Aircraft skin cleaning method based on composite laser

CN118768323AActive Publication Date: 2024-10-15SICHUAN UNIV +1

Patent Information

Application Number
CN202411072308.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-15
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

When existing laser paint removal technology treats multi-layer structural surfaces, a single laser cleaning can easily cause paint layer ablation to adhere to the substrate or cause irreversible damage, and the control of paint removal parameters for multi-laser combinations has not been discussed.

Method used

A composite laser paint removal device is used to conduct a small circular area cleaning simulation experiment by combining continuous laser and pulse laser to control laser parameters, including the power density of the flat-top beam and Gaussian beam of the continuous laser, and the energy density and frequency of the pulse laser. Determine the optimal paint removal parameters and fit the relationship model between continuous laser power density and cleaning depth.

Benefits of technology

It effectively solves the problem of ablation adhesion during continuous laser cleaning of aircraft skins, comprehensively considers the laser effect, determines the optimal paint removal parameters, and achieves non-destructive cleaning of aircraft skins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768323A_ABST
    Figure CN118768323A_ABST
Patent Text Reader

Abstract

The invention discloses an aircraft skin cleaning method based on composite laser. The aircraft skin cleaning method comprises the steps that S1, a composite laser paint removing device for outputting continuous laser and pulse laser is constructed; s2, a composite laser paint removal device is used for carrying out a small round area cleaning simulation experiment on the aircraft skin, and optimal paint removal parameters are determined; s3, based on the optimal paint removal parameters, fitting to obtain a relation model between the power density of the continuous laser and the cleaning depth; and S4, carrying out aircraft skin cleaning according to the relation model. The composite laser formed by combining the continuous laser and the pulse laser is used for cleaning the aircraft skin, and the problem that when the continuous laser is used for cleaning the aircraft skin, ablated matter generated by ablating a paint layer adheres to a substrate and is not easy to remove is effectively solved; by determining the relation model between the power density and the cleaning depth obtained by fitting the optimal paint removal parameters during composite laser cleaning, the laser parameters can be adjusted based on the relation model, and reference is provided for laser removal cleaning of the aircraft skin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser paint removal, and in particular relates to an aircraft skin cleaning method based on a composite laser. Background Art

[0002] In recent years, laser cleaning technology, as an emerging cleaning technology, has developed rapidly. Compared with traditional cleaning methods, laser cleaning has shown great development potential in many fields due to its advantages such as higher efficiency, pollution-free and non-destructive.

[0003] In existing research, most of the cleaning is done by using a certain laser alone. The research on using various lasers for combined cleaning is a new laser cleaning idea that has only been studied in recent years. The surface paint layer of many objects to be cleaned (aircraft, trains, etc.) is a multi-layer structure, and there are differences in the physical and chemical properties of each paint layer. If a continuous laser is used alone to clean the paint layer, it is easy to cause the paint layer ablation to adhere to the substrate, thereby damaging the substrate; if a pulsed laser is used alone to clean the paint layer, it is very easy to cause the pulsed laser energy to be too large, causing irreversible damage to the substrate. If the continuous laser and the pulsed laser are combined into a composite laser, the object with a multi-layer paint structure is cleaned, because the composite laser can adjust the laser parameters, it is easier to achieve layered paint removal and improve the paint removal effect. Although most of the research on paint removal cleaning at this stage is a single system, it is the basis for multi-laser combination cleaning. Existing scholars at home and abroad generally achieve the improvement of cleaning effect by controlling parameters such as laser energy, frequency and scanning speed, although the parameter control of multi-laser combination paint removal has not been discussed. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the aircraft skin cleaning method based on composite laser provided by the present invention solves the problem that the paint removal parameters are not considered in the existing composite laser paint removal method.

[0005] In order to achieve the above-mentioned purpose of the invention, the technical solution adopted by the present invention is: a method for cleaning aircraft skin based on a composite laser, comprising the following steps:

[0006] S1. Constructing a composite laser paint removal device that outputs continuous laser and pulsed laser;

[0007] S2. Use a composite laser paint removal device to conduct a small circular area cleaning simulation experiment on the aircraft skin to determine the optimal paint removal parameters;

[0008] S3. Based on the optimal paint removal parameters, a relationship model between the power density of the continuous laser and the cleaning depth during composite laser paint removal is obtained by fitting;

[0009] S4. Clean the aircraft skin according to the relational model.

