Compositions, methods, and systems related to multimodal distribution of vaterite particles
By using bimodal or multimodal compositions of reactive aragonite cement, the shortcomings of cement materials in terms of fluidity and strength are addressed, providing environmentally friendly high-performance concrete and mortar solutions.
Patent Information
- Application Number
- CN202280085787.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-22
- Filing Date
- 2022-12-21
- Publication Date
- 2024-10-11
AI Technical Summary
Existing cement materials have problems such as being environmentally unfriendly, having insufficient strength, and poor workability during production and use, especially in concrete and mortar where it is difficult to achieve ideal control over fluidity and consistency.
A bimodal or multimodal composition of reactive aragonite cement is used, which is mixed with reactive aragonite cement particles of different sizes to form cement, concrete and mortar materials with high fluidity and high strength. The difference in particle size distribution is used to improve filling density and fluidity, and Portland cement is combined to enhance performance.
It has achieved an environmentally friendly high-strength cement material with good workability and fluidity, suitable for concrete and mortar, improving construction efficiency and product performance.
Smart Images

Figure CN118765268A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Application No. 63 / 292,897, filed on December 22, 2021, which is incorporated by reference in its entirety into the disclosure of the present invention herein.
[0003] background
[0004] Carbon dioxide (CO 2 ) emissions have been identified as the main cause of global warming. 2 is a byproduct of combustion and it creates operational, economic and environmental problems. 2 Increased atmospheric concentrations of CO and other greenhouse gases can contribute to the storage of more heat in the atmosphere, leading to increased surface temperatures and rapid climate change. 2 dissolution and formation of carbonic acid, atmospheric CO 2 Increased levels of CO2 could also further acidify the world’s oceans. Reducing the potential risks of climate change requires storing and avoiding CO2 from a variety of anthropogenic processes. 2 Concrete is the second most consumed product on Earth after water, and cement production accounts for 1.3% of the world’s CO 2 Emissions are as high as 8%. Cementitious materials need to be properly selected to make them environmentally friendly, durable, blended for optimal efficiency, and properly controlled to produce consistent concrete strength, workability, finish, and durability.
[0005] Overview
[0006] Provided herein are compositions, methods and systems related to preparing compositions comprising a bimodal or multimodal (e.g., trimodal or higher) distribution of reactive vaterite cement, which produces cement, concrete and mortar materials that are environmentally friendly and have high workability, strength and durability.
[0007] In one aspect, a cement composition is provided, comprising: a bimodal distribution of reactive vaterite cements comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm and reactive vaterite cement B having an average particle size between about 11 μm-50 μm.
[0008] In one aspect, a cement composition is provided, comprising: a trimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and reactive vaterite cement C having an average particle size between about 51 μm-100 μm.
[0009] In some embodiments of the aforementioned aspects, reactive vaterite cement A is between about 5%-95% by weight in the composition, and reactive vaterite cement B is between about 5%-95% by weight in the composition. In some embodiments of the aforementioned aspects and embodiments, reactive vaterite cement A is between about 5%-75% by weight in the composition, and reactive vaterite cement B is between about 25%-95% by weight in the composition. In some embodiments of the aforementioned aspects and embodiments, reactive vaterite cement A is between about 5%-40% by weight; reactive vaterite cement B is between about 25%-50% by weight; and reactive vaterite cement C is between about 5%-10% by weight. In some embodiments of the aforementioned aspects and embodiments, the composition increases the packing density of cement paste in water between about 1%-35%. In some embodiments of the aforementioned aspects and embodiments, the reactive vaterite cement A in the composition increases the packing density of cement paste in water by about 1%-35%. In some embodiments of the aforementioned aspects and embodiments, the composition reduces the viscosity of cement paste in water by about 10%-50%. In some embodiments of the aforementioned aspects and embodiments, the reactive vaterite cement B and / or reactive vaterite cement C in the composition reduce the viscosity of cement paste in water by about 10%-50%. In some embodiments of the aforementioned aspects and embodiments, bimodal composition or trimodal composition provides a paste viscosity in water between about 800mPa*s-1600mPa*s. In some embodiments of the aforementioned aspects and embodiments, the ratio of reactive vaterite cement A: reactive vaterite cement B is between about 1:20-20:1. In some embodiments of the aforementioned aspects and embodiments, reactive vaterite cement A has a viscosity of about 4,000mPa*s. 2 / kg-40,000m 2 / kg, and the reactive vaterite cement B has a specific surface area of about 100m 2 / kg-6,000m 2 In some embodiments of the aforementioned aspects and embodiments, the reactive vaterite cement A and the reactive vaterite cement B (as well as the reactive vaterite cement C in trimodal or multimodal distribution) have a spherical morphology.
[0010] In some embodiments of the aforementioned aspects and embodiments, the composition further comprises Portland cement to form a blended cement composition. In some embodiments of the aforementioned aspects and embodiments, the composition further comprises Portland cement to form a blended cement composition. 2 / kg-40,000m 2 In some embodiments of the aforementioned aspects and embodiments, the reactive vaterite cement A of the blended composition with a specific surface area between 100-2000 mPa*s and 1600 mPa*s provides a high surface area to nucleate calcium silicate hydrate and dissolve portland cement in water. In some embodiments of the aforementioned aspects and embodiments, the reactive vaterite cement A in the blended composition increases the packing density of cement paste in water between about 1%-35%. In some embodiments of the aforementioned aspects and embodiments, the reactive vaterite cement B and / or reactive vaterite cement C in the blended composition reduce the viscosity of cement paste in water by about 10%-50%. In some embodiments of the aforementioned aspects and embodiments, the bimodal distribution and / or trimodal distribution in the blended cement composition provides a paste viscosity in water between about 800 mPa*s-1600 mPa*s.
[0011] In some embodiments of the aforementioned aspects and embodiments, reactive vaterite cement A and / or reactive vaterite cement B also include magnesium oxide. In some embodiments of the aforementioned aspects and embodiments, cement composition also includes aluminosilicate material. In some embodiments of the aforementioned aspects and embodiments, aluminosilicate material includes heat-treated clay, natural volcanic ash or artificial volcanic ash, shale, granulated blast furnace slag or its combination. In some embodiments of the aforementioned aspects and embodiments, heat-treated clay includes calcined clay, aluminosilicate glass, calcium aluminosilicate glass or its combination. In some embodiments of the aforementioned aspects and embodiments, pozzolan is selected from the group consisting of fly ash, volcanic ash (volcanic ash) and its mixture. In some embodiments of the aforementioned aspects and embodiments, cement composition also includes slag from metal production, portland cement clinker, calcium aluminate cement clinker and / or calcium sulphoaluminate cement clinker. In some embodiments of the aforementioned aspects and embodiments, cement composition also includes carbonate material, and the carbonate material includes limestone, calcium carbonate, magnesium carbonate, calcium magnesium carbonate or its combination. In some embodiments of the aforementioned aspects and embodiments, cement composition also includes alkali metal accelerator or alkaline earth metal accelerator.In some embodiments of the aforementioned aspects and embodiments, alkali metal accelerator or alkaline earth metal accelerator is selected from sodium sulfate, sodium carbonate, sodium nitrate, sodium nitrite, sodium hydroxide, potassium sulfate, potassium carbonate, potassium nitrate, potassium nitrite, potassium hydroxide, lithium sulfate, lithium carbonate, lithium nitrate, lithium nitrite, lithium hydroxide, calcium sulfate, calcium nitrate, calcium nitrite and combination thereof.In some embodiments of the aforementioned aspects and embodiments, composition includes by weight the composition including reactive vaterite cement between about 5%-50%, the heat-treated clay between about 5%-40%, the limestone between about 0-10% and the portland cement clinker between about 15%-90%.In some embodiments of the aforementioned aspects and embodiments, composition after solidification and hardening has the 28-day compressive strength of at least 21MPa. In some embodiments of the aforementioned aspects and embodiments, the cement composition further comprises an admixture selected from the group consisting of: setting accelerators, setting retardants, air entraining agents, foaming agents, defoamers, alkali reactivity reducers, bonding admixtures, dispersants, coloring admixtures, corrosion inhibitors, moisture-proof admixtures, gas forming agents, permeability reducers, pumping aids, shrinkage compensating admixtures, fungicidal admixtures, bactericidal admixtures, insecticide admixtures, rheology modifiers, finely divided mineral admixtures, volcanic ash, aggregates, wetting agents, strength enhancers, waterproofing agents, reinforcing materials, and combinations thereof. In some embodiments of the aforementioned aspects and embodiments, the reinforcing material is a fiber selected from the group consisting of zirconium oxide-containing materials, aluminum, glass, steel, carbon, ceramics, grass, bamboo, wood, glass fiber, synthetic materials, and combinations thereof.
[0012] In one aspect, a concrete mixture is provided, the concrete mixture comprising the above-mentioned cement composition.
[0013] In one aspect, a cement paste or cement slurry composition is provided, the cement paste or cement slurry composition comprising: reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and optionally reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water; and interlocking acicular shapedaragonite. In some embodiments of the foregoing aspects, the cement paste or cement slurry composition further comprises Portland cement. In some embodiments of the foregoing aspects and embodiments, the cement paste or cement slurry composition comprises Portland cement having an average particle size between about 4,000 μm and about 100 μm. 2 / kg-40,000m 2 In some embodiments of the aforementioned aspects and embodiments, reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C provide a paste viscosity between about 800mPa*s-1600mPa*s. In some embodiments of the aforementioned aspects and embodiments, cement paste or cement slurry compositions also include aluminosilicate material (for example, heat-treated clay) and carbon aluminate.
[0014] In one aspect, a cement product is provided, comprising: an interlocking needle-like aragonite microstructure. In some embodiments of the foregoing aspects, the interlocking needle-like aragonite surrounds one or more voids. In some embodiments of the foregoing aspects and embodiments, the interlocking needle-like aragonite surrounding one or more voids forms a honeycomb structure.
[0015] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the mixture comprising lime in an N-containing salt solution to produce an aqueous solution comprising a calcium salt; and (c) treating the aqueous solution comprising the calcium salt with a gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0016] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the mixture comprising lime in an N-containing salt solution to produce an aqueous solution comprising a calcium salt; (c) treating the aqueous solution comprising the calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; and treating the aqueous solution comprising the calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; (d) mixing the composition comprising reactive vaterite cement A and the composition comprising reactive vaterite cement B to form a composition comprising a bimodal distribution of reactive vaterite cements, wherein the bimodal distribution of reactive vaterite cements comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0017] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) dissolving limestone in an N-containing salt solution to produce an aqueous solution comprising a calcium salt and a gas stream comprising carbon dioxide; and (b) treating the aqueous solution comprising a calcium salt with the gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0018] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) dissolving limestone in an N-containing salt solution to produce an aqueous solution containing a calcium salt and a gas stream containing carbon dioxide; (b) treating the aqueous solution containing the calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; and treating the aqueous solution containing the calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; (c) mixing the composition containing reactive vaterite cement A and the composition containing reactive vaterite cement B to form a composition containing a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement contains reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0019] In some embodiments of the aforementioned aspects and embodiments, the method also includes adding water to the cementitious composition and converting reactive vaterite cement A and reactive vaterite cement B into interlocking needle-shaped aragonite and / or optionally local calcite when dissolving and reprecipitating in water. In some embodiments of the aforementioned aspects and embodiments, the method also includes making aragonite and / or calcite solidify and harden and form cement products. In some embodiments of the aforementioned aspects and embodiments, the cement products have a hardness of about 25lb / ft 3 -200lb / ft 3 The packing density between.
[0020] In some embodiments of the aforementioned aspects and embodiments, reactive vaterite cement A and / or reactive vaterite cement B improves or increases the packing density of the cement paste by between about 1%-35% and / or reduces the viscosity of the cement paste by 10% or more or between 10%-50%.
[0021] In one aspect, a system for forming a composition is provided, the system comprising:
[0022] (i) a calcining reactor configured to calcine limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide;
[0023] (ii) a dissolution reactor operably connected to the calcination reactor, the dissolution reactor being configured for dissolving a mixture comprising lime in an aqueous N-containing brine solution to produce an aqueous solution comprising a calcium salt;
[0024] (iii) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured to treat an aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0025] In one aspect, a system for forming a composition is provided, the system comprising:
[0026] (i) a calcining reactor configured to calcine limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide;
[0027] (ii) a dissolution reactor operably connected to the calcination reactor, the dissolution reactor being configured for dissolving a mixture comprising lime in an aqueous N-containing brine solution to produce an aqueous solution comprising a calcium salt;
[0028] (iii) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured for treating an aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm;
[0029] (iv) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured for treating an aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; and
[0030] (v) a mixing reactor operably connected to the treatment reactor, the mixing reactor being configured to mix a composition comprising reactive vaterite cement A and a composition comprising reactive vaterite cement B to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0031] Attached photos
[0032] The features of the present invention are particularly set forth in the appended claims. A better understanding of the features and advantages of the present invention will be obtained by referring to the following detailed description and the accompanying drawings, which set forth illustrative embodiments utilizing the principles of the present invention, wherein:
[0033] Figure 1 The figures illustrate some embodiments of the compositions, methods, and systems provided herein relating to unimodal, bimodal, trimodal, or multimodal distributions of reactive vaterite cement particles.
[0034] Figure 2A The figures illustrate some embodiments of the methods and systems provided herein that employ the calcination of limestone to form a reactive vaterite cement composition.
[0035] Figure 2B The figures illustrate some embodiments of the methods and systems provided herein that directly employ limestone to form a reactive vaterite cement composition.
[0036] Figure 3A The figures illustrate some embodiments of the methods and systems provided herein that employ the calcination of limestone to form a reactive vaterite cement composition.
[0037] Figure 3BThe figures illustrate some embodiments of the methods and systems provided herein that directly employ limestone to form a reactive vaterite cement composition.
[0038] Figure 4A The figures illustrate some embodiments of the methods and systems provided herein that employ the calcination of limestone to form a reactive vaterite cement composition.
[0039] Figure 4B The figures illustrate some embodiments of the methods and systems provided herein that directly employ limestone to form a reactive vaterite cement composition.
[0040] Figure 5 The figure shows a SEM image of an aragonite needle microstructure as provided in Example 1 herein.
[0041] Figure 6 The figure shows a SEM image of aragonite needle-like microstructures surrounding one or more voids to form a honeycomb structure as provided in Example 2 herein.
[0042] Figure 7 The figure shows the effect of bimodal distribution on the flow of mortar, as described in Example 3 herein.
[0043] Figure 8 The figure shows the effect of bimodal distribution on compressive strength, as described in Example 3 herein.
[0044] Fig. 9 The graph shows the particle size distribution of Portland cement; the particle size distribution of a unimodal reactive vaterite mixture used to produce a blended cement mixture; and the particle size distribution of a multimodal blend (B1 ), as described in Example 4.
[0045] Fig.10 The graph shows the paste viscosity as a function of the surface area of the cement blended, as described in Example 4.
[0046] describe
[0047] Disclosed herein are bimodal distribution and / or multimodal distribution comprising reactive vaterite cement particles, unique compositions, methods and systems related to compositions of for example trimodal distribution or more peak distributions, bimodal distribution and / or multimodal distribution of reactive vaterite cement particles, for example trimodal distribution or more peak distributions produce cement, concrete and mortar materials with environmental friendliness and high workability, strength and durability. "Unimodal distribution" as used herein includes materials with identical median particle size or average particle size, span or other particle size distribution characteristics. "Bimodal distribution" as used herein includes a combination of two materials, and these two materials have different median particle size or average particle size, span or other particle size distribution characteristics that distinguish them. "Trimodal distribution" as used herein includes a combination of three materials, and the three materials have different median particle size or average particle size, span or other particle size distribution characteristics that distinguish them. "Multimodal distribution" as used herein includes a combination of three or more materials, and the three or more materials have different median particle size or average particle size, span or other particle size distribution characteristics that distinguish them.
[0048] I. Composition
[0049] Typically, when making cement, concrete or mortar; consistency, setting time and fluidity may play an important role. For example, the consistency of a cement mixture plays a role in the performance of the mixture when poured through the reinforcement in the formwork and the time required for the mortar or concrete to set. A consistency test can be performed to assess the amount of water required to form a paste of normal consistency, which is defined as the percentage of water demand for the cement paste. When water is added to cement, the resulting paste may begin to harden and gain compressive strength. By way of example only, the Vicat needle test can measure the time taken for a cement-water mixture to harden or set. Consistency can be measured by a Vicat test, which provides both an initial setting time and a final setting time—measurements that can be considered as two hardening states of cement. The beginning or initial setting of curing can mark the point in time when the paste becomes unusable, and the time taken to fully cure marks the final setting. This requires a sufficiently short time so that construction activities can resume within a reasonable time after placing the concrete. The determination of consistency can also be performed by using a flow bench test device. The cement paste may act as a separator for the aggregate in the mortar, and a lack of sufficient mortar may result in a mixture with limited flow. Such a mixture may be prone to segregation and may be difficult to finish. Therefore, it is desirable for the cement paste, mortar or concrete to have sufficient fluidity, because if the paste has too much fluidity, it may take too long to set, and if the fluidity is too low, the paste is difficult to work with and may result in premature hardening.
[0050] Provided herein are compositions, methods and systems relevant to some particle distribution mixtures of reactive vaterite cement with different median particle diameters or mean particle diameters, to improve the reactivity and fluidity of cement, concrete or mortar.Applicant surprisingly and unexpectedly find that the reactive vaterite cement particles mixing some particle diameters cause high reactivity of cement setting and hardening and high fluidity and workability (example provided herein) of cement paste, concrete or mortar.Applicant also surprisingly finds that the particle distribution of reactive vaterite cement particles and median particle diameter affect the packed density or bulk density of cement products in the composition, make by using particle distribution and median particle diameter of the expectation of reactive vaterite cement particles in the composition, can form cement products with packed density or bulk density scope.
[0051] " reactive vaterite " or " reactive vaterite cement " as used interchangeably herein comprise vaterite material, it is converted into interlocking needle-like aragonite and / or calcite and / or carbon aluminate during and / or after dissolving-reprecipitation process in water, and solidifies and hardens into cement product.In some embodiments, reactive vaterite cement provided herein has spherical morphology.Carboaluminate or carbon aluminate hydrate include but are not limited to single carbon aluminate, half carbon aluminate or its combination.
[0052] The applicant unexpectedly and surprisingly found that the unimodal particle distribution of the reactive vaterite cement of smaller size particles may cause high reactivity due to high surface area, yet it can also cause rapid solidification and hardening, high viscosity or low fluidity of cement.In some embodiments, the unimodal particle distribution of the reactive vaterite cement of larger size particles may cause low reactivity due to low surface area, yet it can cause low viscosity or high fluidity.The character of the reactive vaterite cement in cement paste, concrete or mortar can also interact with other components added in paste (described herein), affecting its reactivity and fluidity.
[0053] Applicant also unexpectedly and surprisingly found that the water demand of reactive vaterite cement particles of different sizes is different, affects the packing density or bulk density of cement products.For example, in the unimodal distribution of reactive vaterite cement particles, a kind of spherical vaterite particles of average size can be matched together to leave space or space between particles.According to the particle diameter of reactive vaterite cement, the volume of space or space can be changed, to produce space or space in the cement products with the packing density or bulk density of variation of gained.In addition, the surface area increased in the reactive vaterite cement particles of small size may need more water to wet.More water in the paste may cause the cement products with lower density, because water may leave pore or space after evaporation and drying.In some embodiments, when reactive vaterite cement is bimodal distribution, the vaterite particles of small size mix with the vaterite particles of large size, and wherein small particle can be filled between large particle, thereby increase solid volume and density, therefore increase the packing density or bulk density of cement products.
[0054] Therefore, the particle size and distribution of reactive vaterite cement play an important role in the processability, fluidity, packing density and compressive strength of cement products. Provided herein are compositions, methods and systems related to bimodal particle distribution, trimodal particle distribution or multimodal particle distribution of reactive vaterite cement providing high packing density but high fluidity. Although bimodal distribution and multimodal distribution of reactive vaterite cement particles are provided herein, for example, multiple examples of trimodal distribution, other multimodal distributions including 4 kinds, or 5 kinds, or 6 kinds or more kinds of particle size distributions are fully within the scope of the present invention. It should also be understood that within the scope of mean particle size, for example, reactive vaterite cement A with mean particle size between about 0.1 μm-10 μm, more than one median particle size distribution may be present. For example only, in the table 2 of embodiment 4 herein, blend B1 is included in two different median particle sizes of 4 μm and 7 μm in the mean particle size between about 0.1 μm-10 μm. Mean particle size or median particle size are used interchangeably herein.
[0055] Figure 1 The figure shows a unimodal particle distribution, a bimodal particle distribution, a trimodal particle distribution or a multimodal particle distribution of the reactive vaterite cement. It should be understood that Figure 1 It is merely a pictorial representation of the particle size of the mixture and in no way limits the particle size of the mixture or the mixture design or packing density or flowability or any other property.
[0056] In some embodiments of cement compositions provided herein, reactive vaterite cement has a spherical particle shape with an average particle size between about 0.1 μm-100 μm (micrometer). The average particle size (or average particle diameter) can be measured using any conventional particle size determination method, such as but not limited to multi-detector laser scattering or laser diffraction or sieving.
[0057] In one aspect, a cement composition is provided, comprising: a bimodal distribution of reactive vaterite cements comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm and reactive vaterite cement B having an average particle size between about 11 μm-50 μm.
