Precipitated silica and method thereof

By using silica with a primary particle size greater than 80nm in the toothpaste formula, the problem of poor compatibility with CPC, BAC and fragrances is solved, and a balance of cleaning and wear is achieved within the range of normal PCR and RDA values ​​in toothpaste.

CN118765261APending Publication Date: 2024-10-11EVONIK OPERATIONS GMBH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202280084500.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-08
Filing Date
2022-12-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve good compatibility with CPC, BAC and fragrances in toothpaste formulations, while failing to achieve PCR and RDA values ​​within the normal range.

Method used

By continuously adding acid and alkali metal silicates or alkaline earth metal silicates under stirring at a specific temperature and pH value to form silica with a primary particle size greater than 80 nm, the BET surface area and total mercury pressure volume are adjusted to Improve compatibility with CPC, BAC and fragrances, and be used in toothpaste.

Benefits of technology

It achieves high compatibility with CPC, BAC and fragrances in oral care applications, and achieves PCR and RDA values ​​within the normal range in toothpaste, improving the cleaning and wear balance performance of toothpaste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004902409430000101
    Figure BDA0004902409430000101
  • Figure BDA0004902409430000121
    Figure BDA0004902409430000121
  • Figure BDA0004902409430000141
    Figure BDA0004902409430000141
Patent Text Reader

Abstract

The present disclosure relates to precipitated silica characterized by a mean primary particle size greater than 80 nm, a BET surface area of 10-40 m2 / g, a total mercury injection volume of 0.75-2.00 cc / g, and an oil absorption of 60-120 cc / 100 g. The silica of the invention is produced by a process comprising (a) continuously feeding an acid and an alkali or alkaline earth metal silicate under agitation into a liquid medium at a silicate addition rate V1 and a temperature of 70-96 DEG C to form silica particles, (b) stopping feeding the alkali or alkaline earth metal silicate and the acid, (c) adding an alkali metal silicate or alkaline earth metal silicate and an acid while stirring, the silicate addition rate being 1 to 40% of the silicate addition rate V1, and during the addition of the alkali metal silicate or alkaline earth metal silicate, maintaining a constant pH value of 9.0 to 10.0 by adjusting the acid rate, (d) stopping the addition of the alkali metal silicate or alkaline earth metal silicate and adding an acid under stirring until a pH of 5.0 to 7.0 is reached. The precipitated silica of the present invention is useful in cosmetics, anti-caking free / flow, food, carrier applications, dentifrice and mouthwash.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to precipitated silica and methods of making and using the same. Background Art

[0002] Porous precipitated silica is usually prepared by the reaction of an alkaline silicate solution (e.g., sodium silicate) with an inorganic acid. Sulfuric acid is mainly used commercially, although other acids such as hydrochloric acid may also be used. Acid and sodium silicate solution are added to water simultaneously under stirring. When silica is precipitated from the dispersion due to the neutralization reaction and the generation of a byproduct sodium salt (sodium sulfate), precipitated silica is produced. Precipitated silica is composed of aggregates (secondary particles) of primary (or final) colloidal silica particles. Primary particles are mostly spherical and generally have a diameter in the range of 5 to 50 nm. The primary particles in the aggregates are covalently bonded to each other by forming siloxane bonds. Aggregates are three-dimensional clusters of these primary particles. Aggregates have a diameter of up to 500 nm. During the preparation process, aggregates are not chemically connected to form a huge gel network. Aggregates themselves can be physically connected to larger agglomerates with a diameter of up to 100 μm before grinding by forming hydrogen bonds between silanol groups on their surfaces. The median size of the agglomerates is about 20–50 μm in diameter (before grinding). The porosity and surface area of ​​these precipitated silica particles vary with the size of the primary particles and how they aggregate and agglomerate. The pores are formed by the spaces between the primary particles and the aggregates. Typical surface areas for commercial precipitated silicas are 5–800 m 2 / g. They are sold in powder form. The tamped density (which is a measure of the weight of these porous powders) is 50-500 kg / m 3 They have a high absorption capacity of about 175–320 g / 100 g.

[0003] U.S. Pat. No. 8,597,425 reports that porous precipitated silica with a primary particle size of 10-80 nm can be used in applications including rubber and tires, battery separators, anti-caking agents, matting agents for inks and paints, carriers for agricultural products and feed, coating materials, printing inks, fire extinguisher powders, plastics, non-impact printing sectors, articles in the pulp or personal care sectors, etc.

[0004] J. Soc Cosmet. Chem August 1978, 29, 497-521 reports that precipitated silica having a primary particle size of 12-51 nm can be used in cosmetic applications including toothpaste.

[0005] The commercial product SIPERNAT 22, which can be used as a carrier and anti-caking free-flowing additive in food and feed applications, is reported to have a primary particle size of 18 nm (Degussa literature No. 64, Physiological Behavior of highly dispersed Oxides of Silicon, Aluminum and Titanium 1978, page 26-27).

[0006] U.S. Patent No. 6,946,119 discloses a precipitated silica product comprising silica particles having a median diameter of 1 to 100 microns supported thereon by a surface deposit, the surface deposit comprising active precipitated amorphous silica, a silica particle having a diameter of 1 to 50 microns effective to provide the silica particles with a surface deposit having a median diameter of 1 to 100 microns. 2 The material is present in an amount of BET surface area of ​​100 g / g. Precipitated silica is used in oral care applications.

