Environment-friendly and low-cost method for preparing Ag2BiI5 photoelectric film

The preparation of Ag2BiI5 optoelectronic films using non-toxic solvents and low-temperature annealing processes solves the problems of toxic solvents and high costs in existing technologies, achieving low-cost, environmentally friendly optoelectronic film preparation with excellent optoelectronic properties.

CN118763000APending Publication Date: 2024-10-11HEFEI UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410819698.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11

Smart Images

  • Figure CN118763000A_ABST
    Figure CN118763000A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly and low-cost method for preparing an Ag2BiI5 photoelectric film, which comprises the following steps of: dispersing silver iodide and bismuth iodide powder which are mixed according to a certain molar ratio into a non-toxic solvent, and stirring at room temperature; then, placing the dispersion liquid in a reaction kettle, and enabling the dispersion liquid to react at a relatively low temperature; and after the reaction is sufficient, repeatedly washing and grinding a crude product to obtain Ag2BiI5 powder. And finally, ultrasonically dispersing the Ag2BiI5 powder in a non-toxic solvent to prepare low-concentration slurry, and spraying the low-concentration slurry to form a film. The method has the advantages of simplicity in operation, low cost, non-toxic and environment-friendly solvent and the like. In addition, the photocurrent, responsivity and detectivity of the prepared compact Ag2BiI5 photoelectric film can reach 14.5 [mu] A, 1.1 * 10 <-4 > AW <-1 > and 1.2 * 10 < 8 > Jone respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of perovskite materials, and in particular to an environmentally friendly and low-cost method for preparing an Ag2BiI5 photoelectric film. Background Art

[0002] Perovskite materials, represented by organic-inorganic hybrid perovskites, have attracted extensive attention as photoelectric conversion materials in the fields of solar cells and photodetectors due to their large light absorption coefficient, high carrier mobility and long photogenerated carrier lifetime. However, the low stability and high toxicity of such materials limit their application prospects. Silver bismuth iodide (Ag2BiI5) in all-inorganic perovskite materials has become one of the photoelectric conversion materials with great development potential due to its non-toxicity, high stability and high photoelectric conversion efficiency.

[0003] At present, the mainstream preparation method of Ag2BiI5 photoelectric film is one-step solution spin coating. The solvent used in this process is usually a mixed solution of dimethyl sulfoxide (DMSO) and N-dimethylformamide (DMF) with a concentration of 0.1-1 mol / L. DMSO and DMF may enter the human body through the skin during volatilization, and have vascular toxicity and hepato-renal toxicity. In addition, although some researchers avoid using toxic solvents and prepare Ag2BiI5 photoelectric film by vacuum thermal evaporation of Ag on BiI3 film or by mixing AgI with BiI3 powder and then spin coating after high-temperature solid-phase reaction, the preparation cost of such methods is relatively high. Therefore, it is necessary to develop an environmentally friendly and low-cost film preparation method to promote the further development of Ag2BiI5 photoelectric film. Summary of the invention

[0004] The object of the present invention is to provide an environmentally friendly, low-cost method for preparing Ag2BiI5 photoelectric film, which has a simple process and uses non-toxic solvents.

[0005] In one aspect of the present invention, the present invention provides an environmentally friendly, low-cost method for preparing Ag2BiI5 photoelectric film. According to an embodiment of the present invention, the method comprises the following steps:

[0006] (1) mixing silver iodide and bismuth iodide powders and dispersing them in a non-toxic solvent to prepare a precursor solution;

[0007] (2) placing the precursor solution in a reaction vessel for reaction;

[0008] (3) After the reaction is complete, the crude product is repeatedly washed, dried, and ground to obtain Ag2BiI5 powder;

[0009] (4) ultrasonically dispersing Ag2BiI5 powder in a non-toxic solvent to prepare a slurry;

[0010] (5) After the slurry is prepared into a film by spraying, low-temperature annealing is performed to further densify it, thereby obtaining the Ag2BiI5 photoelectric film.

[0011] In addition, the environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to the above embodiment of the present invention may also have the following additional technical features:

[0012] In some embodiments of the present invention, in step (1), the molar ratio of silver iodide to bismuth iodide powder is 2:1, and the concentration of the precursor solution is 0.0375-0.075 mol / L.