[0058] It should be understood that the terms A, B and C used for the reactive vaterite cement are used only for the purpose of distinguishing based on the particle size of the reactive vaterite cement.
[0059] In one aspect, a cement composition is provided, comprising: a bimodal distribution of reactive vaterite cement comprising:
[0060] Reactive vaterite cement A, the reactive vaterite cement A having an average particle size between about 0.1-10 μm, or between about 0.1-9 μm, or between about 0.1-8 μm, or between about 0.1-7 μm, or between about 0.1-6 μm, or between about 0.1-5 μm, or between about 0.1-4 μm, or between about 0.1-3 μm, or between about 0.1-2 μm, or between about 0.1-1 μm, or between about 1-10 μm, or between about 1-8 μm, or between about 1-5 μm, or between about 1-3 μm, or between about 3-10 μm, or between about 3-8 μm, or between about 4-6 μm, or between about 6-8 μm; and
[0061] Reactive vaterite cement B, the reactive vaterite cement B has a particle size of between about 11-50 μm, or between about 11-45 μm, or between about 11-40 μm, or between about 11-35 μm, or between about 11-30 μm, or between about 11-25 μm, or between about 11-20 μm, or between about 11-15 μm, or between about 15-50 μm, or between about 15-45 μm. or an average particle size of about 15-40 μm, or about 15-35 μm, or about 15-30 μm, or about 15-25 μm, or about 15-20 μm, or about 20-50 μm, or about 20-40 μm, or about 30-50 μm, or about 30-40 μm, or about 40-50 μm, or about 20-30 μm.
[0062] In one aspect, a cement composition is provided, comprising: a bimodal distribution of reactive vaterite cements, comprising: reactive vaterite cement A, wherein the reactive vaterite cement A has an average particle size between about 0.1-10 μm, or between about 0.1-8 μm, or between about 0.1-5 μm, or between about 0.1-2 μm, or between about 0.1-1 μm, or between about 3-10 μm, or between about 4-6 μm, or between about 6-8 μm; and reactive vaterite cement B, wherein the reactive vaterite cement B has an average particle size between about 11-50 μm, or between about 11-25 μm, or between about 11-20 μm, or between about 15-30 μm, or between about 20-50 μm, or between about 30-50 μm, or between about 40-50 μm.
[0063] In one aspect, a cement composition is provided, comprising: a trimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and reactive vaterite cement C having an average particle size between about 51 μm-100 μm.
[0064] In one aspect, a cement composition is provided, comprising: a trimodal distribution of reactive vaterite cement comprising:
[0065] Reactive vaterite cement A, the reactive vaterite cement A having an average particle size between about 0.1-10 μm, or between about 0.1-9 μm, or between about 0.1-8 μm, or between about 0.1-7 μm, or between about 0.1-6 μm, or between about 0.1-5 μm, or between about 0.1-4 μm, or between about 0.1-3 μm, or between about 0.1-2 μm, or between about 0.1-1 μm, or between about 1-10 μm, or between about 1-8 μm, or between about 1-5 μm, or between about 1-3 μm, or between about 3-10 μm, or between about 3-8 μm, or between about 4-6 μm, or between about 6-8 μm;
[0066] Reactive vaterite cement B, the reactive vaterite cement B has a particle size of about 11-50 μm, or about 11-45 μm, or about 11-40 μm, or about 11-35 μm, or about 11-30 μm, or about 11-25 μm, or about 11-20 μm, or about 11-15 μm, or about 15-50 μm, or about 15-45 μm. , or an average particle size between about 15-40 μm, or between about 15-35 μm, or between about 15-30 μm, or between about 15-25 μm, or between about 15-20 μm, or between about 20-50 μm, or between about 20-40 μm, or between about 30-50 μm, or between about 30-40 μm, or between about 40-50 μm, or between about 20-30 μm; and
[0067] Reactive vaterite cement C, the reactive vaterite cement C has an average particle size between about 51-100 μm; between about 51-90 μm; or between about 51-75 μm; or between about 51-60 μm; or between about 60-100 μm; or between about 60-75 μm; or between about 70-100 μm; or between about 70-80 μm; or between about 80-100 μm; or between about 80-90 μm.
[0068] In one aspect, a cement composition is provided, comprising: a trimodal distribution of reactive vaterite cement comprising:
[0069] Reactive vaterite cement A, the reactive vaterite cement A having an average particle size between about 0.1-10 μm, or between about 0.1-8 μm, or between about 0.1-5 μm, or between about 0.1-2 μm, or between about 0.1-1 μm, or between about 3-10 μm, or between about 4-6 μm, or between about 6-8 μm;
[0070] Reactive vaterite cement B, the reactive vaterite cement B having an average particle size between about 11-50 μm, or between about 11-25 μm, or between about 11-20 μm, or between about 15-30 μm, or between about 20-50 μm, or between about 30-50 μm, or between about 40-50 μm; and
[0071] Reactive vaterite cement C, the reactive vaterite cement C having an average particle size between about 51-100 μm; or between about 51-75 μm; or between about 60-100 μm; or between about 60-75 μm; or between about 70-80 μm; or between about 80-90 μm.
[0072] In one aspect, a cement composition is provided, comprising: a reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; and a bimodal distribution of reactive vaterite cement C having an average particle size between about 51 μm and 100 μm.
[0073] In one aspect, a cement composition is provided, comprising: a bimodal distribution of reactive vaterite cement comprising:
[0074] Reactive vaterite cement B, the reactive vaterite cement B has a particle size of between about 11-50 μm, or between about 11-45 μm, or between about 11-40 μm, or between about 11-35 μm, or between about 11-30 μm, or between about 11-25 μm, or between about 11-20 μm, or between about 11-15 μm, or between about 15-50 μm, or between about 15-45 μm. an average particle size of about 15-40 μm, about 15-35 μm, about 15-30 μm, about 15-25 μm, about 15-20 μm, about 20-50 μm, about 20-40 μm, about 30-50 μm, about 30-40 μm, about 40-50 μm, or about 20-30 μm; and
[0075] Reactive vaterite cement C, the reactive vaterite cement C has an average particle size between about 51-100 μm; between about 51-90 μm; or between about 51-75 μm; or between about 51-60 μm; or between about 60-100 μm; or between about 60-75 μm; or between about 70-100 μm; or between about 70-80 μm; or between about 80-100 μm; or between about 80-90 μm.
[0076] In one aspect, a cement composition is provided, comprising: a bimodal distribution of reactive vaterite cements, comprising: reactive vaterite cement B having an average particle size between about 11-50 μm, or between about 11-25 μm, or between about 11-20 μm, or between about 15-30 μm, or between about 20-50 μm, or between about 30-50 μm, or between about 40-50 μm; and reactive vaterite cement C having an average particle size between about 51-100 μm; or between about 51-75 μm; or between about 60-100 μm; or between about 60-75 μm; or between about 70-80 μm; or between about 80-90 μm.
[0077] In some embodiments, reactive vaterite cement comprises two or more, or three or more, or multimodal in the composition, such as for example or four or more, or five or more, or ten or more, or 20 or more, or 3-20, or 4-10 particles of different sizes. For example, the composition can be included in two or more, or three or more, or the particle distribution between 3-20 in the particle range of 0.1 μm-100 μm size.
[0078] A bimodal, trimodal or multimodal distribution can allow surface area to be minimized (due to the mixing of larger sized particles with smaller sized particles of the above range), thus allowing a lower liquid / solid mass ratio (water to cement ratio) when the composition is mixed with water, thereby allowing a higher flow rate. Smaller sized particles with high surface area can provide reactive particles for early reaction to set and harden into interlocking needle-like aragonite forms and / or calcite forms and / or carbonoaluminates (formed with alumina in other components of cements such as, for example, Portland cement).
[0079] In some embodiments of the above aspects, the cement composition comprises a bimodal distribution of reactive vaterite cements, comprising: between about 5%-95% by weight of reactive vaterite cement A in the composition and between about 5%-95% by weight of reactive vaterite cement B in the composition. Thus, in some embodiments of the above aspects, the cement composition comprises a bimodal distribution of reactive vaterite cements, comprising: between about 5%-95% by weight of reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm in the composition; and between about 5%-95% by weight of reactive vaterite cement B having an average particle size between about 11 μm-50 μm in the composition.
[0080] In some embodiments of the above aspects and embodiments, the cement composition comprises the above bimodal distribution of reactive vaterite cement A and reactive vaterite cement B, comprising:
[0081] Reactive vaterite cement A, wherein the reactive vaterite water A is between about 5%-95% by weight, or between about 5%-85% by weight, or between about 5%-75% by weight, or between about 5%-65% by weight, or between about 5%-55% by weight, or between about 5%-45% by weight, or between about 5%-35% by weight, or between about 5%-2 ... % to 15%, or between about 15% to 95% by weight, or between about 15% to 85% by weight, or between about 15% to 75% by weight, or between about 15% to 65% by weight, or between about 15% to 55% by weight, or between about 15% to 45% by weight, or between about 15% to 35% by weight, or between about 15% to 25% by weight, or between about 25% to 95% by weight. 5% by weight, or between about 25%-85% by weight, or between about 25%-75% by weight, or between about 25%-65% by weight, or between about 25%-55% by weight, or between about 25%-45% by weight, or between about 25%-35% by weight, or between about 35%-95% by weight, or between about 35%-85% by weight, or between about 35%-75% by weight %, or between about 35%-65% by weight, or between about 35%-55% by weight, or between about 35%-45% by weight, or between about 50%-95% by weight, or between about 50%-75% by weight, or between about 60%-95% by weight, or between about 60%-75% by weight, or between about 75%-95% by weight, or between about 80%-95% by weight; and
[0082] Reactive vaterite cement B, the reactive vaterite cement B is between about 5%-95% by weight, or between about 5%-85% by weight, or between about 5%-75% by weight, or between about 5%-65% by weight, or between about 5%-55% by weight, or between about 5%-45% by weight, or between about 5%-35% by weight, or between about 5%-25% by weight, or between about 5% to 15%, or between about 15% to 95% by weight, or between about 15% to 85% by weight, or between about 15% to 75% by weight, or between about 15% to 65% by weight, or between about 15% to 55% by weight, or between about 15% to 45% by weight, or between about 15% to 35% by weight, or between about 15% to 25% by weight, or between about 2 ...15% to 25% by weight, or between about 15% to 65% by weight, or between about 15% to 55% by weight, or between about 15% to 45% by weight, or between about 15% to 35% by weight, or between about 15% to 25% by weight, or between about 15% to 35% by weight, or between about 15% to 25% by weight, or between about 15% to 95%, or between about 25%-85% by weight, or between about 25%-75% by weight, or between about 25%-65% by weight, or between about 25%-55% by weight, or between about 25%-45% by weight, or between about 25%-35% by weight, or between about 35%-95% by weight, or between about 35%-85% by weight, or between about 35%-75% by weight % by weight, or between about 35%-65% by weight, or between about 35%-55% by weight, or between about 35%-45% by weight, or between about 50%-95% by weight, or between about 50%-75% by weight, or between about 60%-95% by weight, or between about 60%-75% by weight, or between about 75%-95% by weight, or between about 80%-95% by weight.
[0083] In some embodiments of the above aspects and embodiments, the cement composition comprises the above-mentioned bimodal distribution of reactive vaterite cement A and reactive vaterite cement B, which comprises: reactive vaterite cement A between about 5%-75% by weight in the composition and reactive vaterite cement B between about 25%-95% by weight in the composition.
[0084] In some embodiments of the above aspects and embodiments, the cement composition comprises the above bimodal distribution of reactive vaterite cement A and reactive vaterite cement B, comprising:
[0085] Reactive vaterite cement A, the reactive vaterite cement A is between about 5%-75% by weight, or between about 5%-65% by weight, or between about 5%-55% by weight, or between about 5%-45% by weight, or between about 5%-35% by weight, or between about 5%-25% by weight, or between about 5%-15% by weight, or between about 15%-75% by weight, or between about 15%-55% by weight, or between about 15%-35% by weight, or between about 25%-75% by weight, or between about 25%-55% by weight, or between about 35%-75% by weight, or between about 35%-55% by weight, or between about 50%-75% by weight, or between about 60%-75% by weight, and
[0086] Reactive vaterite cement B, the reactive vaterite cement B is between about 25%-95% by weight, or between about 25%-75% by weight, or between about 25%-55% by weight, or between about 35%-95% by weight, or between about 35%-75% by weight, or between about 35%-55% by weight, or between about 50%-95% by weight, or between about 50%-75% by weight, or between about 60%-95% by weight, or between about 60%-75% by weight, or between about 75%-95% by weight, or between about 80%-95% by weight.
[0087] In some embodiments of the above aspects and embodiments, the cement composition comprises the above-mentioned trimodal distribution of reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C, which comprises: reactive vaterite cement A between about 5%-40% by weight in the composition, reactive vaterite cement B between about 25%-50% by weight in the composition, and reactive vaterite cement C between about 5%-10% by weight in the composition.
[0088] In some embodiments of the foregoing aspects and embodiments, the cement composition comprises a trimodal distribution of reactive vaterite cement comprising:
[0089] between about 5%-40% by weight of reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm in the composition,
[0090] between about 25%-50% by weight of reactive vaterite cement B having an average particle size between about 11 μm-50 μm in the composition, and
[0091] Between about 5%-10% by weight of reactive vaterite cement C having an average particle size between about 51 μm-100 μm is present in the composition.
[0092] In some embodiments of the foregoing aspects and embodiments, the cement composition comprises:
[0093] Reactive vaterite cement A, the reactive vaterite cement A is between about 5%-40% by weight, or between about 5%-35% by weight, or between about 5%-25% by weight, or between about 5%-15% by weight, or between about 15%-40% by weight, or between about 15%-25% by weight, or between about 25%-40% by weight, or between about 30-40% by weight,
[0094] Reactive vaterite cement B, the reactive vaterite cement B is between about 25%-50% by weight, or between about 35-50% by weight, and
[0095] Reactive vaterite cement C, the reactive vaterite cement C is between about 5%-10% by weight, or between about 8%-10% by weight.
[0096] In some embodiments of the above aspects and embodiments, the cement composition comprises a bimodal distribution of reactive vaterite cements comprising: reactive vaterite cement B between about 25%-50% by weight in the composition and reactive vaterite cement C between about 5%-10% by weight in the composition. In some embodiments of the above aspects and embodiments, the cement composition comprises reactive vaterite cement B between about 25%-50% by weight, or between about 35-50% by weight in the composition and reactive vaterite cement C between about 5%-10% by weight, or between about 8%-10% by weight in the composition.
[0097] In some embodiments of the above aspects and embodiments, the cement composition comprises a bimodal distribution of reactive vaterite cement, comprising: between about 25%-50% by weight of reactive vaterite cement B having an average particle size between about 11 μm-50 μm in the composition and between about 5%-10% by weight of reactive vaterite cement C having an average particle size between about 51 μm-100 μm in the composition.
[0098] In some embodiments, reactive vaterite cement A, reactive vaterite cement B and / or reactive vaterite cement C or the multimodal composition improves or increases the packing density of the cement paste (in water) by between about 1%-35%, or between about 1%-30%, or between about 1%-25%, or between about 1%-20%, or between about 1%-15%, or between about 1%-10%, or between about 1%-5%, or between about 5%-35%, or between about 5%-30%, or between about 5%-25%, or between about 5%-20%, or between about 5%-15%, or between about 5%-10%, or between about 10%-35%, or between about 10%-25%, or between about 10%-15%, or between about 20%-35%, or between about 25%-35%.
[0099] As described herein, larger sized particles in a bimodal, trimodal, or multimodal distribution of particles can improve the flowability of cement pastes, mortars, or concrete by allowing a lower liquid / solid mass ratio (or water to cement ratio) when the composition is mixed with water.
[0100] In some embodiments of the above aspects and embodiments, the reactive vaterite cement B with a particle size between about 11 μm-50 μm in a composition comprising a bimodal distribution, a trimodal distribution or a multimodal distribution as provided herein reduces the viscosity of the cement paste or the cement paste in concrete or mortar (or increases the fluidity or increases the slump) by about 10% or more, or about 20% or more, or about 30% or more, or about 35% or more, or about 40% or more, or about 50% or more, or between about 10%-50%, or between about 10%-40%, or between about 10%-30%, or between about 10%-20%, or between about 30%-50%, or between about 30%-40%.
[0101] In some embodiments of the above aspects and embodiments, reactive vaterite cement B with a particle size between about 11 μm-50 μm and / or reactive vaterite cement C with a particle size between about 51 μm-100 μm in a composition comprising a bimodal distribution, a trimodal distribution or a multimodal distribution as provided herein reduces the viscosity of the cement paste in the cement paste or mortar or concrete (or increases the fluidity) by about 10% or more, or about 20% or more, or about 30% or more, or about 35% or more, or about 40% or more, or about 50% or more, or between about 10%-50%, or between about 10%-40%, or between about 10%-30%, or between about 10%-20%, or between about 30%-50%, or between about 30%-40%.
[0102] In some embodiments of the above aspects and embodiments, the ratio of reactive vaterite cement A: reactive vaterite cement B (having a particle size and / or amount described herein) is between about 1:20-20:1, or between about 1:15-15:1, or between about 1:10-10:1, or between about 1:5-5:1, or between about 1:2-2:1.
[0103] In some embodiments of the above aspects and embodiments, the ratio of reactive vaterite cement B: reactive vaterite cement C (having a particle size and / or amount described herein) is between about 1:20-20:1, or between about 1:15-15:1, or between about 1:10-10:1, or between about 1:5-5:1, or between about 1:2-2:1.
[0104] As described herein, the size of the particles affects the surface area of the reactive vaterite cement particles, which in turn affects the water to cement ratio and the reactivity of the cement and the fluidity of the cement paste. In some embodiments, the composition comprises a bimodal distribution of reactive vaterite cement comprising a particle size having a relative humidity of about 100 m / s and a relative humidity of about 20 m / s. 2 / kg-40,000m 2 / kg of reactive vaterite cement A and reactive vaterite cement B. In some embodiments, the composition comprises a bimodal distribution of reactive vaterite cements, which comprises a mean particle size between about 0.1 μm and 10 μm with a particle size between about 4,000 μm and a particle size between about 100 μm and about 200 μm. 2 / kg-40,000m 2 / kg and a total specific surface area of reactive vaterite cement A between about 100 μm and about 11 μm-50 μm. 2 / kg-6,000m 2 / kg of reactive vaterite cement B. In some embodiments, the composition comprises a bimodal distribution of reactive vaterite cement, comprising, having an average particle size between about 0.1 μm-10 μm, having a particle size between about 4,000 μm and a particle size between about 1000 μm and about 2000 μm. 2 / kg-40,000m 2 / kg and a reactive vaterite cement A between about 5% and 95% by weight in the composition; and an average particle size between about 11 μm and 50 μm, with a particle size between about 100 μm and about 100 μm. 2 / kg-6,000m 2 / kg and a reactive vaterite cement B of between about 5% and 95% by weight in the composition.
[0105] In some embodiments, the composition comprises a bimodal distribution of reactive vaterite cement comprising:
[0106] Reactive vaterite cement A, the reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm, having a particle size between about 4,000 and 40,000 μm 2 / kg, or about 4,000-10,000m 2 / kg, or about 4,000-5,000m 2 / kg, or about 5,000-40,000m 2 / kg, or about 5,000-10,000m 2 / kg, or about 10,000-40,000m 2 / kg, or about 10,000-20,000m 2 / kg, or about 20,000-40,000m 2 / kg specific surface area; and
[0107] Reactive vaterite cement B, the reactive vaterite cement B having an average particle size between about 11 μm and 50 μm, having a particle size between about 100 and 6,000 μm 2 / kg, or about 100-5,000m 2 / kg, or about 100-4,000m 2 / kg, or about 100-3,000m 2 / kg, or about 100-2,000m 2 / kg, or about 100-1,000m 2 / kg, or about 100-500m 2 / kg, or about 500-6,000m 2 / kg; or about 500-3,000m 2 / kg; or about 500-1,000m 2 / kg; or about 1,000-6,000m 2 / kg; or about 1,000-4,000m 2 / kg; or about 2,000-6,000m 2 / kg; or about 3,000-6,000m 2 / kg; or about 5,000-6,000m 2 / kg between specific surface area.
[0108] In some embodiments, the composition comprises a trimodal distribution of reactive vaterite cements comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm, having a particle size between about 4,000 and 40,000 μm, and having a particle size between about 100 and 200 μm. 2 / kg specific surface area; reactive vaterite cement B, the reactive vaterite cement B having an average particle size between about 11 μm-50 μm, having a specific surface area between about 100-6,000 m 2 / kg specific surface area between; and reactive vaterite cement C, the reactive vaterite cement C having an average particle size between about 51 μm-100 μm, having a specific surface area between about 50-1000 m 2 / kg between specific surface area.