[0007] U.S. Patent No. 7,255,852 describes a precipitated silica comprising a silica particle product having a porous surface, the silica particles having a diameter less than 8 μm. 2 The cumulative surface area of ​​all pores with a diameter greater than 500 Å (as measured by mercury intrusion porosimetry) is less than about 20 m / g. 2 / g BET specific surface area, and greater than 55% cetylpyridinium chloride compatibility percentage (%CPC). Precipitated silica is used for oral care applications.

[0008] U.S. Patent No. 7,438,895 discloses an abrasive precipitated silica material having a precipitated silica coating thereon, wherein the precipitated silica coating is denser than the material to which it is applied, and wherein the coated precipitated silica material exhibits a median particle size between 5.5 and 8 microns, a particle size up to about 2.4 microns, and a particle size of about 1.5 microns. 2 / g of pore area of ​​pores with a diameter greater than 500 Å, and a cetylpyridinium chloride compatibility percentage of at least 90% after aging the material at 140°F for 7 days.

[0009] U.S20080160053 describes a method for making an abrasive silica material, wherein the method comprises the following sequential steps: reacting a first amount of a silicate and a first amount of an acid together, optionally in the presence of at least one electrolyte present in an amount of 5 to 25% (on a weight / weight basis) compared to the dry weight of the first amount of the silicate, under high shear mixing conditions to form a first silica material; and reacting a second amount of a silicate and a second amount of an acid together, optionally in the presence of at least one electrolyte present in an amount of 5 to 25% (on a weight / weight basis) compared to the dry weight of the second amount of the silicate, in the presence of the first silica material, to form a dense phase coating on the surface of the first silica material, thereby forming a silica-coated silica material; wherein the at least one electrolyte is present in either of the steps "a" or "b" or during both steps, and wherein the step "b" is optionally performed under high shear mixing conditions.

[0010] US Patent No. 10,328,002 discloses a dentifrice composition comprising: an abrasive comprising precipitated silica particles characterized by: a particle size of about 0.1 to about 9 m 2 / g range; a BET surface area in the range of about 35 to about 55 lb / ft3; an Einlehner wear value in the range of about 8 to about 25 mg loss / 100,000 revolutions; a total mercury intrusion pore volume in the range of about 0.4-1.2 cc / g; and a stannous compatibility in the range of about 70 to about 99%; wherein the abrasive contains macropores of about 1000 angstroms or more in size and lacks small pores of less than about 500-1000 angstroms in size.

[0011] WO 2018114280 describes silicon dioxide particles having: a particle size of about 0.1 to about 7 m 2 / g range; a BET surface area in the range of about 35 to about 55 lb / ft3; an Einlehner wear value in the range of about 8 to about 25 mg loss / 100,000 revolutions; a total mercury intrusion pore volume in the range of about 0.7 to about 1.2 cc / g, and a stannous compatibility in the range of about 70 to about 99%.

[0012] US20190374448 discloses a dentifrice composition comprising: a binder; a surfactant; silicon dioxide particles; wherein the silicon dioxide particles comprise: a d50 median particle size in the range of about 4 to about 25 μm; a particle size in the range of 0 to about 10 μm 2 / g range; and a total mercury intrusion pore volume in the range of about 0.2 to about 1.5 cc / g.

[0013] WO 2019238777 describes silica particles characterized by: (i) a d50 median particle size in the range of about 8 to about 20 μm; (ii) a sphericity coefficient (S80) greater than or equal to about 0.9; (iii) a particle size in the range of about 0.1 to about 8 μm. 2 / g range; (iv) a total mercury intrusion pore volume in the range of about 0.35 to about 0.8 cc / g; and (v) a loss on ignition (LOI) in the range of about 3 to about 7 wt%.

[0014] Precipitated silica provides compatibility with ingredients while providing the right balance of cleaning and abrasion, which is important in toothpaste formulations. None of the prior art addresses the lack of compatibility with other ingredients (such as CPC and BAC) and flavor compatibility, while also failing to achieve PCR (80-110) and RDA (100-220) values ​​within the normal range. Summary of the invention

[0015] The inventors of the present invention have now discovered that silica with a high primary particle size can result in high compatibility with CPC, BAC and / or flavors in oral care applications with acceptable PCR / RDA values ​​within the range of current silica cleansers.

[0016] The subject of the present invention is therefore a precipitated silica characterized by a mean primary particle size of greater than 80 nm, preferably greater than 90 nm, more preferably greater than 100 nm, still preferably greater than 110 nm, most preferably between 120 nm and 500 nm, 10-40 nm 2 / g, preferably 10-26m 2 / g, more preferably 10-23m 2 / g, most preferably 10-20m 2 / g of BET surface area, 0.75-2.00cc / g, preferably 0.80-1.80cc / g, more preferably 0.85-1.65cc / g, more preferably 0.90-1.50cc / g of total mercury intrusion volume, and 60-120cc / 100g, preferably 60-110cc / 100g, more preferably 60-100cc / 100g, most preferably 60-90cc / 100g of oil absorption.

