Preparation method of vehicle coating with self-repairing and self-cleaning functions

By adding self-healing materials and titanium dioxide powder prepared by high-temperature and high-pressure reactions into automotive coatings, the problem of scratches and contamination in long-term use of automotive coatings is solved, the self-repairing and self-cleaning functions of the coating are realized, and the service life is extended. The service life of paint.

CN118755375APending Publication Date: 2024-10-11CHONGQING IND POLYTECHNIC COLLEGE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411013622.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing automotive coatings are prone to scratches, contamination and other problems during long-term use, affecting the appearance and service life of the car.

Method used

Using polyethylene glycol, hexamethylene diisocyanate trimer, urethane and monophosphate as raw materials, the self-healing material is prepared through high temperature and high pressure reaction, mixed with titanium dioxide powder, and added to the car paint to form Self-healing and self-cleaning coatings.

Benefits of technology

The coating can automatically repair when scratched or damaged, maintain the integrity and aesthetics of the coating, reduce the adhesion of pollutants, keep the car surface clean and hygienic, extend the service life, and have good weather resistance and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755375A_ABST
    Figure CN118755375A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, in particular to a preparation method of an automotive coating with self-repairing and self-cleaning functions, which comprises the following steps: by taking polyethylene glycol, hexamethylene diisocyanate tripolymer, ethyl carbamate and monophosphate as raw materials, dissolving the raw materials in a nitric acid solvent, reacting in a high-temperature and high-pressure reaction kettle, and cooling to room temperature to obtain the automotive coating with the self-repairing and self-cleaning functions. The preparation method comprises the following steps: preparing a self-repairing material by using titanium dioxide as a raw material, automatically repairing when a coating is scratched or damaged by the self-repairing material, and keeping the integrity and attractiveness of the coating, and adopting titanium dioxide powder as a self-cleaning material, so that the adhesion of pollutants can be effectively reduced, the pollutants can be degraded, and the cleanness and sanitation of the surface of an automobile can be kept; the self-repairing material and the self-cleaning material are mixed and then added into the vehicle paint, the vehicle paint with the self-repairing and self-cleaning functions is prepared, the paint has good weather resistance and wear resistance and can adapt to various weather and environmental conditions, and the service life of the paint is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a method for preparing a vehicle coating with self-repairing and self-cleaning functions. Background Art

[0002] Paint refers to a liquid or powder material that is applied to the surface of a material to form a film with certain functions on the surface of the material. After the production of a car is completed, paint needs to be applied to the surface of the car. With the rapid development of science and technology, the requirements for paint are getting higher and higher.

[0003] Existing automotive paints are not resistant to high temperatures. They will crack, bubble, and fall off if exposed to the sun for a long time. At the same time, they have poor waterproof properties and are easily penetrated by rainwater, causing internal corrosion. In addition, the paint is not resistant to bumps and has poor wear resistance and adhesion. After being scratched, the paint will fall off, making it easy to corrode.

[0004] Prior art CN115073994A discloses a self-cleaning water-based automotive coating and a preparation method thereof. The coating adopts water-based fluorosilicone-modified polyurethane as the main resin and appropriately adds silicone resin and related additives to further reduce the surface energy of the paint film. The low surface energy and low surface roughness structure make the coating have good self-cleaning properties, and also significantly improve the gloss, hydrophobicity and anti-fouling properties of the automotive paint film.

[0005] However, although the above-mentioned automotive coatings have certain weather resistance and wear resistance, they will still have problems such as scratches and pollution during long-term use, which will affect the appearance and service life of the car. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a self-repairing and self-cleaning automotive coating, which aims to solve the technical problem that although the existing automotive coatings have certain weather resistance and wear resistance, they will still have scratches, pollution and other problems during long-term use, thereby affecting the appearance and service life of the car.

[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:

[0008] The present invention provides a method for preparing a vehicle coating having self-repairing and self-cleaning functions, comprising the following steps:

[0009] Step 1: selecting polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate as raw materials, and weighing the raw materials respectively according to a specific mass ratio;

[0010] Step 2: mixing the raw materials uniformly to obtain a mixture, then dissolving the mixture in a nitric acid solvent and stirring uniformly to obtain a mixed solution;

[0011] Step 3: placing the mixed solution in a high-temperature and high-pressure reactor for reaction, and after the reaction, filtering, washing and drying the reaction solution obtained by the reaction to obtain a self-healing material;

[0012] Step 4: Evenly mix the prepared self-repairing material and titanium dioxide powder according to a certain mass ratio, and add the mixed self-repairing and self-cleaning material into the car paint, and stir evenly;

[0013] Step 5: Apply the uniformly stirred paint on the surface of the car, and dry and cure it as needed to form a car coating. At this time, the car surface has self-repairing and self-cleaning functions.

[0014] Wherein, the polyethylene glycol, the hexamethylene diisocyanate trimer, the ethyl formate and the monophosphate in the step 1 are mixed in a mass ratio of 6:1:2:1.

[0015] Wherein, the mass ratio of the mixture in the step 2 to the nitric acid solvent is 1:4.

