconium carbide, carbon black, carbon nanotubes, nano aluminum powder, aluminum powder, and graphene; the median particle size of the mineralizer is 0.05 to 40 μm.

[0018] Preferably, the median particle size of the nano-alumina is 30–50 nm.

[0019] Preferably, the acrylate photosensitive resin is an acrylate monomer and an acrylate oligomer;

[0020] In the acrylate photosensitive resin, the content of acrylate monomers is 55wt% to 65wt%, and the content of acrylate oligomers is 35wt% to 45wt%.

[0021] Preferably, the acrylate monomer is at least one selected from 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, trimethylolpropane triacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, hydroxyethyl methacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylate, dipentaerythritol hexaacrylate, isobornyl acrylate, isobornyl methacrylate, polyethylene glycol (200) diacrylate, and polyethylene glycol (400) diacrylate.

[0022] The acrylate oligomer is at least one of aliphatic polyurethane acrylate, aromatic polyurethane acrylate, and modified epoxy acrylate.

[0023] Preferably, the dispersant is at least one of Disperbyk-111, UV dispersant JZ-291, and BASK dispersant.

[0024] This invention also provides a method for preparing the photopolymerizable 3D printing silicon-based ceramic core slurry described above, comprising the following steps:

[0025] Ceramic powder, acrylate photosensitive resin and dispersant are mixed to obtain photocurable 3D printing silicon-based ceramic core slurry;

[0026] The ceramic powder is obtained by mixing quartz glass powder, mineralizer and nano alumina.

[0027] This invention also provides a method for molding the photopolymerizable 3D printing silicon-based ceramic core slurry described above, comprising the following steps:

[0028] A) Photopolymer 3D printing of silicon-based ceramic core slurry is performed to obtain a green body;

[0029] The process parameters for photopolymerization 3D printing include: a curing thickness of 75–100 μm and a curing power of 12–15 mW / cm². 2 The curing time for a single layer is 3 to 5 seconds;

[0030] B) The preform is degreased and sintered to obtain a photopolymerizable 3D printed silicon-based ceramic core.

[0031] The present invention also provides a photopolymerization 3D printing silicon-based ceramic core prepared by the molding method described above.

[0032] This invention provides a photocurable 3D printing silicon-based ceramic core slurry, comprising: 55wt%–65wt% ceramic powder; 32wt%–42wt% acrylate photosensitive resin; and 3wt%–5wt% dispersant; the sum of the above components is 100%; the ceramic powder comprises: 89wt%–98wt% quartz glass powder; 0.2wt%–10wt% mineralizer; and 0.1wt%–2wt% nano-alumina; the sum of the above components in the ceramic powder is 100%. The photocurable 3D printing silicon-based ceramic core slurry provided by this invention uses nano-alumina as a modifier, which can effectively cooperate with other components to significantly suppress the shrinkage rate of the silicon-based ceramic core. The photocurable 3D printing silicon-based ceramic cores obtained using the photocurable 3D printing silicon-based ceramic core slurry of this invention exhibit superior physical and performance properties.

[0033] Experimental results show that the silicon-based ceramic core obtained by photopolymerization 3D printing using the silicon-based ceramic core slurry of this invention has an apparent porosity of 29.18%–34.53%, a water absorption rate of 18.24%–23.56%, and a bulk density of 1.49–1.58 g / cm³. 3The maximum aperture is 0.228–0.286 mm; the room temperature bending strength is not less than 3.24 MPa, and the high temperature bending strength is not less than 25.13 MPa; the sintering shrinkage rates in the length, width, and height directions of the ceramic core are 1.76%–3.97%, 1.64%–3.47%, and 1.67%–4.04%, respectively, and the casting shrinkage rates in the length, width, and height directions of the ceramic core are 1.74%–7.17%, 3.41%–9.26%, and 6.27%–11.29%, respectively. Detailed Implementation

[0034] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0035] This invention provides a photopolymerizable 3D printing silicon-based ceramic core slurry, comprising:

[0036] Ceramic powder 55wt%~65wt%;

[0037] Acrylic photosensitive resin 32wt%~42wt%;

[0038] Dispersant 3wt%~5wt%;

[0039] The sum of the amounts of the above components is 100%;

[0040] The ceramic powder includes:

[0041] Quartz glass powder 89wt%~98wt%;

[0042] Mineralizing agent 0.2wt%~10wt%;

[0043] Nano-alumina 0.1wt%~2wt%;

[0044] In the ceramic powder, the sum of the amounts of the above components is 100%.

[0045] Regarding ceramic powder:

[0046] The median particle size of the quartz glass powder is 6–8 μm, for example, 7 μm.