[0017] The subject of the invention is also a method comprising:

[0018] (a) feeding an acid and an alkali metal silicate or an alkaline earth metal silicate continuously into a liquid medium under stirring at a silicate addition rate V1 and a temperature of 70-96° C. to form silica particles,

[0019] (b) stopping the feeding of alkali metal silicate or alkaline earth metal silicate and acid, and then raising the temperature to 90 to 100° C., preferably 94 to 96° C., under stirring,

[0020] (c) adding alkali metal silicate or alkaline earth metal silicate and acid under stirring, wherein the silicate addition rate is 1 to 40%, preferably 1 to 30%, more preferably 2 to 10%, still preferably 3 to 5% of the silicate addition rate V1, and during the addition of the alkali metal silicate or alkaline earth metal silicate, the pH value of 9.0 to 10.0, preferably 9.5 to 9.9, more preferably 9.6 to 9.8 is kept constant by adjusting the acid rate,

[0021] (d) The addition of alkali metal silicate or alkaline earth metal silicate is stopped and acid is added with stirring until a pH of 5.0 to 7.0, preferably 5.5 to 6.5, is reached.

[0022] A further subject of the present invention is the use of the silicas according to the invention in cosmetics, anti-caking free / flow, foods, carrier applications, dentifrices and mouthwashes. DETAILED DESCRIPTION

[0023] The precipitated silica of the present invention has a primary particle size mean greater than 80 nm, preferably greater than 90 nm, more preferably greater than 100 nm, still preferably greater than 110 nm, most preferably between 120 nm and 500 nm, 10-40 nm 2 / g, preferably 10-26m 2 / g, more preferably 10-23m 2 / g, most preferably 10-20m 2 / g of BET surface area, 0.75-2.00cc / g, preferably 0.80-1.80cc / g, more preferably 0.85-1.65cc / g, more preferably 0.90-1.50cc / g of total mercury intrusion volume, and 60-120cc / 100g, preferably 60-110cc / 100g, more preferably 60-100cc / 100g, most preferably 60-90cc / 100g of oil absorption.

[0024] The silica of the present invention has a high primary particle size.

[0025] The precipitated silica according to the present invention may have a diameter of 10-35 m 2 / g, preferably 20-30m 2 / g of CTAB surface area.

[0026] The precipitated silica according to the present invention may have a particle size of 0.40-0.80 g / cm 3 , preferably 0.48-0.75g / cm3 The bulk density.

[0027] The precipitated silica according to the invention may have an Einlehner value of less than 18 mg loss / 100 k revolutions, preferably from 3 to 18 mg loss / 100 k revolutions.

[0028] The C content of the silica according to the present invention may be lower than 3%, preferably lower than 1%, more preferably from 0% to 0.5%, most preferably from 0% to 0.1%.

[0029] The precipitated silica according to the present invention may have a primary particle size average greater than 90 nm, 10-26 nm 2 / g BET surface area, 0.75-2.00 cc / g total mercury intruded volume and 60-120 cc / 100 g oil absorption.

[0030] The precipitated silica according to the present invention may have a primary particle size average of greater than 80 nm, 10-30 nm 2 / g BET surface area, 0.80-1.80 cc / g total mercury intrusion volume and 70-110 cc / 100 g oil absorption.

[0031] The precipitated silica according to the present invention may have a primary particle size average greater than 90 nm, 10-26 nm 2 / g BET surface area, 0.80-1.80 cc / g total mercury intrusion volume and 70-110 cc / 100 g oil absorption.

[0032] The precipitated silica according to the present invention may have a primary particle size average greater than 100 nm, 10-23 nm 2 / g BET surface area, 0.75-2.00cc / g total mercury intrusion volume and 60-120cc / 100g oil absorption.

[0033] The precipitated silica according to the present invention may have a primary particle size average of greater than 80 nm, 10-30 nm 2 / g BET surface area, 0.85-1.65cc / g total mercury intrusion volume and 60-100cc / 100g oil absorption.

[0034] The precipitated silica according to the present invention may have a primary particle size average greater than 100 nm, 10-23 nm 2 / g BET surface area, 0.85-1.65cc / g total mercury intrusion volume and 60-100cc / 100g oil absorption.

[0035] The precipitated silica according to the present invention may have a primary particle size average of 120-500 nm, a primary particle size average of 10-20 nm, ...0-20 nm, a primary particle size average of 10-20 nm, a primary particle size average of 10-20 nm, a primary particle size average of 10-20 2 / g BET surface area, 0.75-2.00cc / g total mercury intrusion volume and 60-120cc / 100g oil absorption.

[0036] The precipitated silica according to the present invention may have a primary particle size average of greater than 80 nm, 10-30 nm 2 / g BET surface area, 0.90-1.50cc / g total mercury intrusion volume and 60-90cc / 100g oil absorption.

[0037] The precipitated silica according to the present invention may have a primary particle size average of 120-500 nm, a primary particle size average of 10-20 nm, ...0-20 nm, a primary particle size average of 10-20 nm, a primary particle size average of 10-20 nm, a primary particle size average of 10-20 2 / g BET surface area, 0.90-1.50cc / g total mercury intrusion volume and 60-90cc / 100g oil absorption.