[0109] In some embodiments, the composition comprises a trimodal distribution of reactive vaterite cement comprising:
[0110] Reactive vaterite cement A, the reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm, having a particle size between about 4,000 and 40,000 μm 2 / kg, or about 4,000-10,000m 2 / kg, or about 4,000-5,000m 2 / kg, or about 5,000-40,000m 2 / kg, or about 5,000-10,000m 2 / kg, or about 10,000-40,000m 2 / kg, or about 10,000-20,000m 2 / kg, or about 20,000-40,000m 2 / kg specific surface area;
[0111] Reactive vaterite cement B, the reactive vaterite cement B having an average particle size between about 11 μm and 50 μm, having a particle size between about 100 and 6,000 μm 2 / kg, or about 100-5,000m 2 / kg, or about 100-4,000m 2 / kg, or about 100-3,000m 2 / kg, or about 100-2,000m 2 / kg, or about 100-1,000m 2 / kg, or about 100-500m 2 / kg, or about 500-6,000m2 / kg; or about 500-3,000m 2 / kg; or about 500-1,000m 2 / kg; or about 1,000-6,000m 2 / kg; or about 1,000-4,000m 2 / kg; or about 2,000-6,000m 2 / kg; or about 3,000-6,000m 2 / kg; or about 5,000-6,000m 2 / kg specific surface area; and
[0112] Reactive vaterite cement C, the reactive vaterite cement C has an average particle size between about 51 μm and 100 μm, and has a particle size between about 50 and 1000 μm. 2 / kg; or about 50-500m 2 / kg; or about 50-200m 2 / kg; or about 100-1000m 2 / kg; or about 100-500m 2 / kg; or about 500-1000m 2 / kg between specific surface area.
[0113] In some embodiments, the composition comprises a bimodal distribution of reactive vaterite cements comprising reactive vaterite cement B having an average particle size between about 11 μm and 50 μm, having a particle size between about 100 and 6,000 μm, and having a particle size between about 100 and 6,000 μm. 2 / kg specific surface area between; and reactive vaterite cement C, the reactive vaterite cement C having an average particle size between about 51μm-100μm, having a particle size between about 50-1000m 2 / kg between specific surface area.
[0114] In some embodiments, the composition comprises a bimodal distribution of reactive vaterite cement comprising:
[0115] Reactive vaterite cement B, the reactive vaterite cement B having an average particle size between about 11 μm and 50 μm, having a particle size between about 100 and 6,000 μm 2 / kg, or about 100-5,000m 2 / kg, or about 100-4,000m 2 / kg, or about 100-3,000m 2 / kg, or about 100-2,000m2 / kg, or about 100-1,000m 2 / kg, or about 100-500m 2 / kg, or about 500-6,000m 2 / kg; or about 500-3,000m 2 / kg; or about 500-1,000m 2 / kg; or about 1,000-6,000m 2 / kg; or about 1,000-4,000m 2 / kg; or about 2,000-6,000m 2 / kg; or about 3,000-6,000m 2 / kg; or about 5,000-6,000m 2 / kg specific surface area; and
[0116] Reactive vaterite cement C, the reactive vaterite cement C has an average particle size between about 51 μm and 100 μm, and has a particle size between about 50 and 1000 μm. 2 / kg; or about 50-500m 2 / kg; or about 50-200m 2 / kg; or about 100-1000m 2 / kg; or about 100-500m 2 / kg; or about 500-1000m 2 / kg between specific surface area.
[0117] The composition of bimodal distribution, trimodal distribution or multimodal distribution comprising reactive vaterite cement provided herein may optionally also include magnesium oxide.Magnesium oxide can be introduced into reactive vaterite cement (described further herein) during the production of reactive vaterite cement, or can be added to reactive vaterite cement after reactive vaterite cement production.The magnesium oxide in the composition comprising reactive vaterite cement has been described in detail in No. 63 / 176,709 of U.S. Provisional Application submitted on April 19, 2021, which is incorporated herein by reference in its entirety.
[0118] The bimodal distribution, trimodal distribution or multimodal distribution of the composition comprising reactive vaterite cement provided herein can optionally also include other one or more components (to form blend) selected from the group consisting of slag, portland cement clinker, calcium aluminate clinker, calcium sulphoaluminate cement clinker, aluminosilicate material, supplementary cementitious material (SCM) and combinations thereof from metal production.In some embodiments, the cement composition provided herein also includes portland cement or portland cement clinker to form a blended cement composition.
[0119] In some embodiments, a cement composition is provided, comprising a bimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm and reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and Portland cement. In some embodiments, a cement composition is provided, comprising a bimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm and reactive vaterite cement B having an average particle size between about 11 μm-30 μm; and Portland cement.
[0120] In some embodiments, a cement composition is provided, comprising a trimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and reactive vaterite cement C having an average particle size between about 51 μm-100 μm; and Portland cement.
[0121] Applicant unexpectedly and surprisingly found that, when blended with portland cement, bimodal distribution or multimodal (for example, trimodal) distribution of reactive vaterite cement particles cause high reactivity of cement and low paste viscosity or high fluidity, these two properties are all desirable and difficult to obtain for processability, fluidity, packing density and the compressive strength of cement products.Find that when reactive vaterite particles are combined to produce the blend with portland cement with multimodal distribution (for example, as bimodal blend or trimodal blend), if using unimodal reactive vaterite to produce paste, will show that blend has the paste viscosity lower than their surface area.Lower paste viscosity is relevant with higher fluidity in mortar and higher slump in concrete.In some embodiments, reactive vaterite cement A (for example, with about 4,000m 2 / kg-40,000m 2 / kg) provides a high surface area to nucleate calcium silicate hydrate (CSH) and dissolve Portland cement in water.
[0122] In some embodiments of the above-mentioned blended compositions, the bimodal distribution and / or trimodal distribution in the blended cement composition provides a paste viscosity of between about 800-1600 mPa*s; or between about 800-1500 mPa*s; or between about 800-1400 mPa*s; or between about 800-1300 mPa*s; or between about 800-1200 mPa*s; or between about 800-1150 mPa*s; or between about 800-1100 mPa*s; or between about 800-1050 mPa*s; or between about 800-1000 mPa*s; or between about 900-1500 mPa*s; or between about 1000-1500 mPa*s; or between about 1100-1500 mPa*s; or between about 1000-1200 mPa*s.
[0123] In addition, it is also found that the larger the surface area of reactive vaterite cement particles present in the blended cement, the larger the surface area that can be used to nucleate the calcium silicate hydrate (CSH) of portland cement. The more calcium silicate hydrates of nucleation, the faster portland cement dissolves and produces strength in the blended cement composite. The bimodal distribution or multimodal distribution of reactive vaterite cement particles can make it possible to produce a blended cement composite with a processability or paste viscosity or fluidity similar to its portland cement control (100% portland cement), while providing additional surface area for CSH formation and strength enhancement compared to the blended cement produced with unimodal reactive vaterite.
[0124] In some embodiments, a cement paste or cement slurry composition is provided, comprising reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and optionally reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water; and Portland cement. As described herein, the reactive vaterite cement having a bimodal or multimodal distribution forms interlocking needle-like aragonite after dissolution and reprecipitation in water. In some embodiments, a cement paste or cement slurry composition is provided, which comprises reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and optionally reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water; Portland cement; and interlocking needle-shaped aragonite.
[0125] In some embodiments, the reactive vaterite cement A (e.g., having a 2 / kg-40,000m 2 / kg specific surface area) provides a high surface area to nucleate calcium silicate hydrate and dissolve portland cement in water. In some embodiments, a cement paste or cement slurry composition is provided, which comprises a reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; a reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and optionally a reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water; portland cement; interlocking needle-shaped aragonite; and calcium silicate hydrate.
[0126] In some embodiments, reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C provide a paste viscosity between about 800mPa*s-1600mPa*s in a cement paste or cement slurry composition. In some embodiments, a cement paste or cement slurry composition is provided, comprising reactive vaterite cement A with an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B with an average particle size between about 11 μm-50 μm; and optionally reactive vaterite cement C with an average particle size between about 51 μm-100 μm; water; portland cement; interlocking needle-shaped aragonite; and calcium silicate hydrate, wherein the cement paste or cement slurry has a paste viscosity between about 800mPa*s-1600mPa*s.
[0127] As used herein, "supplementary cementitious material" (SCM) includes SCM as known in the art. In some embodiments, SCM includes slag, fly ash, silica ash or its combination. Aluminosilicate material includes any material rich in aluminate minerals and silicate minerals. These materials can be natural or artificial. In some embodiments, aluminosilicate material includes heat-treated clay, such as calcined clay, natural volcanic ash or artificial volcanic ash, shale, granulated blast furnace slag or its combination. In some embodiments, natural or artificial volcanic ash is selected from the group consisting of fly ash, volcanic ash or its mixture. Volcanic ash can be naturally available and fine particles comprising siliceous and aluminous materials, which can react with the Ca ions in reactive vaterite to form cementitious materials in the presence of water. In some embodiments, heat-treated clay includes but is not limited to calcined clay, aluminosilicate glass, calcium aluminosilicate glass or its combination.
[0128] Various other components that can be blended in the compositions provided herein include, but are not limited to, carbonate materials such as limestone or calcium carbonate or magnesium carbonate or calcium magnesium carbonate; alkali metal promoters; or alkaline earth metal promoters, etc. Alkali metal promoters or alkaline earth metal promoters include, but are not limited to, any alkali metal salt or alkaline earth metal salt, such as, for example, sodium sulfate, sodium carbonate, sodium nitrate, sodium nitrite, sodium hydroxide, potassium sulfate, potassium carbonate, potassium nitrate, potassium nitrite, potassium hydroxide, lithium sulfate, lithium carbonate, lithium nitrate, lithium nitrite, lithium hydroxide, calcium sulfate (or gypsum), calcium nitrate, calcium nitrite, and combinations thereof.
[0129] In some embodiments, the composition of bimodal distribution, trimodal distribution or multimodal distribution comprising reactive vaterite cement provided herein can also include magnesium cation and / or strontium cation.In some embodiments, magnesium cation and / or strontium cation can promote reactive vaterite to be converted into interlocking needle-like aragonite (described further herein).In some embodiments, magnesium cation and / or strontium cation can exist in the form of salt, and the salt includes but is not limited to magnesium halide and / or strontium halide or magnesium sulfate and / or strontium sulfate or magnesium nitrate and / or strontium nitrate etc.In some embodiments, magnesium salt and / or strontium salt are selected from the group consisting of magnesium carbonate, magnesium halide (magnesium fluoride, magnesium chloride, magnesium iodide or magnesium bromide), magnesium hydroxide, magnesium silicate, magnesium sulfate, magnesium nitrate, magnesium nitrite, strontium carbonate, strontium halide, strontium hydroxide, strontium silicate, strontium sulfate, strontium nitrate, strontium nitrite and combination thereof.
[0130] In some embodiments, magnesium and / or strontium is present in a range between about 0.05M-0.1M. In some embodiments of the above method and system aspects and embodiments, the amount of magnesium salt and / or strontium salt used is between about 0-1M; or between about 0-0.5M; or between about 0.01M-1M; or between about 0.01M-0.5M; or between about 0.05M-1M; or between about 0.05M-0.5M; or between about 0.05M-0.1M; or between about 0.1M-1M; or between about 0.1M-0.5M. In some embodiments of the above method and system aspects and embodiments, the ratio of magnesium salt to strontium salt is between about 2:1 or between about 1.5:1 or between about 1:1.
[0131] In some embodiments of the aforementioned aspects and embodiments, the bimodal, trimodal or multimodal compositions comprising reactive vaterite cement provided herein may also contain less than 30% aragonite by weight; or less than 25% aragonite by weight; or less than 20% aragonite by weight; or less than 10% aragonite by weight; or less than 5% aragonite by weight; or less than 1% aragonite by weight; or between 1%-10% aragonite by weight; or between 1%-30% aragonite by weight.
[0132] In some embodiments of the aforementioned aspects and embodiments, the bimodal, trimodal or multimodal compositions comprising reactive vaterite cement provided herein may also include an aluminosilicate material, such as calcined clay or heat-treated clay; and optionally limestone and / or an alkali metal promoter or an alkaline earth metal promoter, and also include between 5%-90% by weight of Portland cement clinker; or between 5%-80% by weight; or between 5%-70% by weight; or between 5%-60% by weight; or between 5%-50% by weight; or between 5%-40% by weight; or between 5%-60% by weight. Between 5% and 30% by weight; or between 5% and 20% by weight; or between 5% and 10% by weight; or between 10% and 90% by weight; or between 10% and 80% by weight; or between 10% and 70% by weight; or between 10% and 60% by weight; or between 10% and 50% by weight; or between 10% and 40% by weight; or between 10% and 30% by weight; or between 10% and 20% by weight; or between 20% and 90% by weight; or between 20% and 80% by weight; or between 20%-70%; or 20%-60% by weight; or 20%-50% by weight; or 20%-40% by weight; or 20%-30% by weight; or 30%-90% by weight; or 30%-80% by weight; or 30%-70% by weight; or 30%-60% by weight; or 30%-50% by weight; or 30%-40% by weight; or 40%-90% by weight; or 40%-80% by weight; or 40%-90% by weight or between 0%-70% by weight; or between 40%-60% by weight; or between 40%-50% by weight; or between 50%-90% by weight; or between 50%-80% by weight; or between 50%-70% by weight; or between 50%-60% by weight; or between 60%-90% by weight; or between 60%-80% by weight; or between 60%-70% by weight; or between 70%-90% by weight; or between 70%-80% by weight; or between 80%-90% by weight of Portland cement clinker.
[0133] In some embodiments of the compositions provided herein, the composition comprises between about 0.1-5% by weight of an alkali metal promoter or an alkaline earth metal promoter, such as lithium carbonate; or between about 0.1%-4% by weight; or between about 0.1%-3% by weight; or between about 0.1%-2% by weight; or between about 0.1%-1% by weight; or between about 0.1%-0.5% by weight; or between about 1%-5% by weight; or between about 1%-4% by weight; or between about 1%-3% by weight; or between about 1%-2% by weight; or between about 2%-5% by weight; or between about 2%-4% by weight; or between about 2%-3% by weight; or between about 3%-5% by weight; or between about 3%-4% by weight; or between about 4%-5% by weight of an alkali metal promoter or an alkaline earth metal promoter.
[0134] In some embodiments of the foregoing aspects and embodiments, the composition may comprise a blend of: about 75% by weight of OPC or Portland cement clinker and a bimodal or trimodal distribution of a reactive vaterite cement as provided herein between about 1%-25%; or about 80% of OPC or Portland cement clinker and a bimodal or trimodal distribution of a reactive vaterite cement between about 1%-20%; or about 85% of OPC or Portland cement clinker and a bimodal or trimodal distribution of a reactive vaterite cement between about 1%-15%; or about 90% of OPC or Portland cement clinker and a bimodal or trimodal distribution of a reactive vaterite cement between about 1%-10%; or about 95% of OPC or Portland cement clinker and a bimodal or trimodal distribution of a reactive vaterite cement between about 1%-5%. The amount of particle distribution in reactive vaterite cement and / or particle diameter and / or surface area have all been described in this article, and they are all applicable to multiple blends described herein.In some embodiments of aforementioned aspects and embodiments, the remainder in the composition can include one or more of aluminosilicate material and optionally carbonate material and alkali metal promoter or alkaline earth metal promoter.
[0135] In some embodiments of the reactive vaterite cement compositions provided herein, the compositions comprise, by weight, between about 5%-50% reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle sizes, amounts, ratios and / or surface areas are all described herein), between about 5%-40% heat-treated clay, between about 0-10% limestone, and between about 15%-90% Portland cement clinker.
[0136] In some embodiments of the reactive vaterite cement compositions provided herein, the compositions comprise, by weight, between about 10%-50% reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle size, amount, ratio and / or surface area are all described herein), between about 10%-35% aluminosilicate material, between about 0-10% carbonate material and between about 15%-90% Portland cement clinker.
[0137] In some embodiments of the reactive vaterite cement composition provided herein, the composition comprises by weight between about 10%-50% reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle size, amount, ratio and / or surface area are all described herein), between about 10%-35% aluminosilicate material, between about 0-10% carbonate material, between about 15%-90% Portland cement clinker and between about 0.1-5% alkali metal accelerator or alkaline earth metal accelerator.
[0138] In some embodiments of the reactive vaterite cement compositions provided herein, the compositions comprise between about 10%-50% by weight of reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle sizes, amounts, ratios and / or surface areas are all described herein), between about 10%-35% calcined clay, between about 0-10% limestone, and between about 15%-90% Portland cement clinker.
[0139] In some embodiments of the reactive vaterite cement compositions provided herein, the compositions comprise, by weight, between about 10%-50% reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle size, amount, ratio and / or surface area are all described herein), between about 10%-35% calcined clay, between about 0-10% limestone, between about 15%-90% Portland cement clinker, and between about 0.1-5% gypsum or lithium carbonate.
[0140] In some embodiments of the reactive vaterite cement compositions provided herein, the compositions comprise between about 10-20% by weight of reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle size, amount, ratio and / or surface area are all described herein), between about 10%-25% calcined clay, between about 0-10% limestone, between about 25%-55% Portland cement clinker, and between about 2%-5% gypsum or lithium carbonate.
[0141] In some embodiments of the reactive vaterite cement compositions provided herein, the compositions comprise, by weight, between about 25%-35% reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C or reactive vaterite cement B and reactive vaterite cement C (particle sizes, amounts, ratios and / or surface areas are all described herein), between about 25%-35% calcined clay, between about 0-5% limestone, between about 25%-35% Portland cement clinker, and between about 2%-5% gypsum or lithium carbonate.
[0142] In some embodiments, the reactive vaterite cement compositions provided herein have a 28-day compressive strength of at least 21 MPa after setting and hardening.
[0143] In some embodiments, the reactive vaterite cement composition in wet form or dry form provided herein can also include one or more plasticizers. The example of plasticizer includes but is not limited to superplasticizer based on polycarboxylate, MasterGlenium 7920, MasterGlenium 7500, Fritz-Pak Supercizer PCE, sodium salt of poly-(naphthalenesulfonic acid), Fritz-Pak Supercizer 5 and the like.
[0144] In some embodiments, the composition of bimodal distribution, trimodal distribution or multimodal distribution comprising reactive vaterite cement provided herein can also include one or more admixtures to give product one or more properties, including but not limited to strength, flexural strength, compressive strength, porosity, thermal conductivity, etc. The amount of the admixture adopted can vary according to the properties of the admixture. In some embodiments, the amount of one or more admixtures is in the range of from 0.1%w / w to 10%w / w. The example of admixture includes but is not limited to setting accelerator, setting delay agent, air entraining agent, foaming agent, defoamer, alkali reactivity reducer, bonding admixture, dispersant, coloring admixture, corrosion inhibitor, moisture-proof admixture, gas forming agent, permeability reducer, pumping aid, shrinkage compensation admixture, fungicidal admixture, bactericidal admixture, insecticidal admixture, rheology modifier, finely crushed mineral admixture, volcanic ash, aggregate, wetting agent, strength enhancer, waterproofing agent, reinforcing material such as fiber and any other admixture. When an admixture is used, the reactive vaterite cement composition into which the admixture raw material is introduced is mixed for a sufficient time to disperse the admixture raw material relatively uniformly throughout the composition.
[0145] In some embodiments, for example, in the case of fiber-reinforced products, the bimodal distribution, trimodal distribution or multimodal distribution of the composition comprising reactive vaterite cement provided herein can also include reinforcing materials, such as fibers. Fiber can be made of materials, aluminum, glass, steel, carbon, ceramics, grass, bamboo, wood, glass fiber or synthetic materials comprising zirconium oxide, for example polypropylene, polycarbonate, polyvinyl chloride, polyvinyl alcohol, nylon, polyethylene, polyester, rayon, high-strength aramid (i.e. ) or a mixture thereof.
[0146] In one aspect, a concrete mixture comprising any of the aforementioned compositions is provided, the aforementioned compositions comprising a bimodal distribution, a trimodal distribution or a multimodal distribution of reactive vaterite cement. "Concrete" as used herein comprises water, aggregate (e.g., rock, sand or gravel) and a cement composition provided herein.
[0147] In one aspect, a mortar mixture is provided comprising any of the aforementioned compositions comprising a bimodal distribution, a trimodal distribution, or a multimodal distribution of reactive vaterite cement. "Mortar" as used herein comprises water, sand, and a cement composition provided herein.
[0148] In one aspect, a cement paste or cement slurry composition is provided, comprising: a reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; a reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and water, and optionally interlocked needle-shaped aragonite, calcite, carbonoaluminate, or a combination thereof. In one aspect, a cement paste or cement slurry composition is provided, comprising: a reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; a reactive vaterite cement B having an average particle size between about 11 μm-50 μm; water and interlocked needle-shaped aragonite, calcite, carbonoaluminate, or a combination thereof. In one aspect, a cement paste or cement slurry composition is provided, comprising: a reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; a reactive vaterite cement B having an average particle size between about 11 μm-50 μm; water and interlocking needle-shaped aragonite.
[0149] In one aspect, a cement paste or cement slurry composition is provided, the cement paste or cement slurry composition comprising: reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water and optionally interlocked needle-shaped aragonite, calcite, carbonoaluminate or a combination thereof. In one aspect, a cement paste or cement slurry composition is provided, the cement paste or cement slurry composition comprises: reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water and interlocked needle-shaped aragonite, calcite, carbonoaluminate or a combination thereof. In one aspect, a cement paste or cement slurry composition is provided, which comprises: reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water and interlocking needle-shaped aragonite.
[0150] In one aspect, a cement paste or cement slurry composition is provided, the cement paste or cement slurry composition comprising: reactive vaterite cement B having an average particle size between about 11 μm-50 μm; reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water and optionally interlocked needle-shaped aragonite, calcite, carbonoaluminate or a combination thereof. In one aspect, a cement paste or cement slurry composition is provided, the cement paste or cement slurry composition comprises: reactive vaterite cement B having an average particle size between about 11 μm-50 μm; reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water and interlocked needle-shaped aragonite, calcite, carbonoaluminate or a combination thereof. In one aspect, a cement paste or cement slurry composition is provided, comprising: a reactive vaterite cement B having an average particle size between about 11 μm-50 μm; a reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water and interlocking needle-shaped aragonite.