[0013] In some embodiments of the present invention, in step (2), the reaction temperature is 170-210° C., and the reaction time is 2-3 h.

[0014] In some embodiments of the present invention, in step (3), washing is performed using a non-toxic solvent.

[0015] In some embodiments of the present invention, in step (4), the slurry concentration is 0.01-0.03 mol / L.

[0016] In some embodiments of the present invention, in step (5), the slurry is sprayed onto a substrate placed on a heating platform at 100° C. for 25-75 seconds to prepare a film.

[0017] In some embodiments of the present invention, in step (5), the low-temperature annealing is carried out in a tube furnace in an argon atmosphere at a temperature of 120-135° C. and an annealing time of 10 min.

[0018] In some embodiments of the present invention, the non-toxic solvent is anhydrous ethanol.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) The preparation method provided by the present invention has a simple process, uses a non-toxic solvent, and can be prepared at a relatively low temperature.

[0021] 2) The preparation method provided by the present invention can prepare Ag2BiI5 film with excellent photoelectric performance at a relatively low concentration, with a photocurrent of up to 14.5μA and a responsivity of 1.1×10 -4 AW -1 , the detection degree is 1.2×10 8 Jones. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1is the XRD pattern of the Ag2BiI5 powder prepared in Examples 1, 2 and 3 of the present invention, wherein the red line represents the Ag2BiI5 standard PDF card (PDF#35-1025);

[0023] Figure 2 is a SEM image of the Ag2BiI5 photoelectric film prepared in Examples 2, 4, and 5 of the present invention;

[0024] Figure 3 is the UV-visible light absorption spectrum of the Ag2BiI5 photoelectric film prepared in Examples 1-5 of the present invention;

[0025] Figure 4 It spectra of Ag2BiI5 photoelectric films prepared in Examples 1-5 of the present invention, (a) is 5 cycles of 20s of illumination followed by 20s of darkness, (b) is continuous illumination for 100s;

[0026] Figure 5 It is the electrochemical impedance spectrum of the Ag2BiI5 photoelectric film prepared in Examples 1-5 of the present invention;

[0027] Figure 6 This is an optical photograph of the Ag2BiI5 photoelectric film prepared in embodiment 5 of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] An environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film comprises the following steps:

[0031] Step 1: silver iodide and bismuth iodide powders are mixed at a molar ratio of 2:1, dispersed in anhydrous ethanol to prepare a 0.075 mol / L precursor solution, and magnetically stirred at room temperature for standby use;

[0032] Step 2: The Ag2BiI5 dispersion obtained in step 1 is transferred to a reaction vessel and reacted at 170°C for 2h for later use;

[0033] Step 3: The crude Ag2BiI5 product obtained in step 2 is washed with anhydrous ethanol for multiple times, and then dried and ground to obtain Ag2BiI5 powder, and the obtained Ag2BiI5 powder is stored at room temperature for later use;

[0034] Step 4: Disperse the Ag2BiI5 powder obtained in step 3 in anhydrous ethanol to prepare a 0.01 mol / L Ag2BiI5 slurry, homogenize it with ultrasound, and set aside;

[0035] Step 5: Use a spray gun to spray the slurry prepared in step 4 onto a substrate placed on a heating platform at 100° C. for 25 seconds to obtain an Ag2BiI5 film with a thickness of about 0.5 μm for later use;

[0036] Step 6: Place the Ag2BiI5 film obtained in step 5 in a tubular furnace and anneal it at 130°C for 10 minutes in an argon atmosphere to obtain a dense Ag2BiI5 photoelectric film.

[0037] Example 2

[0038] An environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film comprises the following steps:

[0039] Step 1: Silver iodide and bismuth iodide powders are mixed at a molar ratio of 2:1, dispersed in anhydrous ethanol to prepare a 0.075 mol / L precursor solution, and magnetically stirred at room temperature for standby use;

[0040] Step 2: Transfer the Ag2BiI5 dispersion obtained in step 1 to a reactor and react at 190°C for 2h;

[0041] Step 3: The crude Ag2BiI5 product obtained in step 2 is washed with anhydrous ethanol for multiple times, and then dried and ground to obtain Ag2BiI5 powder, and the obtained Ag2BiI5 powder is stored at room temperature for later use;

[0042] Step 4: Disperse the Ag2BiI5 powder obtained in step 3 in anhydrous ethanol to prepare a 0.01 mol / L Ag2BiI5 slurry, homogenize it with ultrasound, and set aside;

[0043] Step 5: Use a spray gun to spray the slurry prepared in step 4 onto a substrate placed on a heating platform at 100° C. for 25 seconds to obtain an Ag2BiI5 film with a thickness of about 0.5 μm for later use;

[0044] Step 6: Place the Ag2BiI5 film obtained in step 5 in a tubular furnace and anneal it at 130°C for 10 minutes in an argon atmosphere to obtain a dense Ag2BiI5 photoelectric film.