[0038] The method according to the invention comprises at least four steps:

[0039] (a) continuously feeding an acid and an alkali metal silicate or an alkaline earth metal silicate into a liquid medium under stirring at a silicate addition rate V1 and a temperature of 70-96° C. to form silica particles

[0040] (b) stopping the feeding of alkali metal silicate or alkaline earth metal silicate and acid, and then raising the temperature to 90 to 100° C., preferably 94 to 96° C., under stirring,

[0041] (c) adding alkali metal silicate or alkaline earth metal silicate and acid under stirring, wherein the silicate addition rate is 1 to 40%, preferably 5 to 30%, more preferably 7 to 25%, still preferably 10 to 20% of the silicate addition rate V1, and during the addition of the alkali metal silicate or alkaline earth metal silicate, the pH value of 9.0 to 10.0, preferably 9.5 to 9.9, more preferably 9.6 to 9.8 is kept constant by adjusting the acid rate,

[0042] (d) The addition of alkali metal silicate or alkaline earth metal silicate is stopped and acid is added with stirring until a pH of 5.0 to 7.0, preferably 5.5 to 6.5, is reached.

[0043] The silica from step (d) can be filtered (e), for example in a filter press.

[0044] The silicon dioxide of step (e) can be dried (f), for example in a spray dryer.

[0045] The silica of step (f) may be ground.

[0046] Preferably 35 to 65% of the total volume of the alkali metal silicate or alkaline earth metal silicate is added during step (a).

[0047] The liquid medium in step (a) may be an alkali metal silicate or an alkaline earth metal silicate and water.

[0048] The temperature in step (a) may range from 70 to 95°C, preferably from 70 to 90°C, more preferably from 80 to 90°C.

[0049] The acid rate in step (a) may be sufficient to maintain the pH between 8.5 and 10.5, more preferably 9.5 to 10.2.

[0050] The silicate rate in step (c) may be slowed to 5 to 30%, more preferably 10 to 20% of the rate in step (a).

[0051] The alkali metal silicate in steps (a) and (c) may preferably be sodium silicate.

[0052] The silicate addition rate in step (c) may be adjusted so that the % / hr of silicate added in this step is less than 30% / hr, preferably 15 to 25% / hr, based on the total amount of silicate added during the batch. The % / hr of silicate added is calculated by: volume of silicate used in step (c) / time in hours of step (c) / volume of silicate used in step (a) and step (c)*100.

[0053] The acid in steps (a), (c) and (d) may preferably be sulfuric acid.

[0054] The time of step (c) may be 100 to 500 minutes, preferably 150 to 300 minutes.

[0055] The precipitated silica of the present invention can be produced by the method of the present invention.

[0056] The precipitated silica of the present invention can be used in cosmetics, anti-caking free / flowing, food, carrier applications, dentifrices and mouthwashes.

[0057] The precipitated silica of the present invention has improved compatibility with cetylpyridinium chloride (CPC), benzalkonium chloride (BAC) and flavors in oral care applications.

[0058] Example

[0059] The average primary particle size was determined by SEM.

[0060] Images were taken with a scanning electron microscope at a magnification of 50,000 times. The images were sputtered with platinum and care was taken so that the sputtering did not cause texturing of the particle surface, as this could be mistaken for primary structure. The images had to represent the entire sample and contain a minimum of 30 particles. The primary particles were then measured. If the particles were not completely round, the minimum diameter across each particle was used. Particles on the edges of the image that could not be fully observed should not be used. The mean and median values ​​were then calculated based on the data set.

[0061] Carbon content

[0062] Carbon content was measured on a LECO SC832 carbon / sulfur analyzer.

[0063] brightness

[0064] The silica samples were pressed into smooth-surfaced pellets and analyzed using a Technidyne Brightmeter S-5 / BC. The instrument has a dual-beam optical system where the sample is illuminated at an angle of 45° and the reflected light is observed at 0°. It complies with TAPPI test methods T452 and T646, and ASTM standard D985. The powder material was pressed into pellets of approximately 1 cm with sufficient pressure to provide a smooth surface to the pellets without loose particles or sheen.

[0065] Moisture

[0066] Moisture was determined by heating silica at 105°C for 2 hours.

[0067] BET surface area

[0068] The BET surface area of ​​the silica of the present invention is determined using a Micromeritics TriStar 3020 instrument by the BET nitrogen adsorption method of Brunaur et al., J. Am. Chem. Soc., 60, 309 (1938), which is known in the art of particulate materials such as silica and silicate materials.

[0069] Oil absorption

[0070] Oil absorption values ​​are determined using linseed oil (cc of oil absorbed per 100 g of particles) according to the rub-out method described in ASTM D281. Generally, higher oil absorption levels indicate higher structure particles, while lower values ​​generally indicate lower structure particles.

[0071] Total mercury intrusion volume

[0072] Mercury intrusion volume or total pore volume (Hg) is measured by mercury porosimetry using a Micromeritics AutoPore IV 9520 (or Micromeritics AutoPore V 9620) device. The pore diameter is calculated by the Washburn equation using a contact angle Theta (θ) equal to 130° and a surface tension gamma equal to 484 dynes / cm. Due to the effect of pressure, mercury is forced into the voids of the particles, and the volume of mercury intruded per gram of sample is calculated at each pressure setting. The total pore volume expressed herein represents the cumulative volume of mercury intruded at pressures from vacuum to 60,000 psi. The volume increment (cm 3 / g) is plotted against the pore radius or diameter corresponding to the pressure setting increment. The peak in the indentation volume relative to the pore radius or diameter curve corresponds to the mode in the pore size distribution and determines the most common pore size in the sample. Specifically, the sample size is adjusted to achieve a handle volume of 25 to 90% in a powder penetrometer with a 5 mL sphere and a handle volume of about 1.1 mL. The sample is evacuated to a pressure of 50 μm Hg and maintained for 5 minutes. Mercury fills the pores at a pressure of 4.0 to 60,000 psi, with a 10 second equilibrium time for each data collection point. The total pore volume as described above collects the volume of intra-particle porosity generated by the pore structure within each particle, as well as the volume of inter-particle porosity formed by the interstitial spacing of the filled particles under pressure. In order to better separate and measure the actual intra-particle porosity of the produced amorphous silica, the pore volume of pores <0.11 μm can be used.