[0151] In some embodiments, the cement paste or cement slurry further comprises one or more of the other components described herein. In embodiments where the cement composition further comprises Portland cement or Portland cement clinker and / or aluminosilicate material, the cement paste and / or slurry further comprises carbon aluminate.
[0152] II. Methods and Systems
[0153] Method and system for forming cement products
[0154] Disclosed herein is a method and system for forming a cement product, the cement product comprising interlocking needle-like aragonite, calcite and / or carbon aluminate.Also disclosed herein is a method and system for forming a cement product with a bulk density that varies, the cement product comprising interlocking needle-like aragonite, calcite and / or carbon aluminate.As used herein, " interlocking needle-like aragonite " comprises randomly interlocking needle-like aragonite.In some embodiments, needle-like aragonite grows from the surface of reactive vaterite during conversion, and in some embodiments, due to the bimodal or multimodal (e.g., trimodal) distribution of reactive vaterite cement particles causing needle-like aragonite to interlock.In some embodiments, unique interlocking needle-like aragonite provides high shear resistance, thereby providing high compressive strength and durability.
[0155] In some embodiments of the methods and systems described herein, the compositions result in the formation of a cement product having a unique morphology of an interlocking needle-like aragonite microstructure that provides the cement product with a unique lightness, durability, and strength. For example, the interlocking needle-like aragonite structure of the aggregate has been used, for example, in Figure 5 and Figure 6The invention is shown in the figure and described in the examples herein.
[0156] The packing density or bulk density of variation can be realized by selecting the unique bimodal, trimodal or multimodal particle distribution composition of reactive vaterite cement particles provided herein, which produces a cement product comprising interlocking needle-like aragonite optionally around one or more voids after mixing in water and after solidification. One or more voids form a honeycomb structure (wherein the needle-like thing radiates outwards from the vaterite sphere or its previous position) together with the interlocking needle-like aragonite around, for example, as Figure 6 As shown, the honeycomb structure provides porosity or lightness (reduced packing density or bulk density) to the cement product. Unique compositions of bimodal, trimodal or multimodal particle distributions of reactive vaterite cement particles have been described herein, which result in cement products with varying bulk densities.
[0157] In one aspect, a method for forming a cement product of a desired bulk density is provided, the method comprising preparing a wet composition comprising reactive vaterite cement and water by adding water to a composition comprising a bimodal, trimodal or multimodal particle distribution of reactive vaterite cement as provided herein; and a solidified cement product to convert reactive vaterite cement into interlocking needle-like aragonite to form a cement product of a desired bulk density. In some embodiments, by changing the amount of reactive vaterite cement A, reactive vaterite cement B and / or reactive vaterite cement C in a bimodal composition or trimodal composition as provided herein, a cement product of a varying bulk density can be obtained.
[0158] The composition of bimodal, trimodal or multimodal particle distribution comprising reactive vaterite cement has been described in detail herein. The method and system of producing reactive vaterite cement composition has been provided herein. In some embodiments, the mixer system configured to prepare wet composition by adding water in the composition comprising reactive vaterite cement is a rotary mixer, static mixer, pin mixer, Hobart mixer, tilted drum mixer, Omni mixer, Henschel mixer, V-type mixer or Nauta mixer. Such mixer is commercially known in the art.
[0159] In some embodiments, aragonite can be produced with reactive vaterite cement during the production of the reactive vaterite cement composition and / or aragonite can be added to the reactive vaterite cement composition and / or added to the water for preparing the wet composition and / or added to the wet composition itself. In some embodiments, aragonite serves as a seed for converting reactive vaterite cement into interlocking needle-like aragonite during and / or after curing.
[0160] In some embodiments, the ratio of water to cement can affect the packing density or bulk density of the cement product (as described herein). In some embodiments, the ratio of water to cement is between about 0.1:1 and 1.2:1; or between about 0.1:1 and 1:1; or between about 0.1:1-0.5:1.
[0161] In some embodiments, depending on the water to cement ratio of the composition comprising reactive vaterite cement and the additives used, the average particle size and / or particle distribution, the porosity of the cement product can be controlled to be between about 10%-90% and / or the bulk density to be between about 25-110 lb / ft 3 By way of example only, when the cement product is an aggregate, the aggregate is an aggregate having a porosity between about 10%-90% and / or a porosity between about 25-75 lb / ft 3 The production of the aggregate has been described in detail in the U.S. provisional application entitled "Compositions, methods, and systems related to aggregates" filed on the same date as the present application.
[0162] After forming cement product, product can be solidified by providing one or more of pressure, heat and / or humidity to convert reactive vaterite cement in cement product into interlocking needle-shaped aragonite and / or calcite and / or carbon aluminate to form cement product that solidifies and hardens. System for solidification includes any commercially known solidification system in the art, such as but not limited to autoclave, heated conveyor belt and / or solidification chamber. In some embodiments, pressure during solidification is between about 10psi-10,000psi; heat is between about 20℃-150℃; and / or humidity is between about 40%-100% relative humidity (RH). These ranges can vary according to the composition of cement product, including its water content or desired bulk density.
[0163] In some embodiments of the foregoing embodiments,
[0164] The pressure is between about 10-100,000 psi, or between about 10-75,000 psi, or between about 10-50,000 psi, or between about 10-25,000 psi, or between about 10-10,000 psi, or between about 10-2,000 psi, or between about 10-1,000 psi, or between about 10-500 psi;
[0165] heat between about 20°C-300°C, or between about 20°C-200°C, or between about 20°C-150°C, or between about 20°C-125°C, or between about 20°C-100°C, or between about 20°C-75°C, or between about 20°C-50°C, or between about 40°C-60°C, or between about 40°C-50°C, or between about 40°C-100°C, or between about 50°C-60°C, or between about 50°C-80°C, or between about 50°C-100°C, or between about 60°C-80°C, or between about 60°C-100°C; and / or
[0166] The humidity is between about 40-100% RH, or between about 40-75% RH, or between about 40-50% RH, or between about 50%-75% RH, or 40% RH, or 50% RH, or 60% RH, or 70% RH, or 90% RH, or 98% RH.
[0167] In some embodiments of the foregoing embodiments, the pressure is between about 10-1,000 psi, or between about 10-500 psi, or between about 10-100 psi; the heat is between about 40°C-150°C, or between about 40°C-95°C, or between about 60°C-80°C, or between about 75°C-100°C, or between about 100°C-150°C; and / or the humidity is between about 75-100% RH, or between about 80-100% RH, or between about 90-100% RH, or is 100% RH.
[0168] In some embodiments, the curing system provides heat and humidity in the form of steam to the reactive vaterite cement composition. The combination of curing conditions such as pressure, temperature, relative humidity and exposure time, etc. can vary depending on the size and composition of the cement product and the desired results.
[0169] During the curing process of cement products, in some embodiments, the bimodal distribution or multimodal distribution of reactive vaterite cement in wet composition can be dissolved in water and reprecipitated into interlocking needle-like aragonite, rather than participating in actual cementitious reaction like conventional cement. Therefore, after cementitious reaction is completed and interlocking needle-like aragonite is formed, water may remain in cement products. Water may leave pores or voids after evaporation and drying. In addition, reactive vaterite has a lower specific gravity than aragonite, and it is expected that the transition from reactive vaterite to interlocking needle-like aragonite can leave extra pore space or voids in matrix. In some embodiments, the unique interlocking needle-like aragonite in cement products forms a honeycomb structure around one or more voids left by the dissolution of reactive vaterite cement. The unique honeycomb structure with one or more voids surrounded by interlocking needle-like aragonite reduces the bulk density of cement products, and unique interlocking needle-like aragonite provides high compressive strength and durability. As described herein, the ratio of the water of the composition comprising reactive vaterite cement and reactive vaterite cement, average grain size and particle distribution affect the packing density or bulk density of cement products, and therefore, the cement products with the bulk density of variation can be formed by the unique combination of the ratio of the water of the composition comprising reactive vaterite cement and reactive vaterite cement, average grain size and particle distribution.As described herein, in some embodiments, smaller size particles and larger size particles are piled up with the bimodal distribution or the trimodal distribution of reactive vaterite cement, and cause around one or more spaces and form the unique form of the interlocking needle-like aragonite of cellular structure.
[0170] In some embodiments, the aggregate formed by the methods and systems described herein has a porosity between about 10%-90%; has a porosity between about 25-110 lb / ft 3 having a Mohs hardness of less than 6; and / or having a wear resistance of less than 50%.
[0171] In some embodiments, the methods and systems described herein further include when the reactive vaterite cement has a spherical morphology with a diameter of 100-1,000 m 2 / kg specific surface area, and / or with a bimodal distribution, forming 25-65lb / ft 3 The bimodal distribution comprises reactive vaterite cement having an average particle size between 0.1 μm and 10 μm and reactive vaterite cement having an average particle size between 11 μm and 50 μm, wherein the ratio of water to reactive vaterite cement in the wet composition is between about 0.1:1 and 1.2:1.
[0172] In some embodiments, the methods and systems described herein further include when the reactive vaterite cement has a spherical morphology with a diameter of 100-1,000 m 2 / kg specific surface area, and / or with a bimodal distribution, forming 25-65lb / ft 3 The bimodal distribution comprises a reactive vaterite cement having an average particle size between 0.1 μm and 10 μm and a reactive vaterite cement having an average particle size between 11 μm and 50 μm, wherein the ratio of water to reactive vaterite cement in the wet composition is between about 0.1:1 and 1.2:1.
[0173] In some embodiments, the methods and systems described herein further include when the reactive vaterite cement has a spherical morphology with a diameter of 100-1,000 m 2 / kg specific surface area, and / or with trimodal distribution, forming 25-65lb / ft 3 The trimodal distribution comprises reactive vaterite cement A having an average particle size between 0.1 μm and 10 μm, reactive vaterite cement B having an average particle size between 11 μm and 50 μm, and reactive vaterite cement C having an average particle size between 51 μm and 100 μm, wherein the ratio of water to reactive vaterite cement in the wet composition is between about 0.1:1 and 1.2:1.
[0174] In some embodiments, the methods and systems described herein further include when the reactive vaterite cement has a spherical morphology with a diameter of 100-1,000 m 2 / kg specific surface area, and / or with trimodal distribution, forming 25-65lb / ft 3 The trimodal distribution comprises reactive vaterite cement A having an average particle size between 0.1 μm and 10 μm, reactive vaterite cement B having an average particle size between 11 μm and 50 μm, and reactive vaterite cement C having an average particle size between 51 μm and 100 μm, wherein the ratio of water to reactive vaterite cement in the wet composition is between about 0.1:1 and 1.2:1.
[0175] In some embodiments, the methods and systems described herein further include when the reactive vaterite cement has a spherical morphology with a diameter of 100-1,000 m 2 / kg specific surface area, and / or with a bimodal distribution, forming 25-65lb / ft 3The bimodal distribution comprises a reactive vaterite cement B having an average particle size between 11 μm and 50 μm and a reactive vaterite cement C having an average particle size between 51 μm and 100 μm, wherein the ratio of water to reactive vaterite cement in the wet composition is between about 0.1:1 and 1.2:1.
[0176] In some embodiments, the methods and systems described herein further include when the reactive vaterite cement has a spherical morphology with a diameter of 100-1,000 m 2 / kg specific surface area, and / or with a bimodal distribution, forming 25-65lb / ft 3 The bimodal distribution comprises a reactive vaterite cement B having an average particle size between 11 μm and 50 μm and a reactive vaterite cement C having an average particle size between 51 μm and 100 μm, wherein the ratio of water to reactive vaterite cement in the wet composition is between about 0.1:1 and 1.2:1.
[0177] In some embodiments, the methods and systems described herein further comprise producing a reactive vaterite cement prior to the preparing step.Methods and systems for producing reactive vaterite cement compositions have been described herein.
[0178] Method and system for producing reactive vaterite cement compositions
[0179] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the mixture comprising lime in an N-containing salt solution to produce an aqueous solution comprising a calcium salt; and (c) treating the aqueous solution comprising the calcium salt with a gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0180] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the mixture comprising lime in an N-containing salt solution to produce an aqueous solution comprising a calcium salt; (c) treating the aqueous solution comprising the calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; and treating the aqueous solution comprising the calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; (d) mixing the composition comprising reactive vaterite cement A and the composition comprising reactive vaterite cement B to form a composition comprising a bimodal distribution of reactive vaterite cements, wherein the bimodal distribution of reactive vaterite cements comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0181] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) dissolving limestone in an N-salt solution to produce an aqueous solution comprising a calcium salt and a gas stream comprising carbon dioxide; and (b) treating the aqueous solution comprising a calcium salt with the gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0182] In one aspect, a method for producing a cement composition is provided, the method comprising: (a) dissolving limestone in an N-containing salt solution to produce an aqueous solution containing a calcium salt and a gas stream containing carbon dioxide; (b) treating the aqueous solution containing the calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; and treating the aqueous solution containing the calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; (c) mixing the composition containing reactive vaterite cement A and the composition containing reactive vaterite cement B to form a composition containing a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement contains reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0183] In some embodiments of the above aspects, the method also includes forming a composition comprising reactive vaterite cement C having an average particle size between about 51 μm-100 μm; and mixing the composition comprising reactive vaterite cement A and the composition comprising reactive vaterite cement B with the composition comprising reactive vaterite cement C to form a composition comprising a trimodal distribution.
[0184] In some embodiments, the above method can be used to form a bimodal distribution composition of reactive vaterite cement, which comprises reactive vaterite cement B having an average particle size between about 11 μm-50 μm and reactive vaterite cement C having an average particle size between about 51 μm-100 μm.
[0185] It should be understood that reactive vaterite cement compositions having a particular particle size can be formed separately and then mixed to form a bimodal, trimodal, or multimodal distribution and / or mixed reactive vaterite cement compositions having particle sizes can be formed using the methods and systems described herein.
[0186] In some embodiments of the above aspects and embodiments, the method also includes adding water to the cement composition and converting the reactive vaterite cement A and reactive vaterite cement B and / or reactive vaterite cement C into interlocking needle-shaped aragonite and / or calcite and / or carbon aluminate after dissolution and reprecipitation in water.
[0187] In some embodiments of the above aspects and embodiments, the composition comprising reactive vaterite cement A and reactive vaterite cement B and optionally reactive vaterite cement C improves or increases the packing density of the cement paste by between about 1%-35% and / or reduces the viscosity of the cement paste by 10% or more.
[0188] In some embodiments of the foregoing aspects and embodiments, the method further comprises allowing the aragonite and / or calcite to set and harden and form a cement product.
[0189] In one aspect, a system is provided, the system comprising:
[0190] (i) a calcining reactor configured to calcine limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide;
[0191] (ii) a dissolution reactor operably connected to the calcination reactor, the dissolution reactor being configured for dissolving a mixture comprising lime in an aqueous N-containing brine solution to produce an aqueous solution comprising a calcium salt;
[0192] (iii) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured to treat an aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0193] In one aspect, a system is provided, the system comprising:
[0194] (i) a calcining reactor configured to calcine limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide;
[0195] (ii) a dissolution reactor operably connected to the calcination reactor, the dissolution reactor being configured for dissolving a mixture comprising lime in an aqueous N-containing brine solution to produce an aqueous solution comprising a calcium salt;
[0196] (iii) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured for treating an aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm;
[0197] (iv) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured to treat an aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; and
[0198] (v) a mixing reactor operably connected to the treatment reactor, the mixing reactor being configured to mix a composition comprising reactive vaterite cement A and a composition comprising reactive vaterite cement B to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
[0199] In some embodiments of the aforementioned system aspects and embodiments, the processing reactor in the system also forms a composition comprising a trimodal distribution of reactive vaterite cement, wherein the trimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm, reactive vaterite cement B having an average particle size between about 11 μm-50 μm, and reactive vaterite cement C having an average particle size between about 51 μm-100 μm.
[0200] In some embodiments of the aforementioned system aspects and embodiments, a system for forming a cement product is operably connected to a system for producing a bimodal, trimodal or multimodal composition comprising reactive vaterite cement, the system comprising: a mixer system configured to prepare a wet composition by adding water to the bimodal, trimodal or multimodal composition comprising reactive vaterite cement; and a curing system configured to cure the composition to convert the reactive vaterite cement into interlocking acicular aragonite and / or calcite and / or carbonaluminate to form a cement product.
[0201] In some embodiments of the aforementioned aspects and embodiments, the mixer system is a rotary mixer, a static mixer, a pin mixer, a Hobart mixer, a tilted drum mixer, an Omni mixer, a Henschel mixer, a V-mixer, or a Nauta mixer. In some embodiments of the aforementioned aspects and embodiments, the curing system is one or more autoclaves. In some embodiments of the aforementioned aspects and embodiments, the system further comprises a control system configured to remotely and / or automatically control the components of the system.
[0202] In some embodiments of the aforementioned aspects and embodiments, the system also includes a blending reactor operably connected to the processing reactor, and the blending reactor is configured to blend one or more components selected from the group consisting of slag from metal production, Portland cement clinker, calcium aluminate cement clinker, calcium sulfoaluminate clinker, aluminosilicate materials, SCM and combinations thereof with a bimodal, trimodal or multimodal composition comprising a reactive vaterite cement composition.
[0203] In some embodiments of the aforementioned aspects and embodiments, the system further comprises a transfer system operably connected to a processing reactor of a system for producing a composition comprising reactive vaterite cement and a mixer system of a system for forming a cement product, and configured to transfer the composition comprising reactive vaterite cement from the processing reactor to the mixer system.
[0204] The reactive vaterite cement compositions can be prepared using a variety of methods and systems, as further described herein and Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B As shown in the figure. Reactive vaterite cement compositions can be produced using limestone as a raw material, wherein the limestone is used as is in the process or is calcined to form lime. The method and system for producing reactive vaterite cement compositions provided herein have several advantages, such as, but not limited to, reducing carbon dioxide emissions by incorporating carbon dioxide back into the method for forming reactive vaterite cement. The composition of reactive vaterite produced in the method and system provided herein provides such advantages, which include saving operating costs by reducing fuel consumption and reducing carbon footprint. In the method and system provided herein, CO from the calcination of limestone into lime 2 Emissions can be avoided by recapture it back in the cementitious reactive vaterite material (cementitious reactive vaterite material).By recapture carbon dioxide, cement products are likely to eliminate a large amount of cement carbon dioxide emissions and the global total emissions from all sources.This reactive vaterite cement composition provided herein can be used as self cement and / or replaces ordinary portland cement (OPC) or portland cement clinker as SCM wholly or in part.
[0205] In some embodiments, limestone can be used directly to form a reactive vaterite cement composition (e.g. Figure 2B , Figure 3B and Figure 4B ), or the limestone may be calcined to form lime, which may be used to form a reactive vaterite cement composition (e.g. Figure 2A , Figure 3A and Figure 4A The above aspects and embodiments of the methods and systems provided herein are as follows Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B It should be understood that the steps illustrated in the figure may be modified, or the order of the steps may be changed, or more steps may be added or deleted, depending on the desired results.
[0206] Calcination or calcining is a thermal process that causes the thermal decomposition of limestone. As used herein, "limestone" means CaCO 3And may also include other impurities that are normally present in limestone. Limestone is a naturally occurring mineral. The chemical composition of this material may vary from region to region and between different deposits in the same region. Therefore, the lime containing calcium oxide and / or calcium hydroxide obtained from calcining limestone from each natural deposit may be different. Generally, limestone may contain calcium carbonate (CaCO 3 ), magnesium carbonate (MgCO 3 ), silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), iron (Fe), sulfur (S) or other trace elements.
[0207] Limestone deposits are widely distributed. Limestone from various deposits may differ in physicochemical properties and may be classified according to its chemical composition, texture, and geological formation. Limestone may be classified into the following types: high-calcium limestone, in which the carbonate content may comprise primarily calcium carbonate, with the magnesium carbonate content not exceeding 5%; magnesium limestone, which may comprise approximately 5% to 35% magnesium carbonate; or dolomitic limestone, which may comprise between 35% and 46% MgCO. 3 , the balance is calcium carbonate. Limestone from different sources may differ significantly in chemical composition and physical structure. It should be understood that the methods and systems provided herein are applicable to all cement plants that calcine limestone from any source listed above or from commercial sources. Quarries include, but are not limited to, quarries associated with cement kilns, limestone quarries for aggregates used in concrete, limestone quarries (roadbeds) for other purposes, and / or quarries associated with lime kilns.
[0208] Limestone calcination is a decomposition process in which the chemical reactions used to decompose the limestone are:
[0209] CaCO 3 →CaO+CO 2 (g).
[0210] This step is Figure 2A , Figure 3A and Figure 4A The first step of calcining limestone to form lime is shown in the figure. However, in some embodiments, the calcining step can be omitted and limestone is used directly as a raw material ( Figure 2B , Figure 3B and Figure 4B ).