[0047] The mineralizer is at least one of alumina powder, silicon carbide powder, zirconium silicate powder, zirconium oxide powder, mullite powder, cristobalite, metallic silicon powder, silica micropowder, nano-silicon powder, nano-aluminum powder, aluminum powder, zirconium carbide, carbon nanotubes, carbon black, and graphene; the median particle size of the mineralizer is 0.05–40 μm, such as 20 μm, 5 μm, or 0.1 μm.

[0048] The median particle size of the nano-alumina is 30–50 nm, such as 30 nm, 40 nm, or 50 nm.

[0049] Regarding acrylate photosensitive resins:

[0050] The acrylate photosensitive resin comprises acrylate monomers and acrylate oligomers. In the acrylate photosensitive resin, the content of acrylate monomers is 55wt%–65wt%, and the content of acrylate oligomers is 35wt%–45wt%.

[0051] The acrylate monomers are at least one of the following: 1,6-hexanediol diacrylate (HDDA), 1,6-hexanediol dimethacrylate (HDDMA), dipropylene glycol diacrylate (DPGDA), trimethylolpropane triacrylate (TMPTA), triethylene glycol diacrylate (TEGDA), tripropylene glycol diacrylate (TPGDA), hydroxyethyl methacrylate (HEMA), pentaerythritol tetraacrylate (PET4A), pentaerythritol tetraacrylate ethoxylate (PPTTA), dipentaerythritol hexaacrylate (DPHA), isobornyl acrylate (IBOA), isobornyl methacrylate (IBOMA), polyethylene glycol (200) diacrylate (PEG(200)DA), and polyethylene glycol (400) diacrylate (PEG(400)DA).

[0052] The acrylate oligomer is at least one of aliphatic polyurethane acrylate, aromatic polyurethane acrylate, and modified epoxy acrylate. The aliphatic polyurethane acrylate is selected from at least one of bifunctional aliphatic polyurethane acrylate oligomer, trifunctional aliphatic polyurethane acrylate, and waterborne aliphatic polyurethane acrylate; the aromatic polyurethane acrylate is selected from at least one of trifunctional aromatic polyurethane acrylate oligomer, aromatic polyurethane modified acrylate, and aromatic polyurethane diacrylate; the modified epoxy acrylate is selected from at least one of epoxy acrylate oligomer, bisphenol A epoxy acrylate, and silicone modified epoxy acrylate.

[0053] The dispersant is at least one of Disperbyk-111, UV dispersant JZ-291, and BASK dispersant.

[0054] The solid content of the photopolymerizable 3D printing silicon-based ceramic core slurry is 55 vol.% to 65 vol.%, for example, 60 vol.%; the viscosity is 2400 to 3660 mPa·s, for example, 2894 mPa·s, 3660 mPa·s, 2648 mPa·s, 2801 mPa·s, 2986 mPa·s, 2718 mPa·s, 2400 mPa·s, 3525 mPa·s, and 3447 mPa·s. Viscosity affects the flowability of the slurry during the printing process, which in turn affects the uniformity of particle dispersion in the slurry, ultimately affecting the performance of the printed sample.

[0055] This invention provides a method for preparing the photopolymerizable 3D printing silicon-based ceramic core slurry described above, comprising the following steps:

[0056] Ceramic powder, acrylate photosensitive resin and dispersant are mixed to obtain photocurable 3D printing silicon-based ceramic core slurry;

[0057] The ceramic powder is obtained by mixing quartz glass powder, mineralizer and nano alumina.

[0058] The mixing specifically refers to mixing evenly.

[0059] This invention also provides a method for molding the photocurable 3D printing silicon-based ceramic core slurry described above, or the photocurable 3D printing silicon-based ceramic core slurry prepared by the preparation method described above, comprising the following steps:

[0060] A) Photopolymer 3D printing of silicon-based ceramic core slurry is performed to obtain a green body;

[0061] The process parameters for photopolymerization 3D printing include: a curing thickness of 75–100 μm and a curing power of 12–15 mW / cm². 2 The curing time for a single layer is 3 to 5 seconds;

[0062] B) The preform is degreased and sintered to obtain a photopolymerizable 3D printed silicon-based ceramic core.

[0063] In step B):

[0064] The degreasing and sintering include:

[0065] After raising the temperature from room temperature to 200-270℃ and holding it for 1-3 hours, raise the temperature to 300-400℃ and hold it for 1-3 hours, then raise the temperature to 500-600℃ and hold it for 1-2 hours, and finally raise the temperature to 1100-1300℃ and hold it for 4-8 hours.