[0073] Einlehner

[0074] The Einlehner AT-1000 Abrader was used as follows: (1) a pre-cleaned and dried Fourdrinier brass screen was weighed and exposed to the action of a 10% silica suspension in water for a fixed length of time, specifically 100 g of sample in 900 g of deionized water; (2) the amount of wear was then measured as milligrams of brass lost per 100,000 revolutions of the Fourdrinier screen. The result measured in mg loss was characterized as the 10% brass Einlehner (BE) wear value.

[0075] CTAB surface area

[0076] The CTAB surface area disclosed herein is determined by the absorption of CTAB (hexadecyltrimethylammonium bromide) on the silica surface, the excess separated by centrifugation, and the amount measured by titration with sodium dodecyl sulfate using a surfactant electrode. Specifically, about 0.5 g of silica particles are placed in a 250 mL beaker containing 100 mL of CTAB solution (5.5 g / L), mixed on an electric stirring plate for 1 hour, and then centrifuged at 10,000 RPM for 30 minutes. 1 mL of 10% Triton X-100 is added to 5 mL of clear supernatant in a 100 mL beaker. The pH is adjusted to 3 to 3.5 with 0.1 N HCl, and the sample is titrated with 0.01 M sodium dodecyl sulfate using a surfactant electrode (Brinkmann SUR1501-DL) to determine the end point.

[0077] Particle size

[0078] The particle size of the silicon dioxide of the present invention is measured by the angle of scattered laser light using a HORIBA laser scattering dry particle size distribution analyzer LA-960.

[0079] Water-corrected AbC values

[0080] The water absorption value was determined using an Absorptometer "C" torque rheometer from CW Brabender Instruments, Inc. A sample of about 1 / 3 cup of silica was transferred to the mixing chamber of the Absorptometer and mixed at 150 RPM. Water was then added at a rate of 6 mL / min, and the torque required to mix the powder was recorded. The torque reaches a maximum value when the powder changes from free flowing to a paste as the water is absorbed by the powder. The total volume of water added when the maximum torque is reached is then standardized to the amount of water that 100 g of powder can absorb. Since the powder is used on an as is basis (not pre-dried), the free moisture value of the powder is used to calculate the "water-corrected water AbC value" by the following equation.

[0081]

[0082] 5 wt% pH

[0083] 5% pH was measured by weighing 5.0 g of sample (accurate to 0.1 g) and transferring the weighed sample into a 250 mL beaker. 95 mL of DI water was added and the sample was stirred for 5 minutes. The pH was then measured with a pH meter while the sample was stirred.

[0084] Bulk density and pouring density

[0085] The sample of 20.0g is put into the 250mL graduated cylinder with flat rubber bottom to measure bulk density and pour density.Record initial volume and be used for calculating pour density by the weight of used sample divided by this volume.Then graduated cylinder is placed on the tap density machine that rotates on cam with specific RPM.Cam is designed to raise and lower the distance of 5.715cm by graduated cylinder per second, until sample volume is constant, usually lasts 15 minutes.Record this final volume and be used for calculating bulk density by the weight of used sample divided by this volume.

[0086] Example 1A: (Inventive Example)

[0087] 383 mL of sodium silicate (2.65 MR, 1.193 g / mL) and 957 mL of water were added to a 7 L laboratory scale reactor and heated to 85° C. with stirring at 350 RPM from an overhead stirrer equipped with a propeller blade. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 39.0 mL / min and 16.4 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) was added at 10.2 mL / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 150 minutes. After this additional 150 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 5.1 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and dried at 105°C overnight.

[0088] Example 1B: (Inventive Example)

[0089] 273 mL of sodium silicate (2.65 MR, 1.193 g / mL) and 681 mL of water were added to a 7 L laboratory scale reactor and heated to 85° C. with stirring at 350 RPM from an overhead stirrer equipped with a propeller blade. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 27.7 mL / min and 11.7 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) was added at 10.7 mL / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 210 minutes. After the additional 210 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 5.1 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and dried at 105°C overnight.

[0090] Example 1C: (Inventive Example)

[0091] 273 mL of sodium silicate (2.65 MR, 1.193 g / mL) and 681 mL of water were added to a 7 L laboratory scale reactor and heated to 85° C. with stirring at 350 RPM from an overhead stirrer equipped with a propeller blade. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 43.8 mL / min and 18.4 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) was added at 9.8 mL / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 120 minutes. After the additional 120 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 4.7 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and dried at 105°C overnight.

[0092] Example 2A: (Inventive Example)

[0093] 320 mL of sodium silicate (2.65 MR, 1.193 g / mL) and 824 mL of water were added to a 7 L laboratory scale reactor and heated to 85° C. with stirring at 350 RPM from an overhead stirrer equipped with a propeller blade. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 33.8 mL / min and 15.1 mL / min, respectively, for 47 minutes. After 47 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL) was added at 10.4 mL / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 150 minutes. After this additional 150 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 5.0 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and dried at 105°C overnight.