[0211] In some embodiments, limestone is included in magnesium between about 1%-70% and / or magnesium-containing minerals are mixed with limestone before calcination, wherein the magnesium-containing minerals are included in magnesium between about 1%-70%. In some embodiments, magnesium forms magnesium oxide when calcined, and once formed, magnesium oxide can be precipitated and / or incorporated into reactive vaterite cement. In some embodiments, magnesium-containing minerals include magnesium carbonate, magnesium salts, magnesium hydroxide, magnesium silicate, magnesium sulfate or its combination. In some embodiments, magnesium-containing minerals include but are not limited to dolomite, magnesite, brucite, carnallite, talc, olivine, hydromagnesite, hydromagnesite, magnesite, magnesite, dimagnesite, hydromagnesite, magnesite, magnesite and its combination. In some embodiments, the magnesium oxide in the reactive vaterite cement composition is converted into magnesium hydroxide when in contact with water, and magnesium hydroxide can be combined with the converted aragonite and / or calcite.
[0212] "Lime" as used herein refers to calcium oxide and / or calcium hydroxide. The presence and amount of calcium oxide and / or calcium hydroxide in lime will vary according to the conditions under which the lime is formed. Lime can be in dry form, i.e. calcium oxide, and / or in wet form, such as calcium hydroxide, depending on the conditions. The production of lime may depend on the type of kiln, the conditions of calcination, and the properties of the raw material, i.e. limestone. In some embodiments, at relatively low calcination temperatures, the product formed in the kiln may contain both unburned carbonate and lime, and may be referred to as unburned lime. In some embodiments, as the temperature rises, lightly burned lime or highly reactive lime may be produced. In some embodiments, at still higher temperatures, dead-burned lime or low-reactive lime may be produced. When the reaction front reaches the core of the charged limestone and converts all the carbonates present into lime, lightly burned lime is produced. High-yield products may be relatively soft, contain small lime crystallites and have an open porous structure that is easily accessible inside. Such lime may have the best properties of high reactivity, high surface area, and low bulk density. Increasing the degree of calcination beyond this stage may make the lime crystallites larger, agglomerated, and sintered. This may result in a reduction in surface area, porosity and reactivity and an increase in bulk density. Such a product may be referred to as dead burnt lime or low reactive lime. Without being limited by any theory, the methods and systems provided herein form and utilize any one or combination of the above limes. Thus, in some embodiments, the lime is dead burnt lime, light burnt lime, underburnt lime, or a combination thereof. In some embodiments, the lime is dead burnt lime. In some embodiments, the lime is underburnt lime. In some embodiments, the lime is light burnt lime. In some embodiments, the lime is dead burnt lime, light burnt lime, or a combination thereof.
[0213] The production of lime by calcining limestone can be carried out using various types of kilns, such as but not limited to vertical kilns or rotary kilns or electric kilns. The use of electric kilns in calcining and the advantages associated therewith have been described in U.S. Application No. 17 / 363,537 filed on June 30, 2021, which is fully incorporated herein by reference in its entirety.
[0214] These devices for calcining are suitable for calcining limestone in the form of agglomerates having a diameter of a few millimeters to tens of millimeters. Cement plant waste streams include waste streams from both wet and dry plants, which may employ shaft kilns, rotary kilns, electric kilns or a combination thereof, and may include pre-calciners. These industrial plants may each burn a single fuel, or may burn two or more fuels sequentially or simultaneously.
[0215] like Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B As shown in FIG. 1 , limestone obtained from a limestone quarry is used directly or undergoes calcination in a cement plant, resulting in the formation of lime and CO 2 Gas. Lime can be calcium oxide in solid form from a dry kiln / cement process and / or can be a combination of calcium oxide and calcium hydroxide in slurry form in a wet kiln / cement process. When wet, calcium oxide (also known as an alkali anhydride, which is converted to its hydroxide form in water) can exist in its hydrated form, such as but not limited to calcium hydroxide. Although calcium hydroxide (also known as slaked lime) is a common hydrated form of calcium oxide, other intermediate hydrated complexes and / or water complexes can also be present in the slurry and are all included within the scope of the methods and systems provided herein. It should be understood that although lime is illustrated as CaO in some of the figures herein, it can be present as Ca(OH) 2 or CaO and Ca(OH) 2 The combination exists.
[0216] Lime or limestone can be slightly soluble in water. In the methods and systems provided herein, the solubility of lime or limestone is increased by treating it with a solubilizing agent.
[0217] In the methods and systems provided herein, lime or limestone is solvated or dissolved or solubilized with a solubilizing agent (in Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B Step A) in step A) to produce an aqueous solution containing a calcium salt. For illustration purposes only, the solubilizing agent, such as an N-containing salt solution, is illustrated in the accompanying drawings as ammonium chloride (NH4 Cl) solution, and the subsequent calcium salt is illustrated as calcium chloride (CaCl 2 Various examples of N-containing salts have been provided herein and are within the scope of the present invention.
[0218] In some embodiments, the N-containing salt solution solubilizes or dissolves calcium from lime or limestone and leaves behind solid impurities. The N-containing salt includes, but is not limited to, an N-containing inorganic salt, an N-containing organic salt, or a combination thereof.
[0219] As used herein, "N-containing inorganic salt" includes any inorganic salt containing nitrogen. Examples of N-containing inorganic salts include, but are not limited to, ammonium acetate, ammonium halides (halides are any halogens), ammonium sulfate, ammonium sulfite, ammonium nitrate, ammonium nitrite, and the like. In some embodiments, the ammonium halide is ammonium chloride or ammonium bromide. In some embodiments, the ammonium halide is ammonium chloride.
[0220] As used herein, "N-containing organic salt" includes any salt of an organic compound containing nitrogen therein. Examples of N-containing organic compounds include, but are not limited to, aliphatic amines, alicyclic amines, heterocyclic amines, and combinations thereof.
[0221] As used herein, "aliphatic amines" include those of formula (R) n -NH 3-n Any alkylamine, wherein n is an integer from 1 to 3, wherein R is independently a linear or branched and substituted or unsubstituted alkyl group between C1 and C8. Formula (R) n -NH 3-n Examples of the corresponding halide salts (chloride salts, bromide salts, fluoride salts or iodide salts) of the alkylamine of are (R) n -NH 4-n + Cl - In some embodiments, when R is substituted alkyl, the substituted alkyl is independently substituted with halogen, hydroxy, acid and / or ester.
[0222] For example, when R is (R) n -NH 3-n When the alkyl group in the formula (a) is alkyl, the alkylamine may be a primary alkylamine, such as, by way of example only, methylamine, ethylamine, butylamine, pentylamine, etc.; the alkylamine may be a secondary amine, such as, by way of example only, dimethylamine, diethylamine, methylethylamine, etc.; and / or the alkylamine may be a tertiary amine, such as, by way of example only, trimethylamine, triethylamine, etc.
[0223] For example, when R is in (R) n -NH 3-n When the substituted alkyl group is substituted by a hydroxyl group, the substituted alkylamine is an alkanolamine, including but not limited to a monoalkanolamine, a dialkanolamine or a trialkanolamine, such as, for example, monoethanolamine, diethanolamine or triethanolamine.
[0224] For example, when R is in (R) n -NH 3-n In the case of a substituted alkyl group substituted by a halogen, examples of the substituted alkylamine include chloromethylamine, bromomethylamine, chloroethylamine, bromoethylamine and the like.
[0225] For example, when R is in (R) n -NH 3-n In some embodiments, the amino acid is a substituted alkyl amine substituted with an acid, for example, an amino acid. In some embodiments, the amino acid has a polar uncharged alkyl chain, examples include but are not limited to serine, threonine, asparagine, glutamine or a combination thereof. In some embodiments, the amino acid has a charged alkyl chain, examples include but are not limited to arginine, histidine, lysine, aspartic acid, glutamic acid or a combination thereof. In some embodiments, the amino acid is glycine, proline or a combination thereof.
[0226] As used herein, "alicyclic amines" include those of formula (R) n -NH 3-n Any alicyclic amine of, wherein n is an integer from 1-3, wherein R is independently one or more all-carbon rings, which may be saturated or unsaturated, but not aromatic. The alicyclic compound may have one or more aliphatic side chains attached. Formula (R) n -NH 3-n An example of a corresponding salt of an alicyclic amine is (R) n -NH 4-n + Cl - Examples of alicyclic amines include, but are not limited to, cycloalkylamines: cyclopropylamine, cyclobutylamine, cyclopentylamine, cyclohexylamine, cycloheptylamine, cyclooctylamine, and the like.
[0227] As used herein, "heterocyclic amines" include at least one heterocyclic aromatic ring attached to at least one amine. Examples of heterocycles include, but are not limited to, pyrrole, pyrrolidine, pyridine, pyrimidine, and the like. Such chemicals are well known in the art and are commercially available.
[0228] In the methods and systems provided herein, limestone or lime is dissolved or solubilized with a nitrogen-containing salt solution (step A) to produce an aqueous solution containing calcium salts. The dissolving step can form ammonia (in Figure 2A and Figure 2B ) and / or forming a gas stream comprising ammonia (in Figure 3A , Figure 3B , Figure 4A and Figure 4B (shown in the figure).
[0229] like Figure 2A , Figure 3A and Figure 4A As shown in step A, the N-containing salt is ammonium chloride (NH 4 When the possible reaction is the following, lime is reacted with NH 4 Cl (fresh and recycled, as explained further below) is solubilized by treatment:
[0230] CaO+2NH 4 Cl(aqueous solution) → CaCl 2 (aqueous solution) + 2NH 3 +H 2 O
[0231] Ca(OH) 2 +2NH 4 Cl(aqueous solution) → 2NH 3 +CaCl 2 +2H 2 O.
[0232] Similarly, when the N-containing salt is an organic N-containing salt, the reaction may be as follows:
[0233] CaO+2NH 3 RCl → CaCl 2 (aqueous solution) + 2NH 2 R+H 2 O.
[0234] Similarly, if Figure 2B , Figure 3B and Figure 4B As shown in step A, the N-containing salt is ammonium chloride (NH 4 When the possible reaction is as follows, limestone is reacted with NH 4 Cl (fresh and recycled, as explained further below) is solubilized by treatment:
[0235] CaCO 3 (Limestone)+2NH 4 Cl → CaCl 2 (aqueous solution) + 2NH 3 +CO 2 +H 2 O.
[0236] Similarly, when the base is a N-containing organic salt, the reaction can be as follows:
[0237] CaCO 3 (Limestone)+2NH 3 RCl → CaCl 2 (aqueous solution) + 2NH 2 R+CO2 +H 2 O.
[0238] In some embodiments, the base or N-containing inorganic salt such as, but not limited to, an ammonium salt, for example, an ammonium chloride solution, may be supplemented with anhydrous ammonia or an aqueous ammonia solution to maintain an optimal level of ammonium chloride in the solution.
[0239] In some embodiments, the aqueous solution containing calcium salts obtained after dissolution of lime or limestone may contain sulfur, depending on the source of the limestone. Sulfur may be introduced into the aqueous solution after solubilization of the lime or limestone with any of the N-containing salts described herein. In alkaline solutions, a variety of sulfur compounds including a variety of sulfide species may be present in the solution, including but not limited to sulfites (SO 3 2- ), sulfate (SO 4 2- ), Hydrogen sulfide (HS - ), thiosulfate (S 2 O 3 2- ), polysulfide (S n 2- ), thiol (RSH) analogs. As used herein, "sulfur compound" includes any compound containing a sulfide ion.
[0240] In some embodiments, the aqueous solution further comprises a N-containing salt, such as ammonia and / or an inorganic N-containing salt or an organic N-containing salt.
[0241] In some embodiments, the amount of N-containing inorganic salt, N-containing organic salt or combination thereof is more than 20% excess or more than 30% excess relative to lime or limestone. In some embodiments, the molar ratio of N-containing salt: lime (or N-containing inorganic salt: lime or N-containing organic salt: lime or ammonium chloride: lime) or the molar ratio of N-containing salt: limestone (or N-containing inorganic salt: limestone or N-containing organic salt: limestone or ammonium chloride: limestone) is between 0.5:1-2:1; or between 0.5:1-1.5:1; or between 1:1-1.5:1; or 1.5:1; or 2:1; or 2.5:1; or 1:1.
[0242] In some embodiments of the methods and systems described herein, the dissolving step is performed under one or more dissolution conditions selected from the group consisting of: between about 30°C-200°C, or between about 30°C-150°C, or between about 30°C-100°C, or between about 30°C-75°C, or between about 30°C-50°C, or between about 40°C-200°C, or between about 40°C-150°C, or between about 40°C-100°C, or between about 40°C-75°C, or between about 40°C-50°C, or between about 50°C-200°C, or between about 40°C-150°C, or between about 40°C-100°C, or between about 40°C-75°C, or between about 40°C-50°C, or between about 50°C-200°C, or between about A temperature between 50°C-150°C, or between about 50°C-100°C; a pressure between about 0.1-50atm, or between about 0.1-40atm, or between about 0.1-30atm, or between about 0.1-20atm, or between about 0.1-10atm, or between about 0.5-20atm; a wt% of a N-containing inorganic salt or a N-containing organic salt in water between about 0.5%-50%, or between about 0.5%-25%, or between about 0.5%-10%, or between about 3%-30%, or between about 5%-20%; or a combination thereof.
[0243] Agitation can be used to affect the dissolution of lime or limestone and N-containing salt solution in the dissolution reactor, for example by eliminating hot spots and cold spots to optimize the dissolution / solvation of lime or limestone, and high shear mixing, wet grinding and / or ultrasonic treatment can be used to crush the lime or limestone. During or after high shear mixing and / or wet grinding, the lime or limestone suspension can be treated with N-containing salt solution.
[0244] In some embodiments, dissolving lime or limestone with a N-containing salt solution (illustrated as, for example, ammonium chloride) results in an aqueous solution comprising calcium salts and solids. In some embodiments, solid insoluble impurities ( Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and 4B The solids may optionally be removed from the aqueous solution by filtration and / or centrifugation techniques.
[0245] It should be understood that Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and 4B Step B in the step is optional, and in some embodiments, the solid may not be removed from the aqueous solution (not shown in the figure), and the aqueous solution containing the calcium salt and the solid is contacted with carbon dioxide (at Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and 4B In step C) to form a precipitate. In such embodiments, the precipitation material also comprises a solid.
[0246] In some embodiments, the solids obtained from the dissolution of lime or limestone (in Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and 4B ) is a calcium-poor solid and can be used as a cement substitute (such as a substitute for Portland cement). In some embodiments, the solid comprises silicate, iron oxide, aluminum oxide, or a combination thereof. Silicates include, but are not limited to, clays (phyllosilicates), aluminosilicates, and the like.
[0247] In some embodiments, the solids are between about 1 wt%-85 wt%; or between about 1 wt%-80 wt%; or between about 1 wt%-75 wt%; or between about 1 wt%-70 wt%; or between about 1 wt%-60 wt%; or between about 1 wt%-50 wt%; or between about 1 wt%-40 wt%; or between about 1 wt%-30 wt%; or between about 1 wt%-20 wt%; or between about 1 wt%-10 wt% or between about 1 wt%-5 wt%; or between about 1 wt%-2 wt% in the aqueous solution, in the precipitation material, or a combination thereof.
[0248] like Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and 4B As shown in step C of , an aqueous solution comprising a calcium salt (and optionally a solid) and dissolved ammonia and / or ammonium salt is contacted with a gas stream comprising carbon dioxide recycled from the calcination step of a limestone calcination process or the dissolution step of a direct limestone process to form a precipitation material comprising calcium carbonate, wherein the calcium carbonate comprises reactive vaterite, as shown in the following reaction:
[0249] CaCl 2 (aqueous solution) + 2NH 3 (aqueous solution) + CO 2 (g)+H 2 O-->CaCO 3 (s)+2NH 4 Cl (aqueous solution).
[0250] CO 2Absorption into aqueous solution produces a charge CO containing carbonic acid 2 of water, carbonic acid being a substance in equilibrium with both bicarbonate and carbonate. The precipitation material is prepared under one or more precipitation conditions suitable for forming a reactive vaterite cement material, as described herein.
[0251] In one aspect, the ammonia formed in the dissolving step A may be partially or completely present in gaseous form. Figure 3A and Figure 3B As shown in the figure.
[0252] In one aspect, a method for forming a reactive vaterite cement composition is provided by the following steps: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the mixture comprising lime in a nitrogen-containing salt solution to produce an aqueous solution comprising a calcium salt and a gas stream comprising ammonia; and (c) treating the aqueous solution comprising a calcium salt with a gas stream comprising carbon dioxide and a gas stream comprising ammonia to form a reactive vaterite cement composition. This aspect is Figure 3A The middle figure shows that the CO 2 The gas stream and the gas stream from step A of the process containing NH 3 The gas stream is recycled to the precipitation reactor (step C) for forming reactive vaterite cement. Figure 3A The remaining steps are Figure 2A It should be understood that Figure 2A and Figure 3A Both processes may also take place simultaneously, so that the N-containing salt, such as an inorganic N-containing salt or an organic N-containing salt and optionally ammonia may be present partly in the aqueous solution and partly in the gas stream.
[0253] The reactions occurring in the above aspects can be shown as follows:
[0254] CaCl 2 (aqueous solution) + 2NH 3 (g)+CO 2 (g)+H 2 O-->CaCO 3 (s)+2NH 4 Cl (aqueous solution).
[0255] In one aspect, a method for forming a reactive vaterite cement composition is provided by the following steps: (a) dissolving limestone in a nitrogen-containing salt solution to produce an aqueous solution containing a calcium salt, and a gas stream containing ammonia and a gas stream containing carbon dioxide; and (c) treating the aqueous solution containing the calcium salt with a gas stream containing carbon dioxide and a gas stream containing ammonia to form a reactive vaterite cement composition. This aspect is Figure 3B The diagram shows that the CO2 The airflow and the NH 3 The gas stream is recycled to the precipitation reactor (step C) for forming reactive vaterite cement. Figure 3B The remaining steps are Figure 2B It should be understood that Figure 2B and Figure 3B Both processes may also take place simultaneously, so that the N-containing salt, such as an inorganic N-containing salt or an organic N-containing salt and optionally ammonia may be present partly in the aqueous solution and partly in the gas stream.
[0256] In some embodiments of the aspects and embodiments provided herein, the gas stream comprising ammonia can have ammonia from an external source and / or be recovered and recycled from step A of the process.
[0257] In some embodiments of the aspects and embodiments provided herein, wherein the gas stream comprises ammonia and / or the gas stream comprises carbon dioxide, no external source of carbon dioxide and / or ammonia is used, and the process is a closed-loop process. Such a closed-loop process is illustrated in the figures described herein.
[0258] In some embodiments, the dissolution of lime or limestone with some N-containing organic salts may not result in the formation of ammonia gas, or the amount of ammonia gas formed may not be very large. In embodiments where ammonia gas is not formed or is not formed in a large amount, Figure 2A and Figure 2B The method and system illustrated in is applicable, wherein the aqueous solution containing the calcium salt is treated with carbon dioxide gas. In such an embodiment, the organic amine salt can remain in the aqueous solution in a completely or partially dissolved state, or can be separated into an organic amine layer, as shown in the following reaction:
[0259] CaO+2NH 3 R + Cl - →CaCl 2 (aqueous solution) + 2NH 2 R+H 2 O.
[0260] The N-containing organic salt or N-containing organic compound remaining in the supernatant solution after precipitation may be referred to as residual N-containing organic salt or residual N-containing organic compound. Methods and systems for recovering residual compounds from precipitates and supernatant solutions have been described herein.
[0261] In one aspect, ammonia and CO can be recovered prior to mixing the cooled solution with the aqueous solution comprising a calcium salt. 2 The gas is cooled in a cooling reactor. Figure 4A and Figure 4B As shown in the figure.
[0262] In one aspect, a method for forming a reactive vaterite cement composition is provided by the following steps: (i) calcining limestone to form lime and a gas stream containing carbon dioxide; (ii) dissolving lime in an aqueous solution of an inorganic salt containing N or an organic salt containing N to produce a first aqueous solution containing a calcium salt and a gas stream containing ammonia; (iii) recovering a gas stream containing carbon dioxide and a gas stream containing ammonia, and subjecting the gas stream to a cooling process to condense a second aqueous solution containing ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof; and (iv) treating the first aqueous solution containing a calcium salt with a second aqueous solution containing ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof to form a reactive vaterite cement composition. This aspect is Figure 4A The middle figure shows that the CO 2 The gas stream and the gas stream from step A of the process containing NH 3 The gas stream is recycled to the cooled reactor / reaction (step F) for forming carbonate and bicarbonate solutions as shown in further reactions below. Figure 4A The remaining steps are Figure 2A and Figure 3A The steps are the same.
[0263] It should be understood that Figure 4A The above aspects illustrated in FIG can be combined with Figure 2A and / or Figure 3A The combination of aspects illustrated in FIG. 1, wherein the precipitation step C comprises treating the first aqueous solution comprising the calcium salt (at Figure 4A ), and comprising treating an aqueous solution comprising a calcium salt (in Figure 2A and / or comprising treating an aqueous solution comprising a calcium salt (in Figure 3A ). In such an embodiment, the gas stream containing carbon dioxide is divided into a stream flowing to the cooling process and a stream flowing to the precipitation process. Similarly, in such an embodiment, the gas stream containing ammonia is divided into a stream flowing to the cooling process and a stream flowing to the precipitation process. Figure 2A , Figure 3A and Figure 4A Any combination of the processes depicted in is possible and is within the scope of the present disclosure.