[0045] Example 3

[0046] An environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film comprises the following steps:

[0047] Step 1: Silver iodide and bismuth iodide powders are mixed at a molar ratio of 2:1, dispersed in anhydrous ethanol to prepare a 0.075 mol / L precursor solution, and magnetically stirred at room temperature for standby use;

[0048] Step 2: Transfer the Ag2BiI5 dispersion obtained in step 1 to a reactor and react at 210°C for 2h;

[0049] Step 3: The crude Ag2BiI5 product obtained in step 2 is washed with anhydrous ethanol for multiple times, and then dried and ground to obtain Ag2BiI5 powder, and the obtained Ag2BiI5 powder is stored at room temperature for later use;

[0050] Step 4: Disperse the Ag2BiI5 powder obtained in step 3 in anhydrous ethanol to prepare a 0.01 mol / L Ag2BiI5 slurry, homogenize it with ultrasound, and set aside;

[0051] Step 5: Use a spray gun to spray the slurry prepared in step 4 onto a substrate placed on a heating platform at 100° C. to obtain an Ag2BiI5 film. Spray for 25 seconds to obtain an Ag2BiI5 film with a thickness of about 0.5 μm for later use.

[0052] Step 6: Place the Ag2BiI5 film obtained in step 5 in a tubular furnace and anneal it at 130°C for 10 minutes in an argon atmosphere to obtain a dense Ag2BiI5 photoelectric film.

[0053] like Figure 1 As shown, well-crystallized Ag2BiI5 crystals can be prepared in a non-toxic solvent by solvothermal method.

[0054] Example 4

[0055] An environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film comprises the following steps:

[0056] Step 1: Silver iodide and bismuth iodide powders are mixed at a molar ratio of 2:1, dispersed in anhydrous ethanol to prepare a 0.075 mol / L precursor solution, and magnetically stirred at room temperature for standby use;

[0057] Step 2: Transfer the Ag2BiI5 dispersion obtained in step 1 to a reactor and react at 190°C for 2h;

[0058] Step 3: The crude Ag2BiI5 product obtained in step 2 is washed with anhydrous ethanol for multiple times, and then dried and ground to obtain Ag2BiI5 powder, and the obtained Ag2BiI5 powder is stored at room temperature for later use;

[0059] Step 4: Disperse the Ag2BiI5 powder obtained in step 3 in anhydrous ethanol to prepare a 0.03 mol / L Ag2BiI5 solution, homogenize it with ultrasound, and set aside;

[0060] Step 5: Use a spray gun to spray the slurry prepared in step 4 onto a substrate placed on a heating platform at 100° C. to obtain an Ag2BiI5 film. Spray for 25 seconds to obtain an Ag2BiI5 film with a thickness of about 0.5 μm for later use.

[0061] Step 6: Place the Ag2BiI5 film obtained in step 5 in a tubular furnace and anneal it at 130°C for 10 minutes in an argon atmosphere to obtain a dense Ag2BiI5 photoelectric film.

[0062] Depend on Figure 2 As described above, low-concentration spraying can obtain a Ag2BiI5 photoelectric film with a uniform and dense surface.

[0063] Example 5

[0064] An environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film comprises the following steps:

[0065] Step 1: Silver iodide and bismuth iodide powders are mixed at a molar ratio of 2:1, dispersed in anhydrous ethanol to prepare a 0.075 mol / L precursor solution, and magnetically stirred at room temperature for standby use;

[0066] Step 2: Transfer the Ag2BiI5 dispersion obtained in step 1 to a reactor and react at 190°C for 2h;

[0067] Step 3: The crude Ag2BiI5 product obtained in step 2 is washed with anhydrous ethanol for multiple times, and then dried and ground to obtain Ag2BiI5 powder, and the obtained Ag2BiI5 powder is stored at room temperature for later use;

[0068] Step 4: Disperse the Ag2BiI5 powder obtained in step 3 in anhydrous ethanol to prepare a 0.01 mol / L Ag2BiI5 solution, homogenize it with ultrasound, and set aside;

[0069] Step 5: Use a spray gun to spray the slurry prepared in step 4 onto a substrate placed on a heating platform at 100° C. to obtain an Ag2BiI5 film. Spray for 75 seconds to obtain an Ag2BiI5 film with a thickness of about 1 μm for later use.