[0094] Table 1 shows the analysis values ​​of Examples.

[0095] Table 1

[0096]

[0097] Comparative Example 5A:

[0098] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 85° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 25.3 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 25.3 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0099] Comparative Example 5B:

[0100] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 85° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 21.6 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 21.6 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0101] Comparative Example 5C:

[0102] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 85° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 29.2 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 29.2 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0103] Comparative Example 5D:

[0104] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 85° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 29.2 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 29.2 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0105] Comparative Example 5E:

[0106] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 85° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 19.1 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 19.1 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0107] Table 2 shows the analytical values ​​of Examples.

[0108] Table 2

[0109]

[0110] Comparative Example 6A

[0111] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 80° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 21.6 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 21.6 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0112] Comparative Example 6B

[0113] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 85° C.) and 1483 mL of water were added to a 7 L reactor and heated to 90° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 85° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 21.6 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 21.6 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0114] Comparative Example 6C

[0115] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 90° C.) and 1483 mL of water were added to a 7 L reactor and heated to 95° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 90° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 21.6 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 21.6 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0116] Table 3 shows the analytical values ​​of Examples.

[0117] Table 3

[0118]

[0119] Comparative Example 7A:

[0120] 594 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1483 mL of water were added to a 7 L reactor and heated to 85° C. with stirring at 650 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 60.4 mL / min and 25.4 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 25.4 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0121] Table 4 shows the analytical values ​​of Examples.

[0122] Table 4

[0123]

[0124] Comparative Example 8A

[0125] 510 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1310 mL of water were added to a 7 L reactor and heated to 80° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 53.7 mL / min and 24.0 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 24.0 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0126] Comparative Example 8B

[0127] 510 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1310 mL of water were added to a 7 L reactor and heated to 80° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 53.7 mL / min and 27.5 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 27.5 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0128] Comparative Example 8C

[0129] 510 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1310 mL of water were added to a 7 L reactor and heated to 80° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 53.7 mL / min and 20.4 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 20.4 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0130] Comparative Example 8D

[0131] 510 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1310 mL of water were added to a 7 L reactor and heated to 80° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 53.7 mL / min and 19.2 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 19.2 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0132] Comparative Example 8E

[0133] 510 mL of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 1310 mL of water were added to a 7 L reactor and heated to 80° C. with stirring at 350 RPM. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 53.7 mL / min and 18.0 mL / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 18.0 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed with 14 L of water and oven dried overnight.

[0134] Table 5 shows the analytical values ​​of Examples.

[0135] Table 5

[0136]

[0137] Example 10A: (Inventive Example)

[0138] 62 L of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 154 L of water were added to the 1200 L reactor and heated to 85° C. with stirring at 80 RPM and recirculation at 80 L / min. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 6.27 L / min and 2.24 L / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) was added at 1.63 L / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 150 minutes. After the additional 150 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 0.82 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed until the conductivity was <1500 μS, spray dried to a target moisture of 5%, and ground to a particle size of approximately 10 μm.

[0139] Example 10B: (Inventive Example)

[0140] 53 L of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 133 L of water were added to the 1200 L reactor and heated to 85° C. with stirring at 80 RPM and recirculation at 80 L / min. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 5.42 L / min and 1.82 L / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) was added at 1.63 L / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 180 minutes. After the additional 180 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 0.82 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed until the conductivity was <1500 μS, spray dried to a target moisture of 5%, and ground to a particle size of approximately 10 μm.

[0141] Example 10C: (Inventive Example)

[0142] 44 L of sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and 115 L of water were added to the 1200 L reactor and heated to 85° C. with stirring at 80 RPM and recirculation at 80 L / min. Once 85° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) and sulfuric acid (1.121 g / mL) were added simultaneously at rates of 4.48 L / min and 1.51 L / min, respectively, for 38 minutes. After 38 minutes, the flow of sodium silicate and sulfuric acid was stopped and the reaction mixture was heated to 95° C. Once 95° C. was reached, sodium silicate (2.65 MR, 1.193 g / mL, heated to 80° C.) was added at 1.73 L / min and sulfuric acid (1.121 g / ml) was added at a rate sufficient to maintain pH 9.6 (+ / - 0.1) for an additional 210 minutes. After the additional 210 minutes, the flow of sodium silicate was stopped and the pH was adjusted to pH 6.0 by continuing to flow sulfuric acid (1.121 g / mL) at a rate of 0.82 mL / min. Once the pH stabilized at pH 6.0, the batch was filtered, washed until the conductivity was <1500 μS, spray dried to a target moisture of 5%, and ground to a particle size of approximately 10 μm.

[0143] Tables 6a and 6b show the analytical values ​​for the Examples.

[0144] Table 6a

[0145]

[0146] Table 6b

[0147]

[0148] Example 11: Toothpaste formulation

[0149] The inventive silica from above was incorporated into toothpaste for rheology and PCR / RDA measurements. The formulation and results (Table 7a) are shown below. The stannous compatibility and fluoride compatibility of the inventive examples are shown in Table 7b.

[0150] Table 7a

[0151]

[0152] (PCR / RDA run at Indiana University School of Dentistry)

[0153] Table 7b

[0154]

[0155] The data in Table 7a show that toothpastes containing silica of the present invention achieve PCR and RDA values ​​within the normal range.