[0016] Wherein, the reaction conditions of the mixed solution in the step 3 in the high temperature and high pressure reactor are: 180° C., 8 MPa.

[0017] Wherein, the reaction time of the mixed solution in the step three in the high temperature and high pressure reactor is 1 hour.

[0018] Among them, the mass ratio of the self-healing material to the titanium dioxide powder in the step four is 5:1.

[0019] Among them, the mass ratio of the self-repairing and self-cleaning material in step four to the car paint is 3:7.

[0020] The present invention discloses a method for preparing a vehicle coating with self-repairing and self-cleaning functions. The method adopts polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate as raw materials, dissolves the raw materials in a nitric acid solvent, and then reacts in a high-temperature and high-pressure reactor to prepare a self-repairing material. The self-repairing material can automatically repair the coating when it is scratched or damaged, thereby maintaining the integrity and aesthetics of the coating. Titanium dioxide powder is used as the self-cleaning material, thereby effectively reducing the adhesion of pollutants and degrading pollutants, thereby maintaining the cleanliness and hygiene of the surface of the automobile. Afterwards, the self-repairing material and the self-cleaning material are mixed and added to a vehicle paint to prepare a vehicle coating with self-repairing and self-cleaning functions. The coating has good weather resistance and wear resistance, can adapt to various climates and environmental conditions, and prolongs the service life of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention is further illustrated by means of the non-limiting examples given in the accompanying drawings.

[0022] Figure 1 It is a process step diagram of a method for preparing a vehicle coating with self-repairing and self-cleaning functions according to the first embodiment of the present invention. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0024] First embodiment

[0025] See also Figure 1 , Figure 1 1 is a process flow chart of a method for preparing a coating for a vehicle having a self-repairing and self-cleaning function according to a first embodiment of the present invention. The present invention provides a method for preparing a coating for a vehicle having a self-repairing and self-cleaning function, comprising the following steps:

[0026] S101, step 1: selecting polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate as raw materials, and weighing the raw materials respectively according to a specific mass ratio;

[0027] S102, step 2: mixing the raw materials uniformly to obtain a mixture, then dissolving the mixture in a nitric acid solvent and stirring uniformly to obtain a mixed solution;

[0028] S103, step three: placing the mixed solution in a high-temperature and high-pressure reactor for reaction, and after the reaction, filtering, washing and drying the reaction solution obtained by the reaction to obtain a self-healing material;

[0029] S104, step 4: mixing the prepared self-repairing material and titanium dioxide powder in a certain mass ratio, adding the mixed self-repairing and self-cleaning material to the car paint, and stirring evenly;

[0030] S105, step five: applying the uniformly stirred coating to the surface of the car, and drying and curing the coating as required to form a car coating. At this time, the car surface has self-repairing and self-cleaning functions.

[0031] In this embodiment, the present invention adopts polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate as raw materials, dissolves the raw materials in nitric acid solvent, and then places them in a high temperature and high pressure reactor for reaction to prepare a self-repairing material. The self-repairing material can automatically repair the coating when it is scratched or damaged to maintain the integrity and aesthetics of the coating. By adopting titanium dioxide powder as a self-cleaning material, it can effectively reduce the adhesion of pollutants and degrade pollutants to keep the surface of the car clean and hygienic. Afterwards, the self-repairing material and the self-cleaning material are mixed and added to the car paint to prepare a car coating with self-repairing and self-cleaning functions. The coating has good weather resistance and wear resistance, can adapt to various climates and environmental conditions, and extend the service life of the coating.

[0032] Wherein, the polyethylene glycol, the hexamethylene diisocyanate trimer, the ethyl formate and the monophosphate in the step 1 are mixed in a mass ratio of 6:1:2:1.

[0033] Secondly, the mass ratio of the mixture in the step 2 to the nitric acid solvent is 1:4, and the uniform mixing of the raw materials in the step 2 and the uniform stirring of the mixture and the nitric acid solvent are both achieved by spiral stirring.

[0034] Again, the reaction conditions of the mixed solution in step three in the high temperature and high pressure reactor are: 180° C., 8 MPa, and the reaction time of the mixed solution in step three in the high temperature and high pressure reactor is 1 hour.

[0035] At the same time, the mass ratio of the self-healing material to the titanium dioxide powder in step four is 5:1.

[0036] In addition, the mass ratio of the self-repairing and self-cleaning material in step four to the vehicle paint coating is 3:7.

[0037] Finally, the self-repairing and self-cleaning material and the vehicle paint in step 4 are uniformly stirred by high-speed stirring in a mixer.

[0038] When using a preparation method of a vehicle coating with self-repairing and self-cleaning functions of the present embodiment, polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate are selected as raw materials, and the raw materials are weighed respectively according to a specific mass ratio, and then the raw materials are mixed uniformly in a mass ratio of 6:1:2:1 to obtain a mixture, and then the mixture is dissolved in a nitric acid solvent in a mass ratio of 1:4 between the mixture and the nitric acid solvent, and the mixture is stirred uniformly by spiral stirring to obtain a mixed solution, and then the mixed solution is placed in a high temperature and high pressure reactor for reaction, and the reaction conditions are: 180°C, 8MPa, and the reaction time is 1h. After the reaction, the reaction solution obtained by the reaction is filtered, washed and dried to obtain a self-repairing material. After obtaining the self-repairing material, the prepared self-repairing material and titanium dioxide powder are evenly mixed in a mass ratio of 5:1, and the mixed self-repairing and self-cleaning material is added to the car paint in a mass ratio of 3:7 between the self-repairing and self-cleaning material and the car paint, and then evenly stirred by a high-speed mixer. After that, the evenly stirred paint is applied to the surface of the car, and dried and cured as needed to form a car coating. At this time, the car surface has self-repairing and self-cleaning functions, which can effectively resist the influence of the external environment.