[0010] Furthermore, in step S1, the composite laser paint removal device includes a continuous laser and a pulse laser, and the continuous laser and pulse laser emitted by the continuous laser and the pulse laser respectively pass through a beam splitter and a reflector and then act on the aircraft skin through a focusing lens.

[0011] Furthermore, in the composite laser paint removal device, the angle between the continuous laser and the pulse laser when incident on the focusing lens is 20°.

[0012] Furthermore, the transmission and reflection energy ratio of the corresponding split laser beams obtained by the continuous laser and the pulse laser through the beam splitter is 8:2.

[0013] Furthermore, the continuous laser includes a flat-top beam and a Gaussian beam, and the Gaussian beam covers the center of the flat-top beam.

[0014] Furthermore, in step S2, the paint removal parameters include the flat-top beam power density and Gaussian beam power density in the continuous laser, the energy density and frequency of the pulsed laser, and the cleaning time.

[0015] Furthermore, the step S2 is specifically as follows:

[0016] S21, using a continuous laser with a preset power density to clean a small circular area of ​​the aircraft skin;

[0017] S22, using a pulsed laser with a preset energy density and frequency to act on the cleaning area of ​​the continuous laser to achieve composite laser cleaning;

[0018] S23, analyzing the cleaning effect of the aircraft skin in the composite laser cleaning area, and setting different paint removal parameters;

[0019] S24, continuously adjust the paint removal parameters and clean the aircraft skin;

[0020] S25. Analyze the aircraft skin cleaning effect under different paint removal parameters, and take the paint removal parameters corresponding to the best paint removal effect as the best paint removal parameters.

[0021] Furthermore, the step S3 is specifically as follows:

[0022] S31, based on the corresponding cleaning experimental data of the optimal paint removal parameters, a power function is used to fit the relationship between the cleaning depth and the cleaning time;

[0023] S32, respectively setting a change ratio p1 of the power density of the flat-top beam in the continuous laser and a change ratio p2 of the power density of the Gaussian beam;

[0024] S33, based on the relationship between the cleaning depth and the cleaning time, and the size change ratios p1 and p2, a relationship model between the power density of the continuous laser and the cleaning depth is obtained by fitting.

[0025] The beneficial effects of the present invention are:

[0026] (1) The present invention uses a composite laser formed by a combination of continuous laser and pulsed laser to clean the aircraft skin, which effectively solves the problem that the ablated products produced by the ablation of the paint layer when using continuous laser to clean the aircraft skin adhere to the substrate and are difficult to remove.

[0027] (2) The method of the present invention comprehensively considers the effects of continuous laser and pulsed laser, determines the optimal paint removal parameters during composite laser cleaning based on a small circular cleaning experiment, and fits the relationship model between power density and cleaning depth at a certain moment. The laser parameters can be adjusted based on the relationship model, providing a reference for laser cleaning of aircraft skin. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A flow chart of the aircraft skin cleaning method based on composite laser provided by the present invention.

[0029] Figure 2 This is a schematic structural diagram of the composite laser paint removal device provided by the present invention.

[0030] Figure 3 This is a schematic diagram of the aircraft skin sample provided by the present invention.

[0031] Figure 4 This is a schematic diagram of the cleaning effect of the Gaussian beam provided by the present invention.

[0032] Figure 5 This is a schematic diagram of the composite laser effect provided by the present invention.

[0033] Figure 6 This is a diagram of the composite laser cleaning effect composed of continuous laser and pulse laser with various parameters provided by the present invention.

[0034] Figure 7 A schematic diagram of the cleaning effect of a small circular area of ​​an aircraft skin using a composite laser provided by the present invention.

[0035] Figure 8 This is a schematic diagram of the cleaning depth variation with time curve provided by the present invention. DETAILED DESCRIPTION

[0036] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0037] Embodiment 1:

[0038] The embodiment of the present invention provides a method for cleaning aircraft skin based on a composite laser, such as Figure 1 As shown, the following steps are included:

[0039] S1. Constructing a composite laser paint removal device that outputs continuous laser and pulsed laser;

[0040] S2. Use a composite laser paint removal device to conduct a small circular area cleaning simulation experiment on the aircraft skin to determine the optimal paint removal parameters;

[0041] S3. Based on the optimal paint removal parameters, a relationship model between the power density of the continuous laser and the cleaning depth during composite laser paint removal is obtained by fitting;

[0042] S4. Clean the aircraft skin according to the relational model.