[0156] Stannous compatibility (%)

[0157] The stannous compatibility of the above samples was determined as follows. A stock solution containing 431.11 g of 70% sorbitol, 63.62 g of deoxygenated deionized water, 2.27 g of stannous chloride dihydrate and 3 g of sodium gluconate was prepared. 34 g of the stock solution was added to a 50 mL centrifuge tube containing 6 g of the silica sample to be tested. The centrifuge tube was placed on a rotating wheel at 5 RPM and aged at 40° C. for 1 week. After aging, the centrifuge tube was centrifuged at 12,000 RPM for 10 minutes, and the stannous concentration in the supernatant was determined by ICP-OES (inductively coupled plasma emission spectrometer). Stannous compatibility is determined by expressing the stannous concentration of the sample as a percentage of the stannous concentration of a solution prepared by the same procedure but without the addition of silica.

[0158] Fluoride compatibility (%)

[0159] The fluoride compatibility of the above samples was determined as follows. A fluoride stock solution containing 1624ppm was prepared. 30.0g of the stock solution was added to a 50mL centrifuge tube containing 7.0g of the silica sample to be tested. The centrifuge tube was placed on a rotating wheel at 5RPM (or equivalent stirring mode) and aged for 1 hour at 60°C. After aging, the centrifuge tube was centrifuged at 12,000RPM for 10 minutes (or until the supernatant was clear). The fluoride concentration in the supernatant was determined by first taking an aliquot and transferring it to a plastic bottle containing a magnetic stirring bar and an equal volume of TISAB II buffer. The concentration was then measured using a pre-calibrated fluoride specific ion electrode (Orion model #96-09BN or equivalent). Fluoride compatibility was determined by expressing the fluoride concentration of the sample as a percentage of the fluoride concentration of the stock solution.

[0160] Relative dentin wear (RDA)

[0161] The RDA values ​​of the dentifrice compositions of Examples DC1-DC14 containing the silica of the present invention were determined according to the method set forth in Hefferen, Journal of Dental Res., July-August 1976, 55(4), pp. 563-573 and described in Wason U.S. Pat. Nos. 4,340,583, 4,420,312, and 4,421,527, the contents of which are incorporated herein by reference in their entirety.

[0162] Biofilm Cleaning Ratio (“PCR”)

[0163] The cleaning performance of a dentifrice composition is usually expressed as a Pellicle Cleaning Ratio ("PCR") value. The PCR test measures the ability of a dentifrice composition to remove bacterial film from teeth under fixed brushing conditions. The PCR test is described in "In Vitro Removal of Stain with Dentifrice" GK Stookey, et al., J. Dental Res., 61, 12-36-9, 1982. Both PCR and RDA results vary depending on the nature and concentration of the components of the dentifrice composition. PCR and RDA values ​​are unitless.

[0164] Example 12: CPC and BAC Compatibility

[0165] In order to determine the given silica capacitance (capacity) for quaternary ammonium compounds, a zeta potential titration was performed. In the titration, a 5 wt% suspension of the desired silica was prepared by taking the required amount of dry silica and diluting it to 160 g with deionized water. In order to get as close as possible to the required 5 wt% (8 g) of silica in 160 g of suspension, the amount of raw silica used was adjusted to compensate for the amount of free moisture (drying loss) and sodium sulfate present. The suspension was magnetically stirred at 500 rpm for 10 minutes to completely wet the silica, and then the suspension was adjusted to a pH of ~8.5 with 0.5 M NaOH or 0.5 M HCl to help consistency of initial surface chemistry and more direct comparison.

[0166] The suspension was then titrated with 0.25 mL increments of 5 wt% cetylpyridinium chloride (CPC) or 5 wt% benzalkonium chloride (BAC), and the capacitance of each silica was determined by the volume of CPC or BAC required to reach a zeta potential of 0 mV. Given that most experiments showed artifacts near the 0 mV crossover point, the capacitance was defined as the first point at which the zeta potential became positive. The volume at this point was then used to determine the mass of CPC or BAC per gram of silica in mg / g.

[0167] Inventive Examples 10A, 10B and 10C showed lower CPC and BAC values ​​and therefore showed improved CPC / BAC compatibility (Table 8).

[0168] Table 8

[0169]

[0170] Example 13: Fragrance

[0171] Method: 500 mg of silica was placed in a headspace vial. 10 μL of flavor (lime oil, Lot MKCF9356 flavor matrix) was added and the headspace vial was equilibrated overnight. The samples were incubated at 60°C with gentle shaking for 60 minutes before sampling the headspace vial. 1 mL of headspace was analyzed in a GC / MS equipped with a Stabilwax column (0.25 mm x 60 m) with a column flow rate of 1.606 mL / min and a temperature gradient of 6°C / min over the temperature range of 40°C to 230°C (HS sampling: 1 mL of headspace was sampled into a gas-tight syringe at 65°C). Peak areas relative to The peak intensity of 113 was normalized.

[0172] Inventive Examples 10A, 10B and 10C show higher values ​​and therefore show improved fragrance compatibility (Table 9).