[0070] Step 6: Place the Ag2BiI5 film obtained in step 5 in a tubular furnace and anneal it at 130°C for 10 minutes in an argon atmosphere to obtain a dense Ag2BiI5 photoelectric film.

[0071] The Ag2BiI5 photoelectric film samples obtained in Examples 1-5 were directly pasted on the sample stage to test the light absorption performance of the film samples. The test wavelength range was 350-750nm. Figure 3 As shown, the optical absorption performance of the low-concentration sprayed Ag2BiI5 photovoltaic film is good.

[0072] The Ag2BiI5 photoelectric film samples obtained in Examples 1-5 were placed in a three-electrode system, and the It curves of the film samples were tested using an electrochemical workstation (CHI660E) and a cold light source xenon lamp (HDL-Ⅱ), with zero bias. The electrolyte was a 1M anhydrous Na2SO4 aqueous solution, the counter electrode was a Pt electrode, the reference electrode was an Ag / AgCl electrode, and a xenon lamp was used to simulate sunlight, with an incident light intensity of 100 mW cm -2 .Depend on Figure 4 As shown, the photocurrent response intensity of the Ag2BiI5 photoelectric film prepared by powdering at 190°C and then spraying is the highest, and the photoelectric response speed and photoelectric response intensity are optimal when the spraying concentration is 0.01M.

[0073] The Ag2BiI5 photoelectric film samples obtained in Examples 1-5 were placed in a three-electrode system, and the electrochemical impedance of the film samples was tested using an electrochemical workstation (CHI660E). The test frequency range was 0.01 to 100,000 Hz. Figure 5 As shown, the impedance of the Ag2BiI5 photoelectric film prepared by spraying 0.01M after powdering at 190℃ is the smallest.

[0074] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An environmentally friendly, low-cost method for preparing Ag2BiI5 photoelectric film, characterized in that: The following steps are involved: (1) mixing silver iodide and bismuth iodide powders and dispersing them in a non-toxic solvent to prepare a precursor solution; (2) placing the precursor solution in a reaction vessel for reaction; (3) After the reaction is complete, the crude product is repeatedly washed, dried, and ground to obtain Ag2BiI5 powder; (4) ultrasonically dispersing Ag2BiI5 powder in a non-toxic solvent to prepare a slurry; (5) After the slurry is prepared into a film by spraying, low-temperature annealing is performed to further densify it, thereby obtaining the Ag2BiI5 photoelectric film.

2. The method for preparing Ag2BiI5 photoelectric film in an environmentally friendly and low-cost manner according to claim 1, characterized in that: In the step (1), the molar ratio of silver iodide to bismuth iodide powder is 2:1, and the concentration of the precursor solution is 0.0375-0.075 mol / L.

3. The environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to claim 1, characterized in that: In the step (2), the reaction temperature is 170-210° C. and the reaction time is 2-3 h.

4. The environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to claim 1, characterized in that: In the step (3), washing is performed using a non-toxic solvent.

5. The environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to claim 1, characterized in that: In the step (4), the slurry concentration is 0.01-0.03 mol / L.

6. The environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to claim 1, characterized in that: In the step (5), the slurry is sprayed onto a substrate placed on a heating platform at 100° C. for 25-75 seconds to form a film.

7. The environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to claim 1, characterized in that: In the step (5), low-temperature annealing is carried out in a tubular furnace in an argon atmosphere at a temperature of 120-135° C. for 10 min.

8. The environmentally friendly and low-cost method for preparing Ag2BiI5 photoelectric film according to claim 1, characterized in that: The non-toxic solvent is anhydrous ethanol.

Citation Information

Cited By

  • Preparation method of large-area CsCu2I3 perovskite photoelectric film

    CN121793498A