[0043] In step S1 of the embodiment of the present invention, the composite laser paint removal device is constructed as follows Figure 2 As shown, it includes a continuous laser and a pulse laser, the continuous laser and the pulse laser emitted by the continuous laser and the pulse laser respectively pass through a beam splitter and a reflector and then act on the aircraft skin through a focusing lens; wherein the continuous laser includes a flat-top beam and a Gaussian beam, and the Gaussian beam covers the center of the flat-top beam.

[0044] In the composite laser paint removal device of this embodiment, the angle between the continuous laser and the pulse laser when incident on the focusing lens is 20°.

[0045] In this embodiment, the transmission and reflection energy ratio of the corresponding split laser beams obtained by the continuous laser and the pulse laser through the beam splitter is 8:2.

[0046] Specifically, in this embodiment, the output beam of the continuous laser can be flat-top and Gaussian, with an output energy between 50W and 2000W, a minimum irradiation time of 30ms, and an output spot diameter of 700μm to 1100μm; the pulse laser energy range of the pulse laser output is 0.2J to 2J, the output frequency range is 1Hz to 20Hz, and the output spot diameter is 2mm.

[0047] When the composite laser paint removal device is working, the continuous laser and the pulsed laser are divided into two beams by a beam splitter, and 80% of the laser energy of the continuous laser and the pulsed laser are applied to the aircraft skin at an angle of 20° after passing through a 1064 reflector and a focusing lens (focal length of 20 cm), and the remaining 20% ​​of the laser energy is used for energy monitoring. In this embodiment, the aircraft skin is placed on a computer-controlled 3D platform for precise adjustment of laser cleaning.

[0048] In step S2 of the embodiment of the present invention, the paint removal parameters include the flat-top beam power density and Gaussian beam power density in the continuous laser, the energy density and frequency of the pulsed laser, and the cleaning time. The cleaning time refers to the action time of the continuous laser, and the pulsed laser acts within the action time of the continuous laser, that is, when the continuous laser stops acting, the pulsed laser also stops acting.

[0049] Step S2 of the embodiment of the present invention is specifically as follows:

[0050] S21, using a continuous laser with a preset power density to clean a small circular area of ​​the aircraft skin;

[0051] S22, using a pulsed laser with a preset energy density and frequency to act on the cleaning area of ​​the continuous laser to achieve composite laser cleaning;

[0052] S23, analyzing the cleaning effect of the aircraft skin in the composite laser cleaning area, and setting different paint removal parameters;

[0053] S24, continuously adjust the paint removal parameters and clean the aircraft skin;

[0054] S25. Analyze the aircraft skin cleaning effect under different paint removal parameters, and take the paint removal parameters corresponding to the best paint removal effect as the best paint removal parameters.

[0055] In this embodiment, Figure 3 The Boeing 717 model aircraft skin sample shown in the figure is used as an example to carry out a small circular area cleaning simulation experiment. The sample has a 1 mm bright silver aluminum alloy metal substrate. The aluminum alloy surface has three layers of materials: red polyurethane topcoat (thickness of about 79 μm), gray epoxy primer and yellow-green chemical conversion coating (thickness of about 130 μm).

[0056] In step S21 of this embodiment, when cleaning the paint layer of the aircraft skin, the characteristics of each paint layer must be fully considered to keep the metal substrate intact as much as possible. In order to make up for the defects of single-mechanism laser cleaning, the Gaussian beam and the flat-top beam are combined into a continuous laser, and a composite laser is formed with a pulsed laser for further cleaning experiments, and the influence of the composite laser under different parameter settings on the cleaning effect of the aircraft skin is explored.

[0057] The effect of cleaning the aircraft skin with Gaussian beams of different powers is as follows: Figure 4 As shown in the figure, it can be seen that as the laser action time increases, the cleaning area gradually becomes larger. The cleaning area includes the silver bright area (the metal base of the aircraft skin is silver bright) and the black area, among which the area of ​​the silver bright area gradually increases, and the area of ​​the black area in the center remains basically unchanged. At the same time, at the same action time point, as the laser power increases from 50W to 100W, the area of ​​the cleaning area gradually increases, and when using Gaussian beam cleaning, the power is 100W and the action time is 100ms, the cleaning range is the largest.