[0264] In one aspect, a method for forming a reactive vaterite cement composition is provided by the following steps: (i) dissolving limestone in an aqueous solution of an inorganic salt containing N or an organic salt containing N to produce a first aqueous solution containing a calcium salt, a gas stream containing carbon dioxide, and a gas stream containing ammonia; (ii) recovering the gas stream containing carbon dioxide and the gas stream containing ammonia and subjecting the gas stream to a cooling process to condense a second aqueous solution containing ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof; and (iii) treating the first aqueous solution containing a calcium salt with a second aqueous solution containing ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof to form a reactive vaterite cement composition. This aspect is Figure 4B The diagram in FIG. 2 shows that the CO 2 The airflow and the NH 3 The gas stream is recycled to the cooled reactor / reaction (step F) for forming carbonate and bicarbonate solutions as shown in further reactions below. Figure 4B The remaining steps are Figure 2B and Figure 3B The steps are the same.
[0265] It should be understood that Figure 4B The above aspects illustrated in FIG can be combined with Figure 2B and / or Figure 3B The combination of aspects illustrated in FIG. 1, wherein the precipitation step C comprises treating the first aqueous solution comprising the calcium salt (at Figure 4B ), and comprising treating an aqueous solution comprising a calcium salt (in Figure 2B and / or comprising treating an aqueous solution comprising a calcium salt (in Figure 3B ). In such an embodiment, the gas stream containing carbon dioxide is divided into a stream flowing to the cooling process and a stream flowing to the precipitation process. Similarly, in such an embodiment, the gas stream containing ammonia is divided into a stream flowing to the cooling process and a stream flowing to the precipitation process. Figure 2B , Figure 3B and Figure 4B Any combination of the processes depicted in is possible and is within the scope of the present disclosure.
[0266] Ammonium carbamate has an ammonium ion NH 4 + and carbamate ions H 2 NCO 2 - The formula is NH 4 [H 2 NCO 2 ].
[0267] The combination of these condensed products in the second aqueous solution may depend on one or more of the cooling conditions during the cooling step.
[0268] In some embodiments of the above aspects and embodiments, the gas stream (e.g., the gas stream flowing to the cooling reaction / reactor ( Figure 4A and Figure 4B In some embodiments of the above aspects and embodiments, the gas stream further comprises between about 20% and 90%; or between about 20% and 80%; or between about 20% and 70%; or between about 20% and 60%; or between about 20% and 55%; or between about 20% and 50%; or between about 20% and 40%; or between about 20% and 30%; or between about 20% and 25%; or between about 30% and 90%; or between about 30% and 80%; or between about 30% and 70%; or between about 30% and 60%; or between about 30% and 50%; or between about or about 30%-40%; or about 40%-90%; or about 40%-80%; or about 40%-70%; or about 40%-60%; or about 40%-50%; or about 50%-90%; or about 50%-80%; or about 50%-70%; or about 50%-60%; or about 60%-90%; or about 60%-80%; or about 60%-70%; or about 70%-90%; or about 70%-80%; or about 80%-90% water vapor.
[0269] Intermediate steps in cooling the reaction / reactor may include forming ammonium carbonate and / or ammonium bicarbonate and / or ammonium carbamate by the following reactions:
[0270] 2NH 3 +CO 2 +H 2 O→(NH 4 ) 2 CO 3
[0271] NH 3 +CO 2 +H 2 O→(NH 4 )HCO 3
[0272] 2NH 3 +CO 2 →(NH 4 )NH 2 CO 2 .
[0273] For N-containing organic salts, a similar reaction can be shown:
[0274] 2NH 2 R+CO 2 +H 2 O→(NH 3 R) 2 CO 3
[0275] NH 2 R+CO 2 +H 2 O→(NH 3 R)HCO 3 .
[0276] The advantage of cooling ammonia in a cooling reaction / reactor is that ammonia may have a limited vapor pressure in the gas phase of the solution reaction. As shown in the above reaction, by reacting ammonia with CO 2 The reaction may remove some ammonia from the vapor space, allowing more ammonia to leave the dissolved solution.
[0277] A second aqueous solution (leaving Figure 4A and Figure 4B The reaction mixture is then treated in a precipitation reaction / reactor with the first aqueous solution containing the calcium salt from the dissolution reaction / reactor (step C) to form a precipitation material containing reactive vaterite cement:
[0278] (NH 4 ) 2 CO 3 +CaCl 2 →CaCO 3 (Vaterite)+2NH 4 Cl
[0279] (NH 4 )HCO 3 +NH 3 +CaCl 2 →CaCO 3 (Vaterite)+2NH 4 Cl+H 2 O
[0280] 2(NH 4 )HCO 3 +CaCl 2 →CaCO 3 (Vaterite)+2NH 4 Cl+H 2 O+CO 2
[0281] (NH4 )NH 2 CO 2 +H 2 O+CaCl 2 →CaCO 3 (Vaterite)+2NH 4 Cl.
[0282] In some embodiments of the aspects and embodiments provided herein, the cooling step is performed under one or more cooling conditions, comprising a temperature between about 0°C-200°C, or between about 0°C-150°C, or between about 0°C-75°C, or between about 0°C-100°C, or between about 0°C-80°C, or between about 0°C-60°C, or between about 0°C-50°C, or between about 0°C-40°C, or between about 0°C-30°C, or between about 0°C-20°C, or between about 0°C-10°C.
[0283] In some embodiments of the aspects and embodiments provided herein, one or more cooling conditions include a pressure between about 0.5-50 atm; or between about 0.5-25 atm; or between about 0.5-10 atm; or between about 0.1-10 atm; or between about 0.5-1.5 atm; or between about 0.3-3 atm.
[0284] In some embodiments, the formation, particle size or distribution thereof, and quality of the reactive vaterite formed in the methods and systems provided herein depend on the amount and / or ratio of condensation products in the second aqueous solution comprising ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof.
[0285] In some embodiments, the presence or absence or distribution of condensation products in the second aqueous solution comprising ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof can be selected to maximize the formation of reactive vaterite and / or obtain a desired particle size distribution. The selection can be based on one or more cooling conditions, such as the pH of the aqueous solution in the cooling reactor, CO 2 and NH 3 Gas flow and / or CO 2 :NH 3 The inlet of the cooling reactor can be carbon dioxide (CO 2(g) ), including ammonia (NH 3(g) ) of the dissolved reactor off-gas, water vapor and optionally fresh make-up water (or some other dilution water stream). The outlet can be a slip stream of the reactor recycle fluid (second aqueous solution) which is directed to the precipitation reactor for contact with the first aqueous solution and optionally additional carbon dioxide and / or ammonia. The pH of the system can be adjusted by adjusting the CO 2 and NH 3The conductivity of the system can be controlled by adding dilution makeup water to the cooling reactor. The volume can be kept constant by using a level detector in the cooling reactor or its reservoir.
[0286] It should be understood that although Figure 4A and Figure 4B A separate cooling reaction / reactor is shown, but in some embodiments, the dissolution reaction / reactor can be integrated with the cooling reaction / reactor. For example, the dissolution reactor can be integrated with a condenser that acts as a cooling reactor. Various configurations of the integrated reactor described above are described in U.S. Application Serial No. 17 / 184,933, filed on February 25, 2021, which is incorporated herein by reference in its entirety.
[0287] In the above-mentioned aspect, both dissolution reactor and cooling reactor are equipped with inlet and outlet, to receive required gas and collect water flow.In some embodiments of the above-mentioned aspect, dissolution reactor comprises agitator to mix lime or limestone with N-containing salt water solution.Agitator can also promote the upward movement of gas.In some embodiments of the above-mentioned aspect, dissolution reactor is configured to collect the solids settled in reactor bottom after removing the first aqueous solution comprising calcium salt.In some embodiments of the above-mentioned aspect, cooling tower comprises one or more trays, and the tray is configured to capture and collect the second aqueous solution of condensation, and prevents it from falling back in the dissolution reactor.Like this, cooling / condensation can be realized by using injector, bubbler, fluid venturi reactor, sprayer, gas filter, atomizer, tray or filling column reactor and the like.
[0288] In some embodiments, the contacting of the aqueous solution comprising the calcium salt with carbon dioxide and optionally ammonia or a second aqueous solution is achieved by contacting the aqueous solution using a convenient protocol (precipitation conditions) as described herein to reach and maintain a desired pH range, a desired temperature range, and / or a desired divalent cation concentration. In some embodiments, the system comprises a precipitation reactor configured to contact the aqueous solution comprising the calcium salt with carbon dioxide and optionally ammonia from step A of the process, or the system comprises a precipitation reactor configured to contact a first aqueous solution comprising the calcium salt with a second aqueous solution comprising ammonium bicarbonate, ammonium carbonate, ammonia, ammonium carbamate, or a combination thereof.
[0289] In some embodiments, the aqueous solution comprising a calcium salt can be placed in a precipitation reactor, wherein the amount of the aqueous solution comprising a calcium salt added is sufficient to raise the pH to a desired level (e.g., a pH that induces precipitation of precipitation material), such as pH 7-9, pH 7-8.7, pH 7-8.5, pH 7-8, pH 7.5-8, pH 8-8.5, pH 8.5-9, pH 9-14, pH 10-14, pH 11-14, pH 12-14, or pH 13-14. In some embodiments, when combined with carbon dioxide and optionally NH 3 When contacting the first or second aqueous solution, the pH of the aqueous solution containing the calcium salt is maintained between 7-9, or between 7-8.7, or between 7-8.5, or between 7.5-8.5, or between 7-8, or between 7.6-8.5, or between 8-8.5, or between 7.5-9.5 to form reactive vaterite.
[0290] Any convenient protocol may be used to mix the aqueous solution comprising the calcium salt with the solution comprising CO. 2 and optionally NH 3 The gas flow of the first aqueous solution is contacted. The contact scheme of interest includes but is not limited to direct contact scheme (for example, gas bubbling is passed through the first aqueous solution), simultaneous contact mode (that is, contact between the gas phase flow and the liquid phase flow of unidirectional flow), countercurrent mode (that is, contact between the gas phase flow and the liquid phase flow of reverse flow) and similar schemes. Therefore, contact can be achieved by using an injector, a bubbler, a fluid venturi reactor, a sprinkler, a gas filter, a sprayer, a tray or a packed column reactor and the like in a precipitation reactor. In some embodiments, gas-liquid contact is achieved by forming a liquid sheet of the solution with a flat nozzle, wherein the gas and liquid sheet move in a countercurrent direction, a downstream direction or a cross-current direction or in any other suitable manner. In some embodiments, gas-liquid contact is achieved by contacting a droplet of a solution with a gas source having a mean diameter of 500 microns or less, such as 100 microns or less.
[0291] Any number of gas-liquid contact schemes described herein can be used.Continue gas-liquid contact or liquid-liquid contact, until the pH of the precipitation reaction mixture is best (multiple optimum pH values have been described herein, to form a precipitation material comprising for example reactive vaterite), allow to stir the precipitation reaction mixture afterwards.The speed that pH declines can be controlled by adding more aqueous solutions comprising calcium salts during gas-liquid contact or liquid-liquid contact.In addition, other aqueous solutions can be added after bubbling so that pH is raised back to alkaline levels, for precipitating part or all of precipitation material.In any case, precipitation material can be formed when removing protons from some material in the precipitation reaction mixture.Then the precipitation material comprising carbonate can be separated, and optionally further processed.
[0292] One or more precipitation conditions comprise the environment of regulating the precipitation reaction mixture to produce those conditions of the required precipitation material comprising reactive vaterite.Such one or more precipitation conditions include but are not limited to the existence of temperature, pH, pressure, ion ratio, precipitation rate, additive, the existence of ionic material, the concentration of additive and ionic material, stirring, residence time, mixing rate, agitation form such as ultrasonic wave, the existence of seed, catalyst, film or substrate, dehydration, drying, ball milling etc.In some embodiments, the average grain size of reactive vaterite can also depend on one or more precipitation conditions used in the precipitation of precipitation material.
[0293] For example, the temperature of the precipitation reaction can be raised to a point where an amount of precipitation suitable for the desired precipitation material occurs. In such embodiments, the temperature of the precipitation reaction can be raised to values such as from 20°C to 60°C, and including from 25°C to 60°C; or from 30°C to 60°C; or from 35°C to 60°C; or from 40°C to 60°C; or from 50°C to 60°C; or from 25°C to 50°C; or from 30°C to 50°C; or from 35°C to 50°C; or from 40°C to 50°C; or from 25°C to 40°C; or from 30°C to 40°C; or from 25°C to 30°C. In some embodiments, the temperature of the precipitation reaction can be raised using energy generated from a low carbon dioxide emission source or a zero carbon dioxide emission source (e.g., solar energy, wind energy, hydroelectric energy, waste heat from flue gas from a carbon emitter, etc.).
[0294] The pH of the precipitation reaction can also be increased to the amount of precipitation that is suitable for the required precipitation material. In such embodiments, the pH of the precipitation reaction can be increased to an alkaline level for precipitation. In some embodiments, the precipitation conditions required for forming the precipitation material include a pH higher than 7 or a pH of 8 or a pH between 7.1-8.5 or a pH between 7.5-8 or a pH between 7.5-8.5 or a pH between 8-8.5 or a pH between 8-9 or a pH between 7.6-8.4, so as to form the precipitation material. The pH can be increased to pH 9 or higher, for example pH 10 or higher, including pH 11 or higher or pH 12.5 or higher.
[0295] Adjusting the major ion ratio during precipitation may affect the properties of the precipitation material. The major ion ratio may have a considerable effect on polymorph formation. For example, as the magnesium:calcium ratio in the water increases, aragonite may become the major polymorph of calcium carbonate in the precipitation material, rather than low-magnesium vaterite. At low magnesium:calcium ratios, low-magnesium calcite may become the major polymorph. In some embodiments, wherein Ca 2+ and Mg 2+ Both exist, Ca in the precipitated material 2+ With Mg 2+ (i.e. Ca 2+ Mg 2+ ) is 1:1 to 1:2.5; 1:2.5 to 1:5; 1:5 to 1:10; 1:10 to 1:25; 1:25 to 1:50; 1:50 to 1:100; 1:100 to 1:150; 1:150 to 1:200; 1:200 to 1:250; 1:250 to 1:500; or 1:500 to 1:1000. In some embodiments, the Mg content of the precipitation material is Mg(II). 2+ With Ca 2+ (i.e. Mg 2+ :Ca 2+ ) in a ratio of 1:1 to 1:2.5; 1:2.5 to 1:5; 1:5 to 1:10; 1:10 to 1:25; 1:25 to 1:50; 1:50 to 1:100; 1:100 to 1:150; 1:150 to 1:200; 1:200 to 1:250; 1:250 to 1:500; or 1:500 to 1:1000.
[0296] In some embodiments, as described above, one or more precipitation conditions producing the desired precipitation material from the precipitation reaction can include temperature and pH, and in some cases, the concentration of additives and ionic substances in water.Additives have been described in this article.The presence of additives and the concentration of additives can also be conducive to the formation of stable or reactive vaterite or PCC.In some embodiments, medium-chain fatty acid esters or long-chain fatty acid esters can be added to the first aqueous solution to form PCC during precipitation.The example of fatty acid ester includes but is not limited to cellulose such as carboxymethyl cellulose, sorbitol, citrates such as sodium citrate or potassium citrate, stearates such as sodium stearate or potassium stearate, phosphates such as sodium phosphate or potassium phosphate, sodium tripolyphosphate, sodium hexametaphosphate, EDTA or its combination.In some embodiments, a combination of stearate and citrate can be added to form PCC during the precipitation step of the process.
[0297] In some embodiments, the gas leaving the precipitation reactor (shown as "scrubbed gas") enters a gas treatment unit for scrubbing. The mass balance and equipment design of the gas treatment unit may depend on the nature of the gas. In some embodiments, the gas treatment unit may incorporate an HCl scrubber for recovering HCl from the waste gas stream that may be removed from the CO 2 The small amount of NH carried by the absorption and precipitation steps 3 NH 3 Can be captured by HCl solution in the following ways:
[0298] NH 3 (g) + HCl (aqueous solution) → NH 4 Cl (aqueous solution).
[0299] NH from HCl scrubber 4 Cl(aq) can be recycled to dissolution step A.
[0300] In some embodiments, the waste gas stream containing ammonia (shown as "scrubbed gas" in the figure) can undergo a scrubbing process in which the waste gas stream containing ammonia is scrubbed with water and carbon dioxide from an industrial process to produce a solution of ammonia. The inlet to the scrubber can be carbon dioxide (CO 2 (g)), including ammonia (NH 3 (g)) of the reactor off-gas and fresh make-up water (or some other dilution water stream). The outlet may be the recirculation fluid of the scrubber (e.g. H 3 N-CO 2(水溶液) or carbamate) which can optionally be returned to the main reactor for contact with carbon dioxide and precipitation. The pH of the system can be adjusted by adjusting the CO 2(g) The flow rate entering the scrubber is controlled.
[0301] In some embodiments, the methods and systems provided herein further comprise separating the precipitation material from the aqueous solution by dehydration ( Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B Step D) in the step to form a reactive vaterite cake or a reactive vaterite cement in wet form or slurry form. The reactive vaterite cement cake may optionally undergo washing and optionally drying ( Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B Then, the dry reactive vaterite cement composition having the desired particle size and distribution can be optionally mixed with other components to form a blended composition of the reactive vaterite cement composition and sent to a method and system for forming a cement product (in Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B In some embodiments, the reactive vaterite cement cake may not be dried and may be sent as is to the method and system for forming a cement product (shown in Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B ).
[0302] The methods and systems provided herein can produce residual N-containing salts such as residual N-containing inorganic salts or N-containing organic salts, such as residual ammonium salts that remain in the supernatant solution and in the precipitate itself after the precipitate is formed. Residual bases as used herein, such as N-containing inorganic salts or N-containing organic salts, such as residual ammonium salts (e.g., residual NH 4 Cl), including any salt that can be formed by ammonium ions and anions present in the solution, the anions include but are not limited to halogen ions such as chloride ions, nitrate ions or nitrite ions, and sulfide ions such as sulfate ions, sulfite ions, thiosulfate ions, hydrosulfide ions and the like. In some embodiments, the residual N-containing inorganic salts include ammonium acetate, ammonium halides, ammonium sulfate, ammonium sulfite, ammonium hydrosulfide, ammonium thiosulfate, ammonium nitrate, ammonium nitrite or a combination thereof. These residual salts can be removed from the supernatant solution and the precipitate and optionally recovered. In some embodiments, the N-containing inorganic salts or N-containing organic salts such as residual ammonium salts (e.g., residual NH 4The supernatant solution of Cl) is recycled back to the dissolution reactor for dissolving lime or limestone (to Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B Step A).
[0303] The cake containing the reactive vaterite cement can be sent to a dryer ( Figure 2A , Figure 2B , Figure 3A , Figure 3B , Figure 4A and Figure 4B In step E) to form the multimodal distribution that comprises reactive vaterite cement or the dry powder composition of reactive vaterite cement with required particle size.The powder form of reactive vaterite cement is further used to form cement product, as described herein.Any drying technology as known in the art can be used to dry cake, and the drying technology is such as but not limited to fluidized bed dryer or eddy current fluidizer.Then the solid powder of gained can be mixed with other components such as aluminosilicate material, SCM (for example limestone), portland cement clinker, admixture, accelerator, additive or its mixture, to prepare dissimilar reactive vaterite cement compositions described herein.In some embodiments, the cake form of reactive vaterite cement composition or the slurry form with the water that reduces are directly used to form cement product, as described herein.
[0304] Depending on the specific drying scheme of the system, the drying station may include a filtration element, a freeze drying structure, a spray drying structure, etc. In some embodiments, the precipitate may be dried by a fluidized bed dryer. In certain embodiments, waste heat from a power plant or similar operation may be used to perform the drying step when appropriate.
[0305] The reactive vaterite cement in the cement product (optionally including solids from step B as described herein) undergoes curing and conversion to interlocking needle-shaped aragonite (optionally containing one or more voids forming a honeycomb structure) or calcite or carbonoaluminate (when combined with Portland cement or aluminosilicate materials), and solidifies and hardens into a cement product.
[0306] In the system provided herein, separation or dehydration step D can be carried out on a separation station.The cake or the precipitate comprising reactive vaterite cement can be stored in the supernatant for a period of time after precipitation and before separation.For example, the precipitate comprising reactive vaterite cement can be stored in the supernatant for a period of time of from a few minutes to a few hours to 1 day to 1000 days or longer, such as 1 day to 10 days or longer in the range of a temperature of 20 ℃ to 25 ℃ of scopes from 1 ℃ to 40 ℃.Separation or dehydration can be realized using any one of the methods in many convenient methods, and the method conveniently comprises draining (for example, the gravity settling of the precipitate comprising reactive vaterite cement, draining subsequently), decantation, filtering (for example, gravity filtration, vacuum filtration, use forced air filtration), centrifugal, pressing or its any combination.Body water is separated from the precipitate comprising reactive vaterite cement to produce the wet cake of the composition comprising reactive vaterite cement, or the composition comprising the dehydration of reactive vaterite cement. A liquid-solid separator such as Epuramat's Extrem-Separator ("ExSep") liquid-solid separator, Xerox PARC's spiral concentrator, or a modified version of Epuramat's ExSep or Xerox PARC's spiral concentrator can be used to separate compositions comprising reactive vaterite cement.
[0307] In some embodiments, reactive vaterite cement composition can be activated so that reactive vaterite cement causes interlocking needle-like aragonite approach rather than calcite approach during dissolution-reprecipitation process. In some embodiments, reactive vaterite cement composition is activated in such a way that after dissolution-reprecipitation process, interlocking needle-like aragonite formation is enhanced, and calcite formation is suppressed. The activation of reactive vaterite cement composition can cause control of interlocking needle-like aragonite formation and crystal growth. Various examples of activation of reactive vaterite cement composition are described herein, such as but not limited to nuclear activation, thermal activation, mechanical activation, chemical activation or its combination. In some embodiments, reactive vaterite is activated by multiple processes so that interlocking needle-like aragonite and its form and / or crystal growth optionally comprising a small amount of calcite can be controlled when reactive vaterite cement composition reacts with water. The interlocking needle-like aragonite with the calcite of optional formation causes the cement product formed by reactive vaterite to have higher tensile strength and fracture tolerance (fracture tolerance).