[0066] The present invention also provides a photopolymerization 3D printing silicon-based ceramic core obtained by the molding method described above.

[0067] The present invention does not impose any special restrictions on the source of the raw materials used above, and they can be commercially available.

[0068] To further illustrate the present invention, the following detailed description, in conjunction with embodiments, describes a photocurable 3D printing silicon-based ceramic core slurry, its preparation method, and its application, but this should not be construed as limiting the scope of protection of the present invention.

[0069] Example 1

[0070] 1) Preparation of ceramic powder:

[0071] Quartz glass powder (median particle size 7 μm), mineralizer (alumina powder, median particle size 20 μm), and nano-alumina (median particle size 30 nm) are mixed evenly to obtain ceramic powder; the ceramic powder contains 89 wt% quartz glass powder, 10 wt% mineralizer, and 1 wt% nano-alumina.

[0072] 2) Preparation of photopolymerizable 3D printing silicon-based ceramic core slurry:

[0073] The ceramic powder, acrylate photosensitive resin, and dispersant (Disperbyk-111) from step 1) are mixed to obtain a photocurable 3D printing silicon-based ceramic core slurry. The acrylate photosensitive resin contains 60 wt% acrylate monomer (HDDA) and 40 wt% acrylate oligomer (epoxy acrylate oligomer). The photocurable 3D printing silicon-based ceramic core slurry contains 60 wt% ceramic powder, 35 wt% acrylate photosensitive resin, and 5 wt% dispersant. The solids content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.%, and the viscosity is 2894 mPa·s.

[0074] 3) A method for forming photopolymer 3D printing silicon-based ceramic core slurry, comprising the following steps:

[0075] 3-1) Photopolymerize the silicon-based ceramic core slurry for 3D printing to obtain a preform;

[0076] The process parameters for the photopolymer 3D printing include: a curing thickness of 85 μm and a curing power of 13 mW / cm². 2 The curing time for a single layer is 4 seconds;

[0077] 3-2) The preform is degreased and sintered to obtain a photopolymerizable 3D printed silicon-based ceramic core;

[0078] The degreasing and sintering are as follows:

[0079] The temperature was raised from room temperature to 230℃ and held for 2 hours, then raised to 350℃ and held for 2 hours, then raised to 550℃ and held for 1.5 hours, and finally raised to 1200℃ and held for 6 hours.

[0080] Example 2

[0081] The difference from Example 1 is as follows:

[0082] 1) Preparation of ceramic powder:

[0083] Quartz glass powder (median particle size of 7 μm), mineralizer (alumina powder, median particle size of 5 μm), and nano-alumina (median particle size of 40 nm) are mixed evenly to obtain ceramic powder; the ceramic powder contains 93 wt% quartz glass powder, 5 wt% mineralizer, and 2 wt% nano-alumina.

[0084] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 3660 mPa·s.

[0085] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0086] Example 3

[0087] The difference from Example 1 is as follows:

[0088] 1) Preparation of ceramic powder:

[0089] Quartz glass powder (median particle size 7 μm), mineralizer (alumina powder, median particle size 0.1 μm), and nano-alumina (median particle size 50 nm) are mixed evenly to obtain ceramic powder; the ceramic powder contains 98 wt% quartz glass powder, 1.8 wt% mineralizer, and 0.2 wt% nano-alumina.

[0090] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 2648 mPa·s.

[0091] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0092] Example 4

[0093] The difference from Example 1 is as follows:

[0094] Replace the alumina mineralizer with silicon carbide powder.

[0095] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 2801 mPa·s.

[0096] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0097] Example 5

[0098] The difference from Example 1 is as follows:

[0099] Replace the alumina mineralizer with zirconium silicate powder.

[0100] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 2986 mPa·s.

[0101] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0102] Example 6

[0103] The difference from Example 1 is as follows:

[0104] Replace the mineralizer, alumina powder, with graphene.

[0105] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 2718 mPa·s.

[0106] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0107] Example 7

[0108] The difference from Example 1 is as follows:

[0109] 2) Preparation of photopolymerizable 3D printing silicon-based ceramic core slurry:

[0110] The ceramic powder, acrylate photosensitive resin, and dispersant (Disperbyk-111) from step 1) are mixed to obtain a photocurable 3D printing silicon-based ceramic core slurry. The acrylate photosensitive resin contains 60 wt% acrylate monomer (HDDA) and 40 wt% acrylate oligomer (epoxy acrylate oligomer). The photocurable 3D printing silicon-based ceramic core slurry contains 55 wt% ceramic powder, 42 wt% acrylate photosensitive resin, and 3 wt% dispersant. The solids content of the photocurable 3D printing silicon-based ceramic core slurry is 55 vol.%, and the viscosity is 2400 mPa·s.