[0058] Although Gaussian beams can clean the paint layer on the surface of aircraft skin, there is a black area in the center after the aircraft skin is cleaned using a 50W to 100W Gaussian beam. Due to the characteristics of the Gaussian beam "high energy in the center and low energy in the surroundings", it can be preliminarily inferred that there may be two situations in which the black area is formed. One is that the paint layer is over-ablated, and black oxides are formed in the center and adhere to the substrate; the other is that the paint layer in the center is instantly vaporized by high temperature, causing black ablation damage to the substrate. The black area is obviously not what should remain after normal cleaning of the aircraft skin. In order to further improve the paint removal effect, improvements to the cleaning light source will be considered in the future.

[0059] In step S22 of this embodiment, in order to make up for the deficiency of Gaussian beam in aircraft skin cleaning, it is considered to add a flat-top beam so that the Gaussian beam is combined into a continuous laser. The purpose is to make the temperature change on the aircraft skin surface more uniform during the paint removal and cleaning process, and avoid the situation where the middle temperature is much higher than the surrounding temperature. At the same time, the high energy effect of the Gaussian beam on the center of the cleaning area is conducive to the ablation effect that spreads from the center of the area to the surrounding area, thereby improving the cleaning effect. In addition, since the black area may be a paint layer ablation, it is considered to add a pulsed laser in the expectation that the stress effect generated by it will remove the residual ablation. Figure 5 These are the preliminary experimental results of the composite laser composed of continuous laser (Gaussian beam plus flat-top beam) and pulsed laser for cleaning aircraft skin.

[0060] Because a large amount of the central black area was removed after the composite laser was applied, it is speculated that the black area is the ablation product formed by the ablation and oxidation of the topcoat and primer. Figure 2 From the experimental materials shown, it can be preliminarily determined that the gray area is the primer that has not been completely ablated, and the silver bright area is the metal substrate. This experiment shows that the composite laser composed of continuous laser and pulsed laser can effectively clean the paint layer on the surface of the aircraft skin, in which the ablation effect of the continuous laser causes the paint layer to be ablated and oxidized, and the stress effect of the pulsed laser causes the oxide ablated from the paint layer to be removed.

[0061] In step S23 of this embodiment, since in the composite laser skin cleaning result, the cleaned skin only exposes part of the metal base (silver bright area), and the paint layer (gray area) and the ablated material (black area) are not completely removed, it is planned to use a composite laser composed of a continuous laser with higher power density and a pulsed laser with different energy densities to remove the paint from the skin to find the best cleaning parameters. There are four main parameters to consider, namely the power density of the Gaussian beam and the flat-top beam, the energy density of the pulsed laser, and the laser action time. In addition, each experiment ensures that the pulsed laser acts at least once during the cleaning process.

[0062] like Figure 6 As shown, when the flat-top beam power density is 105.28W / mm 2 and Gaussian beam power density is 113.23W / mm 2 The skin is cleaned by continuously increasing the energy density of the pulsed laser. When at least one pulsed laser action is ensured, a black area exists regardless of whether the laser action time is 50ms or 100ms. When the continuous laser action time is 50ms, the area of ​​the black area increases first and then decreases with the increase of the pulsed laser energy density. However, when the action time is increased to 100ms, the area of ​​the black area decreases first, then increases, and finally decreases with the increase of the pulsed laser energy density. At the same time, there are scattered silver bright areas in the gray area.

[0063] When the flat-top beam power density is increased to 157.92W / mm 2 , and when the power density of the Gaussian beam remains unchanged, the energy density of the pulsed laser is continuously increased to clean the skin. When at least one pulsed laser is applied, it is also found that no matter the cleaning time is 50ms or 100ms, black areas remain on the surface. Figure 6 (i)~ Figure 6 (p), it can be found that the size of the remaining black area is basically the same, but compared with Figure 6 (a)~ Figure 6 (h) The difference between these experimental results is that the gray area is significantly reduced, and the distribution of the bright silver area in the gray area increases.