[0308] In some embodiments, reactive vaterite can be activated by mechanical means, as described herein.For example, reactive vaterite cement composition can be activated by producing surface defects on vaterite composition, so that the needle-like aragonite of interlocking is formed and is accelerated.In some embodiments, activated vaterite is the reactive vaterite of ball milling or the reactive vaterite with surface defects, so that the needle-like aragonite of interlocking is formed and is promoted.
[0309] Reactive vaterite cement composition can also be activated by providing chemical activation or nuclear activation to the vaterite composition. Such chemical activation or nuclear activation can be provided by one or more of aragonite seeds, inorganic additives or organic additives. The aragonite seeds present in the composition provided herein can be obtained from natural sources or synthetic sources. Natural sources include but are not limited to the hard skeleton materials of reef sand, lime, some freshwater and marine invertebrate organisms, including calcareous endoskeleton, pearl, rock, sediment, ore mineral (such as serpentine) and the like of axepods, gastropods, mollusk shells and warm water and cold water corals. Synthetic sources include but are not limited to precipitated aragonite, such as aragonite formed by sodium carbonate and calcium chloride; or the interlocking needle-shaped aragonite formed by reactive vaterite conversion to aragonite, such as the reactive vaterite of conversion described herein.
[0310] In some embodiments, the inorganic additive or organic additive in the composition provided herein can be any additive that reactive vaterite is activated. Some examples of inorganic additive or organic additive in the composition provided herein include but are not limited to sodium decyl sulfate, lauric acid, lauric acid sodium salt, urea, citric acid, citric acid sodium salt, phthalic acid, phthalic acid sodium salt, taurine, creatine, dextrose, poly (n-vinyl-1-pyrrolidone), aspartic acid, aspartic acid sodium salt, magnesium chloride, acetic acid, acetic acid sodium salt, glutamic acid, glutamic acid sodium salt, strontium chloride, gypsum, lithium chloride, sodium chloride, glycine, sodium citrate dihydrate, sodium bicarbonate, magnesium sulfate, magnesium acetate, sodium polystyrene, sodium dodecyl sulfonate, polyvinyl alcohol or its combination. In some embodiments, the inorganic additives or organic additives in the compositions provided herein include, but are not limited to, taurine, creatine, poly (n-vinyl-1-pyrrolidone), lauric acid, sodium salt of lauric acid, urea, magnesium chloride, acetic acid, sodium salt of acetic acid, strontium chloride, magnesium sulfate, magnesium acetate, or a combination thereof. In some embodiments, the inorganic additives or organic additives in the compositions provided herein include, but are not limited to, magnesium chloride, magnesium sulfate, magnesium acetate, or a combination thereof.
[0311] During reactive vaterite cement composition is optionally mixed with other components as mentioned herein and mixed with aqueous medium to form wet composition, reactive vaterite cement composition can experience high shear mixer (in mixer system). The component of reactive vaterite cement composition can use any suitable scheme blending. Every kind of material can mix when working, or part or all of material can be mixed in advance. As mixing device, any conventional equipment can be used. For example, Hobart mixer, pin mixer, tilted cylinder mixer, Omni mixer, Henschel mixer, V-type mixer and Nauta mixer can be adopted.
[0312] The methods and systems provided herein also include a control system configured to remotely and / or automatically control the calcination reactor, the dissolution reactor, and / or the treatment reactor.
[0313] Described method and system can also comprise one or more detectors, and described one or more detectors are configured to be used for monitoring the system of producing reactive vaterite cement composition and the system of producing cement product.Monitoring can include but not limited to collect the data about pressure, temperature, humidity and composition.Detector can be any convenient device, and it is configured to monitor such as pressure sensor (for example, electromagnetic pressure sensor, potential pressure sensor etc.), temperature sensor (resistance temperature detector, thermocouple, gas thermometer, thermistor, pyrometer, infrared radiation sensor etc.), volume sensor (for example, geophysical diffraction tomography, X-ray tomography, hydroacoustic measuring instrument etc.) and for determining the device (for example, IR spectrometer, NMR spectrometer, ultraviolet-visible spectrophotometer, high performance liquid chromatograph, inductively coupled plasma emission spectrometer, inductively coupled plasma mass spectrometer, ion chromatograph, X-ray diffractometer, gas chromatograph, gas chromatography-mass spectrometer, flow injection analysis, scintillation counter, acidity titration and flame emission spectrometer etc.) of the chemical composition of composition.
[0314] In some embodiments, the detector may further include a computer interface configured to provide the collected data about the composition to a user. In some embodiments, the summary may be stored as a computer readable data file, or may be printed as a user readable document.
[0315] In some embodiments, the detector can be a monitoring device so that it can collect real-time data (e.g., internal pressure, temperature, etc.). In other embodiments, the detector can be one or more detectors configured to determine parameters at regular intervals, such as every 1 minute, every 5 minutes, every 10 minutes, every 30 minutes, every 60 minutes, every 100 minutes, every 200 minutes, every 500 minutes, or some other interval.
[0316] The control station may include a set of valves or a multi-valve system that is manually controlled, mechanically controlled, or digitally controlled, or any other convenient flow regulator solution may be employed. In some cases, the control station may include a computer interface (wherein the regulation is computer-assisted or fully computer-controlled) that is configured to provide input parameters and output parameters to a user to control the production of cement products, as described above.
[0317] III. Cement products
[0318] In one aspect, provide cement product formed by the composition comprising bimodal, trimodal or multimodal reactive vaterite composition provided herein.In some embodiments, cement product comprises interlocking needle-like aragonite microstructure, calcite, carbonoaluminate or its combination.In some embodiments, interlocking needle-like aragonite is around one or more spaces.In some embodiments, the interlocking needle-like aragonite around one or more spaces forms honeycomb structure.In some embodiments, cement product is the lightweight cement product with low bulk density or low bulk density.
[0319] As used herein, "cement product" includes any cement product formed from the reactive vaterite cement compositions provided herein.
[0320] In some embodiments, the cement product formed by the composition provided herein is a building material. "Building material" used herein includes the material used in construction. The example of such structure or building material includes but is not limited to the footing, fence, pole or its module of buildings, driveways, foundations, kitchen boards, furniture, pavements, roads, bridges, highways, flyovers, parking structures, bricks, blocks, walls, gates.
[0321] In some embodiments, the cement product formed from the compositions provided herein is an aggregate, such as, for example, a lightweight aggregate.
[0322] In some embodiments, the cement product comprising interlocking needle-like aragonite provided herein has up to about 99.9% aragonite or up to 99% aragonite or up to 97% aragonite or up to 95% aragonite or up to 90% aragonite or up to 80% aragonite or about 80%-99.9% between aragonite or about 80%-99% between aragonite or about 80%-95% between aragonite.In some embodiments, the residual amount in the cement product is vaterite and / or calcite.The % of aragonite can be wt%.
[0323] In some embodiments, the cement product comprising the interlocking needle-like aragonite provided herein has a porosity between about 10%-90%. The % of porosity can be volume %. In some embodiments, depending on the mean particle size and the particle distribution of the composition comprising reactive vaterite cement, the porosity of cement product can be controlled between 10%-90%. Porosity can be of benefit to the preparation of lightweight cement products, which can be used for building applications, heat insulation, filtration applications and similar applications. In some embodiments, the highly porous cement product comprising the interlocking needle-like aragonite may be required, in other embodiments, the cement product of medium porosity may be required, and in other cases, the cement product of low porosity or no porosity may be required. Above-mentioned porous cement product can be a lightweight cement product. The porosity of the cement product can be measured, for example, by the water absorption after oven drying followed by complete saturation of the cement product by water impregnation, expressed as % dry weight (measured relative to dry weight), and can be in the range of about 10%-90%; or between about 10%-80%; or between about 10%-70%; or between about 10%-60%; or between about 10%-50%; or between about 10%-40%; or between about 10%-30%; or between about 10%-20%; or between about 20%-90%; or between about 20%-80%; or between about 20%-70%; or between about 20%-60%; or between about 20%-50%; or between about 20%-40%; or between about 20%-30%; or between about 3 or about 50%-90%; or about 50%-80%; or about 50%-70%; or about 50%-60%; or about 60%-80%; or about 70%-80%; or about 1%-40%; such as 2%-20% or 2%-15%, including 2%-10% or even 3%-9%.
[0324] In some embodiments, the aggregate comprising interlocking needle-shaped aragonite provided herein can provide mortar as fine aggregate and / or concrete as coarse aggregate. Fine aggregate can be a material that passes almost completely through a No. 4 sieve (ASTM C 125 and ASTM C33), and coarse aggregate can be a material that is mainly retained on a No. 4 sieve (ASTM C 125 and ASTM C 33).
[0325] In some embodiments, the bulk density (unit weight) of the cement product is from 25 to 200 lb / ft 3 (pounds / cubic foot), or from 25-110lb / ft 3 , or from 25-75lb / ft 3 , or from 25-50lb / ft 3 , or from 50-200lb / ft 3 , or from 50-100lb / ft 3 , or from 50-75lb / ft 3 , or from 75-175lb / ft 3 , or from 25-55lb / ft 3 , or from 75-125lb / ft 3 , or from 90-115lb / ft 3 , or from 100-200lb / ft 3 , or from 125-175lb / ft 3 , or from 140-160lb / ft 3 Some embodiments include lightweight cement products, such as those having 25 lb / ft 3 Up to 75 lb / ft 3 Aggregates with a packing density (unit weight) of 25 lb / ft. 3 Up to 55 lb / ft 3 The bulk density (unit weight) of aggregate.
[0326] In some embodiments of the foregoing aspects and the foregoing embodiments, the cement products provided herein comprising interlocking needle-shaped aragonite have a Cementitiousness of between about 250-5000 psi; or between about 250-4000 psi; or between about 250-3000 psi; or between about 250-2000 psi; or between about 250-1000 psi; or between about 250-500 psi; or between about 500-5000 psi; or between about 500-4000 psi; or between about 500-3000 psi; or between about 500-2000 psi. In some embodiments, the compressive strength described herein is the compressive strength after 1 day, or 3 days, or 7 days, or 28 days, or 56 days or more. In some embodiments, the cement product after solidification and hardening has a 28-day compressive strength of at least 250psi. In some embodiments, the cement product after curing and hardening has a 28-day compressive strength of at least 21 MPa (megapascals) or at least 3046 psi.
[0327] In some embodiments, aggregate, such as, for example, lightweight aggregate provided herein, is used to manufacture the various types of materials used in construction. For example only, lightweight aggregate provided herein is the form of coarse aggregate or fine aggregate, which has a lower bulk density (forming more voids or porosity of honeycomb microstructure) and is used to produce lightweight concrete. Common cement applications of lightweight aggregate include but are not limited to floor slabs in high-rise buildings, concrete masonry units or any application of concrete or products that need to reduce weight. Lightweight aggregate can also be used to increase the R value or insulating properties of concrete or other materials by trapping air inside its structure. In some embodiments, the internal curing of concrete is another purpose of lightweight aggregate, wherein lightweight aggregate can be pre-saturated with water before mixing concrete. Water can then be slowly released into the cement paste around, providing water for cement paste to react chemically and obtain strength. In some embodiments, lightweight aggregate is used as soil additive in agricultural applications to improve aeration and water retention or as soilless growth medium, such as in some hydroponic settings.
[0328] In some embodiments, the following ASTM standards may be applicable to the lightweight aggregate provided herein: ASTM C330M-17a Standard Specification for Lightweight Aggregates for Structural Concrete; ASTM C331M-17 Standard Specification for Lightweight Aggregates for Concrete Masonry Units; ASTM C332-17 Standard Specification for Lightweight Aggregates for Insulating Concrete; ASTM C495M-19 Standard Test Method for Compressive Strength of Lightweight Insulating Concrete; ASTM C513M-19 Obtaining and Testing the Compressive Strength of Test Specimens of Hardened Lightweight Insulating Concrete; ASTM C567M-19 Standard Test Method for Determining the Density of Structural Lightweight Concrete; ASTM C641-17 Standard Test Method for Iron-Stained Materials in Lightweight Concrete Aggregates; ASTM C1761M-17 Standard Specification for Lightweight Aggregates for Internal Curing of Concrete.
[0329] In some embodiments, lightweight aggregates used to form concrete help reduce the density of the concrete without compromising the compressive strength of the concrete.
[0330] In some embodiments, the cementitious products formed from the compositions provided herein are formed building materials.As used herein, "formed building materials" include materials that are formed into structures having a defined physical shape.
[0331] Examples of formed building materials that can be produced by the foregoing methods and systems include, but are not limited to, masonry units, such as, by way of example only, bricks, blocks, and tiles, including, but not limited to, ceiling tiles; building panels, such as, by way of example only, cement board and / or drywall; ducts; basins; beams; columns, panels; sound barriers; insulation materials; or combinations thereof. A building panel is a formed building material used in a broad sense to refer to any non-load-bearing structural element that is characterized such that its length and width are substantially greater than its thickness. Thus, a panel can be a plank, board, shingles, and / or tile.
[0332] In some embodiments, cement board and / or drywall can be used to make different types of boards, such as but not limited to paper veneer, fiberglass veneer or fiberglass mat veneer (e.g., surface reinforcement with fiberglass mat), fiberglass mesh reinforced board (e.g., surface reinforcement with glass mesh) and / or fiber reinforced board (e.g., cement reinforcement with cellulose, glass, fiber, etc.). These boards can be used for a variety of applications, including but not limited to, wallboard, such as fiber cement wallboard, roof, arch soffits, sheathing, cladding, cover board, ceiling, shaft liner, wallboard, liner, trim, lintel, shingle and panel, and / or pad. Cement board is a shaped building material, which in some embodiments is used as a backing board for ceramics, which can be used behind bathroom tiles, kitchen counters, backsplashes, etc., and can have a length ranging from 100 cm to 200 cm. Cement board may differ in physical and mechanical properties. In some embodiments, the bending strength can vary, ranging between 1 MPa and 7.5 MPa, including 2 MPa to 6 MPa, such as 5 MPa. The compressive strength may also vary, ranging from 5 MPa to 50 MPa, including 10 MPa to 30 MPa, such as 15 MPa to 20 MPa. In some embodiments, the cement board may be used in environments with substantial exposure to moisture (eg, a commercial sauna).
[0333] Another type of building panel is backer board. Backer board can be used to construct interior and / or exterior floors, walls and ceilings. Another type of building panel is drywall. Drywall includes boards used to construct interior and / or exterior floors, walls and ceilings. One application of cement board or drywall is fiber cement siding.
[0334] In some embodiments, the formed building material is a masonry unit. Masonry units are formed building materials used to construct load-bearing and non-load-bearing structures, which are typically assembled using mortar, grout, and the like. Exemplary masonry units include bricks, blocks, and tiles.
[0335] Another type of formed building material is a conduit. A conduit is a tube or similar structure configured to transport a gas or liquid from one location to another. A conduit may include any number of different structures for transporting liquids or gases, including but not limited to pipes, culverts, box culverts, drainage channels and portals, inlet structures, intake towers, gate wells, outlet structures, and the like.
[0336] Another formed building material is a basin. The term basin may include any configuration of container for holding a liquid such as water. Thus, a basin may include, but is not limited to, structures such as a well, a collection box, a sanitary manhole, a septic tank, a catch basin, a grease trap / separator, a stormwater drainage collection reservoir, and the like.
[0337] Another type of formed building material is a beam, which in a broad sense refers to a horizontal load-bearing structure with great bending and compressive strength. Beams can be rectangular cross-shaped, C-shaped channels, L-shaped edge beams, I-beams, spandrel beams, H-shaped beams, inverted T-shaped designs, etc. Beams can also be horizontal load-bearing units, including but not limited to joists, lintels, arches, and cantilevers.
[0338] Another type of building material is a column, which in a broad sense refers to a vertical load-bearing structure that carries loads primarily through axial compression and includes structural elements such as compression members. Other vertical compression members may include, but are not limited to, pillars, piers, bases, or columns.
[0339] Another type of formed building material is concrete slab. Concrete slabs are those building materials used to construct precast foundations, floors, and wall panels. In some cases, concrete slabs can be used as floor units (e.g., hollow core slab units or double tee designs).
[0340] Another type of building material is a sound barrier, which refers to a structure used as a barrier for the attenuation or absorption of sound. Thus, a sound barrier may include, but is not limited to, structures such as sound absorbing panels, reflective barriers, absorptive barriers, reactive barriers, and the like.
[0341] Another type of building material is insulation, which refers to materials used to attenuate or inhibit the conduction of heat. Insulation can also include materials that reduce or inhibit the radiative transfer of heat.
[0342] In some embodiments, other formed building materials such as precast concrete products include, but are not limited to, bunker silos; cattle feed bunks; cattle grids; agricultural fences; H-bunks; J-bunks; livestock slats; livestock water troughs; building panel walls; cladding (bricks); building trim; foundations; floors, including slabs on the ground; walls; double-wall precast sandwich panels; aqueducts; mechanically stable ground panels; box culverts; three-sided culverts; bridge systems; RR intersections; RR ties; noise walls / barriers; Jersey barriers; tunnel sections; reinforced concrete boxes; utility protection structures; handholes; hollow core products; light pole bases; meter boxes; panel vaults; pull boxes; telecommunication structures; transformer pads; transformer rooms; trenches; utility vaults ... vault; utility pole; controlled environment vault; underground vault; mausoleum; tombstone; coffin; hazardous mat storage container; detention facility; catch basin; manhole; aeration system; distribution box; dosing tank; dry well; grease interceptor; leach pit; sand-oil / oil-water interceptor; septic tank; water / wastewater storage tank; wet well; fire water storage tank; floating dock; underwater infrastructure; deck; railing; seawall; roof tile; pavers; community retaining wall; reservoir retaining wall; modular closure system; and segmented retaining wall.
[0343] In some embodiments, the methods and systems described herein include making artificial marine structures by the compositions provided herein, and the artificial marine structures include but are not limited to artificial corals and artificial reefs. In some embodiments, the artificial structures can be used in aquariums or oceans. In some embodiments, aragonite cement provides a neutral or near-neutral pH, which may be conducive to the maintenance and growth of marine organisms. Aragonite reefs can provide suitable habitats for marine species.
[0344] Throughout the description, where compositions are described as having, including, or comprising specific components, or where processes and methods are described as having, including, or comprising specific steps, it is contemplated that there are additional compositions of the invention consisting essentially of, or consisting of, the stated components, and that there are processes and methods in accordance with the invention consisting essentially of, or consisting of, the stated process steps.
[0345] In this application, when an element or component is referred to as being included in and / or selected from a stated list of elements or components, it should be understood that the element or component may be any one of the stated elements or components, or the element or component may be selected from a group consisting of two or more of the stated elements or components.
[0346] In addition, it should be understood that the elements and / or features of the compositions or processes described herein can be combined in various ways without departing from the spirit and scope of the present invention, whether explicitly or implicitly in this article. For example, with reference to a particular composition, the composition can be used in various embodiments of the compositions of the present invention and / or the processes of the present invention, unless otherwise understood from the context. In other words, in the present application, embodiments have been described and depicted in a manner that can write and draw clear and concise applications, but it is expected and will be understood that embodiments can be combined or separated differently without departing from this teaching and invention. For example, it should be understood that all features described and depicted herein can be applied to all aspects of the present invention described and depicted herein.
[0347] Where a range of values is provided, it is understood that each intermediate value between the upper and lower limits of the range, to one-tenth of the unit of the lower limit (unless the context clearly indicates otherwise), and any other stated values or intermediate values in the stated range, are encompassed within the present invention. The upper and lower limits of these smaller ranges may be independently included in the smaller ranges, and are also encompassed within the present invention, subject to any specific excluded limits in the stated ranges. Where the stated range includes one or both of the limits, ranges excluding either or both of those included limits are also encompassed within the present invention.
[0348] The use of the terms "include," "includes," "including," "have," "has," "having," "contain," "contains," or "containing," including their grammatical equivalents, should generally be understood to be open-ended and non-limiting, e.g., not excluding additional, unrecited elements or steps, unless specifically stated or understood otherwise from the context.
[0349] Unless otherwise claimed, the use of any and all examples or exemplary language herein, such as "such as" or "including" is intended only to better illustrate the invention and does not limit the scope of the invention. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.
[0350] Certain ranges are presented herein where the value is preceded by the term "about". The term "about" is used herein to provide literal support for the exact number preceding it, as well as numbers that are close to or approximately the number preceding the term. As used herein, the term "about" refers to a ±10% difference from the nominal value, unless otherwise specified or inferred.
[0351] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although any processes and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention, representative illustrative processes and materials are described herein.
[0352] All publications, patents and patent applications mentioned in this specification are incorporated herein by reference, just as each individual publication, patent or patent application is specifically and individually indicated to be incorporated by reference. In addition, each cited publication, patent or patent application is incorporated herein by reference to disclose and describe the subject matter related to the publication being cited. Reference to any publication is for its disclosure before the filing date, and should not be construed as admitting that the invention described herein is not entitled to precede such publication due to previous inventions. In addition, the date of the publication provided may be different from the actual publication date that may need to be confirmed separately.