[0111] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0112] Example 8

[0113] The difference from Example 1 is as follows:

[0114] 2) Preparation of photopolymerizable 3D printing silicon-based ceramic core slurry:

[0115] The ceramic powder, acrylate photosensitive resin, and dispersant (Disperbyk-111) from step 1) are mixed to obtain a photocurable 3D printing silicon-based ceramic core slurry. The acrylate photosensitive resin contains 60 wt% acrylate monomer (HDDA) and 40 wt% acrylate oligomer (epoxy acrylate oligomer). The photocurable 3D printing silicon-based ceramic core slurry contains 64 wt% ceramic powder, 32 wt% acrylate photosensitive resin, and 4 wt% dispersant. The solids content of the photocurable 3D printing silicon-based ceramic core slurry is 64 vol.%, and the viscosity is 3525 mPa·s.

[0116] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0117] Example 9

[0118] The difference from Example 1 is as follows:

[0119] The dispersant Disperbyk-111 was replaced with BASK dispersant. The solid content of the photocurable 3D printing silicon-based ceramic core slurry was 60 vol.%, and the viscosity was 3447 mPa·s.

[0120] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0121] Example 10

[0122] The difference from Example 1 is as follows:

[0123] 3-1) Photopolymerize the silicon-based ceramic core slurry for 3D printing to obtain a preform;

[0124] The process parameters for the photopolymerization 3D printing include: a curing thickness of 75 μm and a curing power of 12 mW / cm². 2 The curing time for a single layer is 5 seconds.

[0125] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0126] Example 11

[0127] The difference from Example 1 is as follows:

[0128] 3-1) Photopolymerize the silicon-based ceramic core slurry for 3D printing to obtain a preform;

[0129] The process parameters for the photopolymerization 3D printing include: a curing thickness of 100 μm and a curing power of 15 mW / cm². 2 The curing time for a single layer is 5 seconds.

[0130] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0131] Example 12

[0132] The difference from Example 1 is as follows:

[0133] 3-2) The preform is degreased and sintered to obtain a photopolymerizable 3D printed silicon-based ceramic core;

[0134] The degreasing and sintering are as follows:

[0135] The temperature is raised from room temperature to 200℃ and held for 3 hours, then raised to 300℃ and held for 3 hours, then raised to 500℃ and held for 2 hours, and finally raised to 1100℃ and held for 8 hours.

[0136] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0137] Example 13

[0138] The difference from Example 1 is as follows:

[0139] 3-2) The preform is degreased and sintered to obtain a photopolymerizable 3D printed silicon-based ceramic core;

[0140] The degreasing and sintering are as follows:

[0141] The temperature is raised from room temperature to 270℃ and held for 1 hour, then raised to 400℃ and held for 1 hour, then raised to 600℃ and held for 1 hour, and finally raised to 1300℃ and held for 4 hours.

[0142] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0143] Comparative Example 1

[0144] The difference from Example 1 is that (the ceramic powder does not contain nano-alumina):

[0145] 1) Preparation of ceramic powder:

[0146] Quartz glass powder (median particle size of 7 μm) and mineralizer (alumina powder, median particle size of 20 μm) are mixed evenly to obtain ceramic powder; the content of quartz glass powder in the ceramic powder is 89 wt%, and the content of mineralizer is 11 wt%.

[0147] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 2589 mPa·s.

[0148] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0149] Comparative Example 2

[0150] The difference from Example 1 is that (the ceramic powder does not contain a mineralizer):

[0151] 1) Preparation of ceramic powder:

[0152] Quartz glass powder (median particle size of 7 μm) and nano-alumina (median particle size of 30 nm) are mixed evenly to obtain ceramic powder; the ceramic powder contains 99 wt% quartz glass powder and 1 wt% nano-alumina.

[0153] In step 2), the solid content of the photocurable 3D printing silicon-based ceramic core slurry is 60 vol.% and the viscosity is 2746 mPa·s.

[0154] The remaining steps and parameters are the same as in Example 1, and a photopolymer 3D printed silicon-based ceramic core is obtained.

[0155] The physical properties of the photopolymer 3D printed silicon-based ceramic cores prepared in Examples 1-17 and Comparative Example 1 were tested according to standard number AETM181A, and the results are shown in Table 1.

[0156] Table 1. Physical properties of photopolymerized 3D printed silicon-based ceramic cores prepared in Examples 1-17 and Comparative Examples 1-2

[0157]

[0158] The performance of the photopolymer 3D printed silicon-based ceramic cores prepared in Examples 1-13 and Comparative Examples 1-2 was tested according to standard number HB5353, and the results are shown in Table 2.