[0039] The vehicle coating prepared by the present invention has the following characteristics:

[0040] 1. The coating contains self-healing materials that can automatically repair the coating when it is scratched or damaged, maintaining the integrity and aesthetics of the coating;

[0041] 2. The coating contains self-cleaning materials, which can effectively reduce the adhesion of pollutants and degrade pollutants to keep the surface of the car clean and hygienic;

[0042] 3. The coating has good weather resistance and wear resistance, can adapt to various climate and environmental conditions, and extend the service life of the coating;

[0043] 4. The coating has a simple construction process, is easy to operate and control, and is suitable for all types of automotive surfaces.

[0044] The automotive coating prepared by the present invention can, when the surface of the vehicle is damaged, achieve self-repair of the scratched paint surface through the special components in the coating without damaging the primer, and has a good cleaning effect. At the same time, the durability, aesthetics and functionality of the automotive coating are improved, and the cost and time of daily maintenance of the vehicle are reduced.

[0045] In summary, the present invention adopts polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate as raw materials, dissolves the raw materials in nitric acid solvent, and then places them in a high-temperature and high-pressure reactor for reaction to prepare a self-repairing material. The self-repairing material can automatically repair itself when the coating is scratched or damaged to maintain the integrity and aesthetics of the coating. By adopting titanium dioxide powder as a self-cleaning material, it can effectively reduce the adhesion of pollutants and degrade pollutants to keep the surface of the car clean and hygienic. Afterwards, the self-repairing material and the self-cleaning material are mixed and added to the car paint to prepare a car coating with self-repairing and self-cleaning functions. The coating has good weather resistance and wear resistance, can adapt to various climates and environmental conditions, and extend the service life of the coating.

[0046] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing a vehicle coating having self-repairing and self-cleaning functions, characterized in that: The following steps are involved: Step 1: selecting polyethylene glycol, hexamethylene diisocyanate trimer, ethyl formate and monophosphate as raw materials, and weighing the raw materials respectively according to a specific mass ratio; Step 2: mixing the raw materials uniformly to obtain a mixture, then dissolving the mixture in a nitric acid solvent and stirring uniformly to obtain a mixed solution; Step 3: placing the mixed solution in a high-temperature and high-pressure reactor for reaction, and after the reaction, filtering, washing and drying the reaction solution obtained by the reaction to obtain a self-healing material; Step 4: Evenly mix the prepared self-repairing material and titanium dioxide powder according to a certain mass ratio, and add the mixed self-repairing and self-cleaning material into the car paint, and stir evenly; Step 5: Apply the uniformly stirred paint on the surface of the car, and dry and cure it as needed to form a car coating. At this time, the car surface has self-repairing and self-cleaning functions.

2. The method for preparing a vehicle coating having self-repairing and self-cleaning functions according to claim 1, characterized in that: The polyethylene glycol, the hexamethylene diisocyanate trimer, the ethyl formate and the monophosphate in the step 1 are mixed in a mass ratio of 6:1:2:

1.

3. The method for preparing a vehicle coating having self-repairing and self-cleaning functions according to claim 1, characterized in that: The mass ratio of the mixture in the step 2 to the nitric acid solvent is 1:

4.

4. The method for preparing a vehicle coating having self-repairing and self-cleaning functions according to claim 1, characterized in that: The reaction conditions of the mixed solution in the step 3 in the high temperature and high pressure reactor are: 180° C., 8 MPa.

5. The method for preparing a vehicle coating having self-repairing and self-cleaning functions according to claim 4, characterized in that: The reaction time of the mixed solution in the step 3 in the high temperature and high pressure reactor is 1 hour.

6. The method for preparing a vehicle coating having self-repairing and self-cleaning functions according to claim 1, characterized in that: The mass ratio of the self-healing material to the titanium dioxide powder in the step 4 is 5:

1.

7. The method for preparing a vehicle coating having self-repairing and self-cleaning functions according to claim 1, characterized in that: The mass ratio of the self-repairing and self-cleaning material to the vehicle paint in step 4 is 3:7.

Citation Information

Patent Citations

  • Polyurethane elastomer of high clarity

    CN101039976A

  • Urethane acrylate intermediate of adhesive for bonding touch screen and preparation method thereof

    CN102604034A

  • Anti-corrosive waterborne coating and preparation method thereof

    CN109266188A

  • Antifouling self-repairing coating and preparation method thereof

    CN109401598A

  • Micro-nano structure repairing type super-hydrophobic coating and preparation method thereof

    CN113652125A