[0173] Table 9

[0174]

Claims

1. A precipitated silica, It is characterized in that The average primary particle size is greater than 80 nm, preferably greater than 90 nm, more preferably greater than 100 nm, still preferably greater than 110 nm, most preferably between 120 nm and 500 nm, 10-40 nm 2 / g, preferably 10-26m 2 / g, more preferably 10-23m 2 / g, most preferably 10-20m 2 / g of BET surface area, 0.75-2.00cc / g, preferably 0.80-1.80cc / g, more preferably 0.85-1.65cc / g, more preferably 0.90-1.50cc / g of total mercury intrusion volume, and 60-120cc / 100g, preferably 60-110cc / 100g, more preferably 60-100cc / 100g, most preferably 60-90cc / 100g of oil absorption.

2. The precipitated silica according to claim 1, wherein the precipitated silica has a 2 / g, preferably 20-30m 2 / g of CTAB surface area.

3. The precipitated silica according to claim 1 or 2, wherein the precipitated silica has a carbon content of 0.40-0.80 g / cm 3 , preferably 0.48-0.75g / cm 3 The bulk density.

4. The precipitated silica according to any one of claims 1 to 3, wherein the precipitated silica has an Einlehner value of less than 18 mg loss / 100k revolutions, preferably 3 to 18 mg loss / 100k revolutions.

5. The precipitated silica according to any one of claims 1 to 4, wherein the precipitated silica has a C content of less than 3%, preferably less than 1%, more preferably from 0% to 0.5%.

6. The precipitated silica of claim 1, wherein the precipitated silica has a primary particle size mean greater than 90 nm, a primary particle size of 10-26 ... 2 / g BET surface area, 0.75-2.00cc / g total mercury intrusion volume and 60-120cc / 100g oil absorption.

7. The precipitated silica of claim 1, wherein the precipitated silica has a primary particle size average greater than 80 nm, a primary particle size of 10-30 nm, a primary particle size of 10-30 nm, a primary particle size of 2 ...20-30 nm, a primary particle size of 20-30 nm, a primary 2 / g BET surface area, 0.80-1.80 cc / g total mercury intrusion volume and 70-110 cc / 100 g oil absorption.

8. The precipitated silica of claim 1, wherein the precipitated silica has a primary particle size mean greater than 90 nm, a primary particle size of 10-26 ... 2 / g BET surface area, 0.80-1.80 cc / g total mercury intrusion volume and 70-110 cc / 100 g oil absorption.

9. The precipitated silica of claim 1, wherein the precipitated silica has a primary particle size mean greater than 100 nm, a primary particle size of 10-23 ... 2 / g BET surface area, 0.75-2.00cc / g total mercury intrusion volume and 60-120cc / 100g oil absorption.

10. The precipitated silica of claim 1, wherein the precipitated silica has a primary particle size average greater than 80 nm, a primary particle size of 10-30 nm, a primary particle size of 10-30 nm, a primary particle size of 2 ...20-30 nm, a primary particle size of 20-30 nm, a 2 / g BET surface area, 0.85-1.65cc / g total mercury intrusion volume and 60-100cc / 100g oil absorption.

11. The precipitated silica of claim 1, wherein the precipitated silica has a primary particle size mean greater than 100 nm, a primary particle size of 10-23 ... 2 / g BET surface area, 0.85-1.65cc / g total mercury intrusion volume and 60-100cc / 100g oil absorption.

12. A method for producing precipitated silica, comprising: (a) feeding an acid and an alkali metal silicate or an alkaline earth metal silicate continuously into a liquid medium under stirring at a silicate addition rate V1 and a temperature of 70-96° C. to form silica particles, (b) stopping the feeding of alkali metal silicate or alkaline earth metal silicate and acid, and then raising the temperature to 90 to 100° C., preferably 94 to 96° C., under stirring, (c) adding an alkali metal silicate or an alkaline earth metal silicate and an acid under stirring, wherein the silicate addition rate is 1 to 40%, preferably 1 to 30%, more preferably 2 to 10%, still preferably 3 to 5% of the silicate addition rate V1, and during the addition of the alkali metal silicate or alkaline earth metal silicate, the pH value of 9.0 to 10.0, preferably 9.5 to 9.9, more preferably 9.6 to 9.8 is kept constant by adjusting the acid rate, (d) The addition of alkali metal silicate or alkaline earth metal silicate is stopped and acid is added with stirring until a pH of 5.0 to 7.0, preferably 5.5 to 6.5, is reached.

13. The process for producing precipitated silica according to claim 12, wherein the silica of step (d) is filtered (e) and dried in a spray dryer (f).

14. The process for producing precipitated silica according to claim 13, wherein the silica of step (f) is ground.

15. The method for producing precipitated silica according to claim 12, wherein the liquid medium in step (a) is an alkali metal silicate or an alkaline earth metal silicate and water.

16. The method for producing precipitated silica according to claim 12, wherein the temperature in step (a) ranges from 70 to 95°C, preferably from 70 to 90°C, more preferably from 80 to 90°C.

17. The method for producing precipitated silica according to claim 12, wherein the time period of step (c) is 100 to 500 minutes, preferably 150 to 300 minutes.

18. Use of the precipitated silica as claimed in claim 1 for cosmetics, anti-caking free / flowing, food, carrier applications, dentifrices and mouthwashes.

19. A dentifrice composition comprising the precipitated silica of any of claims 1-11.

Citation Information

Cited By

  • Precipitated silica having low BET specific surface area, composition containing same, and method for producing precipitated silica

    CN121969571A