[0159] Table 2. Performance of the photopolymer 3D printed silicon-based ceramic cores prepared in Examples 1-13 and Comparative Examples 1-2

[0160]

[0161]

[0162] The results in Tables 1 and 2 indicate that the shrinkage of the 3D-printed silicon-based ceramic core is mainly due to interlayer shrinkage and shrinkage between ceramic particles. The more fully the ceramic particles between adjacent layers are sintered, the greater the shrinkage rate. The addition of nano-alumina increases the sintering barrier of quartz glass and reduces the sintering driving force of quartz glass powder, thus helping to reduce the sintering shrinkage rate. However, excessive nano-alumina can lead to a decrease in flexural strength. Furthermore, the higher the solid content and sintering temperature of the ceramic slurry, the greater the driving force during sintering, the higher the densification degree of the sample, and the greater the strength. Therefore, under the combined effect of nano-alumina, solid content, and sintering temperature, the physical and performance properties of the embodiments of the present invention have reached the optimal values. As can be seen from Tables 1 and 2, the physical and performance properties of the embodiments of the present invention meet the casting and use requirements of high-temperature alloy blades. The shrinkage rate of the prepared 3D-printed ceramic core is controllable during preparation and service, and the room temperature strength and high temperature strength are optimal, which well meets the main requirements of high-temperature alloys.

[0163] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A photopolymerizable 3D printing silicon-based ceramic core slurry, comprising: Ceramic powder 55 wt%~65 wt%; Acrylic photosensitive resin 32 wt%~42 wt%; Dispersant 3 wt%~5 wt%; The sum of the amounts of the above components is 100%; The ceramic powder includes: Quartz glass powder 89 wt%~98 wt%; Mineralizing agent 0.2 wt%~10 wt%; Nano-alumina 0.1 wt%~2 wt%; In the ceramic powder, the sum of the amounts of the above components is 100%; The acrylate photosensitive resin comprises acrylate monomers and acrylate oligomers; the acrylate oligomers are at least one of aliphatic polyurethane acrylate, aromatic polyurethane acrylate, and modified epoxy acrylate; in the acrylate photosensitive resin, the content of acrylate monomers is 55 wt%~65 wt%, and the content of acrylate oligomers is 35 wt%~45 wt%. The median particle size of the quartz glass powder is 6~8 μm; The median particle size of the nano-alumina is 30~50 nm.

2. The photopolymerizable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that, The mineralizer is at least one of alumina powder, silicon carbide powder, zirconium silicate powder, zirconium oxide powder, mullite powder, cristobalite, metallic silicon powder, silicon micro powder, nano silicon powder, zirconium carbide, carbon black, carbon nanotubes, nano aluminum powder, aluminum powder, and graphene; the median particle size of the mineralizer is 0.05~40 μm.

3. The photopolymerizable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that, The acrylate monomers are at least one of the following: 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, trimethylolpropane triacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, hydroxyethyl methacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylate, dipentaerythritol hexaacrylate, isobornyl acrylate, isobornyl methacrylate, polyethylene glycol (200) diacrylate, and polyethylene glycol (400) diacrylate.

4. The photopolymerizable 3D printing silicon-based ceramic core slurry according to claim 1, characterized in that, The dispersant is at least one of Disperbyk-111, UV dispersant JZ-291, and BASK dispersant.

5. A method for preparing the photocurable 3D printing silicon-based ceramic core slurry according to any one of claims 1 to 4, comprising the following steps: Ceramic powder, acrylate photosensitive resin and dispersant are mixed to obtain photocurable 3D printing silicon-based ceramic core slurry; The ceramic powder is obtained by mixing quartz glass powder, mineralizer and nano alumina.

6. A method for molding the photopolymerizable 3D printing silicon-based ceramic core slurry according to any one of claims 1 to 4, comprising the following steps: A) Photopolymer 3D printing of silicon-based ceramic core slurry is performed to obtain a green body; The process parameters for photopolymerization 3D printing include: a curing thickness of 75~100 μm and a curing power of 12~15 mW / cm. 2 The curing time for a single layer is 3-5 seconds; B) The preform is degreased and sintered to obtain a photopolymerizable 3D printed silicon-based ceramic core.

7. The photopolymerization 3D printing silicon-based ceramic core prepared by the molding method of claim 6.

Citation Information

Patent Citations

  • Making method of silicon-based ceramic core with adjustable thermal expansion coefficient

    CN104086161A

  • Ceramic core slurry for 3D printing as well as preparation method and application of ceramic core slurry

    CN113563059A