[0353] It should be understood that the expression "at least one of" includes each recited object following the expression individually and multiple combinations of two or more of the recited objects, unless otherwise understood from the context and usage. The expression "and / or" related to three or more recited objects should be understood to have the same meaning, unless otherwise understood from the context.
[0354] It should be noted that, as used herein and in the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. For example, when the plural form is used for compounds, salts, and the like, this also means a single compound, salt, or the like. It should also be noted that the claims can be drafted to exclude any optional elements.
[0355] When reading this disclosure, as will be apparent to those skilled in the art, each embodiment in the separate embodiments described and illustrated herein has discrete parts and features that can be easily separated or combined with the features of any other several embodiments without departing from the scope or spirit of the present invention. Any stated process can be performed in the order of stated events, or in any other order that is logically possible. It should be understood that the order of steps or the order for performing certain actions is unimportant as long as the application remains operable. In addition, two or more steps or actions can be performed simultaneously.
[0356] The following examples are put forward to provide those of ordinary skill in the art with a complete disclosure and description of how to make and use the invention, and are not intended to limit the scope of what the inventors regard as their invention, nor are they intended to represent that the experiments below are all or the only experiments performed. Efforts have been made to ensure accuracy with respect to numbers used (e.g., amounts, temperatures, etc.), but some experimental errors and deviations should be accounted for. Example
[0357] Example 1
[0358] Effect of smaller particle size of reactive vaterite cement on the morphology of cement products
[0359] 100 grams of reactive vaterite cement with a median size of 7.2 μm was combined with 24.8g of 0.4M magnesium nitrate solution. After standing for 30 seconds, the material was mixed at a low speed in a 5-quart Hobart mixer for 30 seconds. After mixing at a medium speed for 30 seconds, the blended wet powder was transferred to a disc granulator. Additional solution was sprayed on the powder tumbling in the disc granulator until it began to agglomerate. The disc granulator was then allowed to run for a sufficient time to obtain the desired size of aggregate. At this point, the aggregate was sprinkled with additional reactive vaterite cement until the surface of the aggregate looked dim or dry. The final water-to-cement ratio of the aggregate was 0.68. The aggregate was then placed in a sealed container and cured at 80°C and 98% relative humidity for 1 day. The aggregate was then dried at 110°C until constant mass. Aggregate was then observed via a scanning electron microscope (SEM), which revealed an interlocking needle-like aragonite microstructure. The phase composition of the lightweight aggregate was then determined via quantitative x-ray diffraction to be 0.1% vaterite, 92.6% aragonite, and 7.3% calcite. Figure 5 An interlocking needle-like aragonite microstructure formed by reactive vaterite cement is shown with a median size of 7.2 μm. The image on the left is at 250x magnification and the image on the right is at 1000x magnification. The aggregate was found to contain fewer voids or less honeycomb structure due to the relatively uniform distribution of needle-like aragonite due to the smaller size particles of the reactive vaterite cement.
[0360] Example 2
[0361] Effect of larger particle size of reactive vaterite cement on the morphology and bulk density of cement products
[0362] 10 kg of reactive vaterite cement with a median size of 16.1 μm was combined with 2,500 g of 0.1 M magnesium nitrate and 0.05 M strontium nitrate solution in a 500 g batch of cement. The material was mixed at low speed for 30 seconds in a 5 quart Hobart mixer, followed by medium speed mixing for 60 seconds. The blended wet powder was then transferred to a disc granulator. Additional solution was sprayed onto the powder tumbling in the disc granulator until it began to agglomerate. The disc granulator was then allowed to run for a sufficient time to obtain the desired size of the aggregate. At this point, the aggregate was sprinkled with additional reactive vaterite cement until the surface of the aggregate looked dull or dry. The final water-to-cement ratio of the aggregate was 0.25. The aggregate was then placed in a sealed container and cured at 80 ° C and 98% relative humidity for 3 days. The aggregate was then dried at 110 ° C until the mass was constant. The aggregate was then observed via SEM, which revealed an interlocking needle-like aragonite microstructure. The phase composition of the lightweight aggregate was then determined via quantitative x-ray diffraction to be 3.9% vaterite, 95.2% aragonite and 0.9% calcite. Sieve analysis showed that 99.3%, 36.3% and 0.3% of the lightweight aggregate passed through a 19 mm sieve, a 9.5 mm sieve and a 4.75 mm sieve, respectively. The lightweight aggregate produced met the grading requirements for lightweight aggregates from 19.0 to 4.75 mm for structural concrete according to ASTM C330. The dry loose bulk density was 54.6 lbft 3 , which is lower than the 55 lb / ft of lightweight coarse aggregate specified by ASTM C330 3 Maximum dry loose bulk density.
[0363] Figure 6 An interlocking needle-like aragonite microstructure is shown with voids surrounded by needles formed by reactive vaterite cement with a median size of 16.1 μm (forming a honeycomb structure). The image on the left is the core of the aggregate at 2500 times magnification and the image on the right is the surface of the aggregate at 2500 times magnification.
[0364] Example 3
[0365] Effect of bimodal distribution on fluidity and strength of cement blends
[0366] Mix and pour binary cement mortar according to ASTM C305 and C109. The ratio of sand to cement is 2.75, and the ratio of water to cementitious material is 0.485. The portland cement used meets ASTM C150 as II / V type cement. 20% of cementitious material is replaced by reactive vaterite cement. Five binary cement blends tested are presented in Table 1. Before mixing, all cementitious materials are premixed to uniformity. The mixing procedure is to combine cement blend and water in 5 quarts of Hobart vertical mixers, and mix at low speed for 30 seconds. Then introduce sand in 30 seconds, while continuing to mix at low speed. Then increase speed to medium speed for 30 seconds. Then stop the mixer for 90 seconds and scrape down for 15 seconds to loosen any material stuck on the mixing bowl and paddle. After scraping down, cover the mixer bowl until continuing to mix at medium speed for another 1 minute. The mortar was then immediately tested for fluidity according to ASTM C1437 and then remixed at medium speed for 15 seconds before pouring 2" mortar cubes. The mortar cubes were then stored at 23°C and 98% relative humidity. After curing for 24 hours, the mortar was demoulded and moved to a saturated lime bath until tested for compressive strength according to ASTM C109 at 3 days, 7 days, 28 days, and 56 days. Three mortar cubes were tested at each age.
[0367] Table 1: Binary mortar mixtures containing unimodal and bimodal particle distributions
[0368]
[0369] like Figure 7 As shown in Figure 2, in binary cement blends containing up to 20% reactive vaterite cement, the fluidity of the resulting mortar increases with increasing amount of larger reactive vaterite particles of size 16 μm. Figure 8 As can be seen, the strength did not decrease in the same consistent manner as flow increased, but rather the bimodal distribution of 5 μm and 16 μm (or um) reactive vaterite particles produced the same 28 day strength as the mortar using only 5 μm reactive vaterite particles as the vaterite cement component.
[0370] Example 4
[0371] Effect of multimodal distribution on paste viscosity and fluidity
[0372] In this experiment, the surface area and particle diameter of reactive vaterite cement are changed to test the viscosity of reactive vaterite cement and portland cement mixture.Viscosity value is produced by mixing the reactive vaterite cement of multiple particle diameters with 85% portland cement with the mass ratio of 0.485 water and cement.Use the MCR 92 of Anton Par to measure viscosity with the shear rate of 250rpm (revolutions per minute) on the downward flow curve, in mPa*s (millipascal-second).The particle diameter used for model is according to the median particle diameter measured by LA-960Horiba laser scattering particle size distribution analyzer.Measure surface area by the Gemini V BET of Micromeritics.Porosity is measured by the AccuPyc II 1340 pycnometer of Micromeritics.100% portland cement has the viscosity of about 1,600mPa*s.
[0373] As shown in Table 2, the reactive vaterite cement (Vat.) of different particle sizes is blended with portland cement (PC).The bimodal distribution of reactive vaterite cement and portland cement is shown as the blended compositions B1-B6 in Table 2.Cement paste is prepared by mixing cement blend with half water at 600rpm for 60 seconds, then adding remaining water, and cement paste is mixed at 1200rpm for other 90 seconds.Then the paste of preparation is transferred to rheometer (MCR 92 of Anton Par).Measure reactive vaterite surface area in water, and measure portland cement surface area in isopropyl alcohol.
[0374] Table 2: Reactive vaterite cement and Portland cement mixtures
[0375]
[0376] The particle size distribution of Portland cement; unimodal reactive vaterite is mixed with PC to produce a blended cement mixture; and the bimodal blend (B1) is Fig. 9 Displayed in.
[0377] Fig.10 Paste viscosity as a function of the surface area of the blended cement is shown. Unimodal reactive vaterite cement blends with PC (4 μm Vat., 7 μm Vat., 9 μm Vat., 15 μm Vat., 17 μm Vat. and 26 μm Vat.) Fig.10Marked with squares and dashed lines in the figure. For a unimodal distribution of reactive vaterite cement particles, the paste viscosity increases with increasing surface area (or decreasing particle size). However, it was found that when reactive vaterite particles were combined in a bimodal distribution (e.g., reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm and reactive vaterite cement B having an average particle size between about 11 μm-50 μm) to produce blends (B1, B2, B3, B4, B5 and B6) (in Fig.10 When using unimodal reactive vaterite to produce paste, it will be shown that the blend has a lower paste viscosity compared to their surface area. For example, bimodal blend B6 has a blended cement paste viscosity of 951mPa*s, but if the paste is produced by unimodal vaterite, the paste viscosity will be 1500mPa*s. Lower paste viscosity is relevant with higher fluidity in mortar and higher slump in concrete.
[0378] In addition, it is also found that the larger the surface area of reactive vaterite cement particles present in the blended cement, the larger the surface area that can be used to nucleate the calcium silicate hydrate (CSH) of PC. The more calcium silicate hydrate nucleated, the faster the PC dissolves and produces strength in the blended cement composite. The bimodal or multimodal distribution of reactive vaterite cement particles accelerates the hydration of PC, making it possible to produce a blended cement composite with a workability or paste viscosity or fluidity similar to its portland cement control (100% portland cement), while providing additional surface area for CSH formation and strength enhancement compared to the blended cement produced with unimodal reactive vaterite cement particles.
[0379] Although the foregoing invention has been described in some detail by way of illustration and example for the purpose of clear understanding, it should be obvious to those of ordinary skill in the art, according to the teachings of the present invention, that certain changes and modifications may be made to it without departing from the spirit or scope of the appended claims. Therefore, the foregoing only illustrates the principles of the present invention. It should be understood that those skilled in the art will be able to design a variety of arrangements, which, although not explicitly described or shown herein, embody the principles of the present invention and are included in its spirit and scope. In addition, all examples and conditional language listed herein are primarily intended to help readers understand the principles of the present invention and the concepts contributed by the inventors to advance the art, and should be interpreted as not being limited to such specific examples and conditions. In addition, all statements of the principles, aspects and embodiments of the present invention and their specific examples are listed herein to cover both their structural and functional equivalents. In addition, it is intended that such equivalents include both currently known equivalents and equivalents developed in the future, that is, any element developed to perform the same function, regardless of its structure. Therefore, the scope of the present invention is not intended to be limited to the exemplary embodiments shown and described herein. It is intended that the appended claims define the scope of the present invention, and thus cover methods and structures and their equivalents within the scope of these claims.
Claims
1. A cement composition comprising: a bimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
2. A cement composition comprising: a trimodal distribution of reactive vaterite cements, comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; and reactive vaterite cement C having an average particle size between about 51 μm and 100 μm.
3. The cement composition of claim 1 or 2, wherein the reactive vaterite cement A is between about 5%-95% by weight in the composition, and the reactive vaterite cement B is between about 5%-95% by weight in the composition.
4. The cement composition of claim 1 or 2, wherein the reactive vaterite cement A is between about 5%-75% by weight in the composition, and the reactive vaterite cement B is between about 25%-95% by weight in the composition.
5. The cement composition of claim 2, wherein the reactive vaterite cement A is between about 5%-40% by weight; the reactive vaterite cement B is between about 25%-50% by weight; and the reactive vaterite cement C is between about 5%-10% by weight.
6. The cement composition of any one of the preceding claims, wherein the composition increases the packing density of cement paste in water by between about 1% and 35%.
7. The cement composition of any one of the preceding claims, wherein the composition reduces the viscosity of cement paste in water by between about 10%-50%.
8. The cement composition according to any one of the preceding claims, wherein the composition provides a paste viscosity in water of between about 800 mPa*s - 1600 mPa*s.
9. The cement composition according to any one of the preceding claims, wherein the ratio of reactive vaterite cement A: reactive vaterite cement B is between about 1:20-20:
1.
10. The cement composition according to any one of the preceding claims, wherein the reactive vaterite cement A has a 2 / kg-40,000m 2 / kg, and the reactive vaterite cement B has a specific surface area of about 100m 2 / kg-6,000m 2 / kg between specific surface area.
11. The cement composition according to any one of the preceding claims, wherein the reactive vaterite cement A and the reactive vaterite cement B have a spherical morphology.
12. The cementitious composition of any one of the preceding claims, further comprising Portland cement to form a blended cementitious composition.
13. The cement composition of claim 12, wherein the cement composition has a 2 / kg-40,000m 2 The reactive vaterite cement A with a specific surface area between 200 Å and 100 Å / kg provides a high surface area to nucleate calcium silicate hydrate and dissolve Portland cement in water.
14. The cement composition according to claim 12 or 13, wherein the bimodal distribution and / or trimodal distribution in the blended cement composition provides a paste viscosity in water between about 800 mPa*s-1600 mPa*s.
15. The cement composition according to any one of the preceding claims, wherein the reactive vaterite cement A and / or the reactive vaterite cement B further comprises magnesium oxide.
16. The cementitious composition according to any one of the preceding claims, wherein the cementitious composition further comprises an aluminosilicate material.
17. The cement composition of claim 16, wherein the aluminosilicate material comprises thermally treated clay, natural or artificial pozzolan, shale, granulated blast furnace slag, or a combination thereof.
18. The cement composition of claim 17, wherein the heat-treated clay comprises calcined clay, aluminosilicate glass, calcium aluminosilicate glass, or a combination thereof.
19. The cement composition of claim 17, wherein the pozzolan is selected from the group consisting of fly ash, pozzolan, and mixtures thereof.
20. The cementitious composition according to any one of the preceding claims, wherein the cementitious composition further comprises slag from metal production, Portland cement clinker, calcium aluminate cement clinker and / or calcium sulphoaluminate cement clinker.
21. The cementitious composition of any one of the preceding claims, wherein the cementitious composition further comprises a carbonate material comprising limestone, calcium carbonate, magnesium carbonate, calcium magnesium carbonate, or a combination thereof.
22. The cementitious composition according to any one of the preceding claims, wherein the cementitious composition further comprises an alkali metal accelerator or an alkaline earth metal accelerator.
23. The cement composition according to claim 22, wherein the alkali metal accelerator or the alkaline earth metal accelerator is selected from the group consisting of sodium sulfate, sodium carbonate, sodium nitrate, sodium nitrite, sodium hydroxide, potassium sulfate, potassium carbonate, potassium nitrate, potassium nitrite, potassium hydroxide, lithium sulfate, lithium carbonate, lithium nitrate, lithium nitrite, lithium hydroxide, calcium sulfate, calcium nitrate, calcium nitrite and combinations thereof.
24. A cementitious composition according to any of the preceding claims, comprising by weight between about 5%-50% of a composition comprising reactive vaterite cement, between about 5%-40% heat-treated clay, between about 0-10% limestone and between about 15%-90% Portland cement clinker.
25. The cement composition of any one of the preceding claims, wherein the composition after curing and hardening has a 28 day compressive strength of at least 21 MPa.
26. The cementitious composition according to any one of the preceding claims, wherein the cementitious composition further comprises an admixture selected from the group consisting of setting accelerators, setting retarders, air entraining agents, foaming agents, defoamers, alkali reactivity reducers, bonding admixtures, dispersants, coloring admixtures, corrosion inhibitors, moisture-proofing admixtures, gas forming agents, permeability reducers, pumping aids, shrinkage compensating admixtures, fungicidal admixtures, bactericidal admixtures, insecticidal admixtures, rheology modifiers, finely divided mineral admixtures, pozzolans, aggregates, wetting agents, strength enhancers, waterproofing agents, reinforcing materials, and combinations thereof.
27. The cementitious composition of claim 26, wherein the reinforcing material is a fiber selected from the group consisting of zirconia-containing materials, aluminum, glass, steel, carbon, ceramic, grass, bamboo, wood, fiberglass, synthetic materials, and combinations thereof.
28. A concrete mixture comprising the cement composition according to any one of the preceding claims 1-27.
29. A cement paste or cement slurry composition comprising: reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; reactive vaterite cement B having an average particle size between about 11 μm-50 μm; and optionally reactive vaterite cement C having an average particle size between about 51 μm-100 μm; water; and interlocking needle-shaped aragonite.
30. The cement paste or cement slurry composition of claim 29, further comprising Portland cement.
31. The cement paste or slurry composition of claim 30, wherein the cement paste or slurry composition has a 2 / kg-40,000m 2 The reactive vaterite cement A with a specific surface area between 200 Å and 100 Å / kg provides a high surface area to nucleate calcium silicate hydrate and dissolve Portland cement in water.
32. A cement paste or cement slurry composition according to any one of claims 29-31, wherein the reactive vaterite cement A and reactive vaterite cement B or reactive vaterite cement A, reactive vaterite cement B and reactive vaterite cement C provide a paste viscosity between about 800 mPa*s-1600 mPa*s.
33. A method for producing a cement composition comprising: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the mixture comprising lime in an N-containing salt solution to produce an aqueous solution comprising a calcium salt; and (c) treating the aqueous solution comprising a calcium salt with the gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
34. A method for producing a cement composition comprising: (a) calcining limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (b) dissolving the lime-containing mixture in an N-containing salt solution to produce an aqueous solution containing a calcium salt; (c) treating the aqueous solution containing a calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; and treating the aqueous solution containing a calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; (d) mixing the composition containing reactive vaterite cement A and the composition containing reactive vaterite cement B to form a composition containing a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement contains reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
35. A method for producing a cement composition comprising: (a) dissolving limestone in a nitrogen-containing salt solution to produce an aqueous solution comprising calcium salts and a gas stream comprising carbon dioxide; and (b) treating the aqueous solution comprising a calcium salt with the gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
36. A method for producing a cement composition comprising: (a) dissolving limestone in a nitrogen-containing salt solution to produce an aqueous solution comprising calcium salts and a gas stream comprising carbon dioxide; (b) treating the aqueous solution containing calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm; and treating the aqueous solution containing calcium salt with the gas stream containing carbon dioxide to form a composition containing reactive vaterite cement B having an average particle size between about 11 μm-50 μm; (c) mixing the composition containing reactive vaterite cement A and the composition containing reactive vaterite cement B to form a composition containing a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement contains reactive vaterite cement A having an average particle size between about 0.1 μm-10 μm and reactive vaterite cement B having an average particle size between about 11 μm-50 μm.
37. The method of any one of claims 33-36, further comprising adding water to the cement composition and converting the reactive vaterite cement A and the reactive vaterite cement B into interlocking needle-like aragonite upon dissolution and reprecipitation in water.
38. The method of claim 37, wherein the reactive vaterite cement A and / or reactive vaterite cement B improves the packing density of the cement paste by between about 1%-35% and / or reduces the viscosity of the cement paste by 10% or more.
39. The method of any one of claims 37-38, further comprising allowing the interlocking acicular aragonite to set and harden and form a cement product.
40. The method of claim 39, wherein the cement product has a relative humidity of about 25 lb / ft 3 -200lb / ft 3 The packing density between.
41. A system for forming a composition, comprising: (i) a calcining reactor configured to calcine limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (ii) a dissolution reactor operably connected to the calcination reactor, the dissolution reactor being configured to dissolve the mixture comprising lime in an aqueous N-containing brine solution to produce an aqueous solution comprising calcium salt; (iii) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured to treat the aqueous solution comprising the calcium salt with the gas stream comprising carbon dioxide to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
42. A system for forming a composition, comprising: (i) a calcining reactor configured to calcine limestone to form a mixture comprising lime and a gas stream comprising carbon dioxide; (ii) a dissolution reactor operably connected to the calcination reactor, the dissolution reactor being configured to dissolve the mixture comprising lime in an aqueous N-containing brine solution to produce an aqueous solution comprising calcium salt; (iii) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured to treat the aqueous solution comprising a calcium salt with the gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm; (iv) a treatment reactor operably connected to the dissolution reactor, the treatment reactor being configured for treating the aqueous solution comprising a calcium salt with the gas stream comprising carbon dioxide to form a composition comprising reactive vaterite cement B having an average particle size between about 11 μm and 50 μm; as well as (v) a mixing reactor operably connected to the treatment reactor, wherein the mixing reactor is configured to mix the composition comprising reactive vaterite cement A and the composition comprising reactive vaterite cement B to form a composition comprising a bimodal distribution of reactive vaterite cement, wherein the bimodal distribution of reactive vaterite cement comprises reactive vaterite cement A having an average particle size between about 0.1 μm and 10 μm and reactive vaterite cement B having an average particle size between about 11 μm and 50 μm.
Citation Information
Cited By
Method of making a concrete or mortar mixture and of making a structural component
EP4763823A1
Method of making a concrete or mortar mixture and of making a structural component
WO2026132245A1