[0064] In addition, under the same continuous laser power density and at least one pulse laser action, whether the continuous laser action is 50ms or 100ms, the silver bright area of ​​the substrate is mixed with the gray area. Figure 6 Among all the cleaning results, the lowest cleaning depth of all cleaning results is 225.0μm (>220μm). Combined with the observation of silver bright area, it shows that the composite laser does clean the metal substrate.

[0065] Therefore, the stress effect of the pulsed laser does have a removal effect on the black area (the ablated paint layer). Figure 6 The experimental results show that after adjusting the energy density and action time of the pulsed laser for many times, there will be residual black areas. This shows that the residual black areas may not all be the ablation products of the paint layer. Therefore, EDS analysis is considered for the black areas to determine whether they are all the ablation products of the paint layer. At the same time, EDS analysis is performed on the other color areas to determine their material composition.

[0066] Combining all the above experimental results and EDS analysis, the following experimental conclusions can be drawn:

[0067] ① The silver bright area after cleaning is the metal base, the gray area is the primer, the black area is the oxides produced by the ablation of the paint layer and the oxides produced by metal damage, and there are even unablated topcoats and primers;

[0068] ② In the composite laser skin cleaning experiment with different parameter settings, the overall power density of the continuous laser may be too high, resulting in ablation and oxidation damage to the metal substrate, turning it black, regardless of whether the continuous laser action time is 50ms or 100ms. The stress effect of the pulsed laser cannot remove this black material.

[0069] ③ By Figure 6 It can be seen from the experiment that although increasing the power density of continuous laser is beneficial to the reduction of gray area (primer), combined with the element content ratio analyzed by EDS, increasing the power density of continuous laser may cause the metal substrate to melt, resulting in a mixed distribution of gray area and silver bright area.

[0070] Based on the above experiments, it can be seen that the composite laser composed of continuous laser and pulsed laser can indeed clean the paint layer on the surface of the skin, but the high power density of the continuous laser will lead to two situations that are not conducive to cleaning: one is damage to the metal substrate, and the other is melting of the metal substrate and merging with the primer. In order to avoid the above negative situations, subsequent experiments will consider reducing the power density of the continuous laser in the composite laser. At the same time Figure 6 The experiment used 0.42J / mm 2 ~1.05J / mm 2 However, this series of pulsed lasers had no significant difference in the removal effect of black matter, and high-energy-density pulsed lasers may cause substrate damage. Therefore, the pulsed laser energy density in subsequent experiments was set to 0.42 J / mm 2 In addition, no matter how long the total cleaning time is, the continuous laser action time is gradually controlled while ensuring that the pulse laser acts at least once in each experiment to conduct further experiments. The experimental results are shown in Figure 7 shown.

[0071] Experiments have shown that by setting appropriate parameters and further controlling the action time, it is indeed possible to achieve non-destructive removal of paint on the skin surface by composite laser. Figure 7 It shows that when the flat-top beam power density is 52.64W / mm 2 , Gaussian beam power density is 56.62W / mm 2 The continuous laser and energy density are 0.42J / mm 2 , the skin cleaning morphology of the composite laser composed of a pulse laser with a frequency of 10Hz at each time point, compared with Figure 6 The experiment reduced the overall energy of the continuous laser, further refined the control of the continuous laser action time, and ensured that the pulsed laser acted at least once before the cleaning was completed.

[0072] When the continuous laser action time is as short as 50ms, it can be observed that most of the surface of the cleaning area is red, and the center is a yellow area. When the continuous laser action time is increased to 80ms, the surface of the cleaning area is basically all silver, without black and gray areas, which is very close to the original morphology of the metal substrate. The cleaning result at this time is already very impressive. In order to further explore the effect of the composite laser on the skin under this parameter setting, the cleaning time is increased to 2000ms. At this time, a very small black area begins to remain on the surface of the cleaning area, but the rest of the area is still basically silver, which is closer to the morphology of the metal substrate. When the cleaning time is further increased to 5000ms, there is a large area of ​​black area on the surface of the cleaning area, indicating that the cleaning effect is significantly reduced.

[0073] When the cleaning time is less than 80ms, the cleaning depth increases with time, indicating that the paint layer on the skin surface is removed by the composite laser. When the cleaning time reaches 2000ms, the substrate is slightly damaged, indicating that between 80ms and 2000ms, the temperature of the skin surface is basically maintained below the melting point of the substrate, which indirectly shows that the composite laser with this parameter setting has high controllability for keeping the aircraft skin intact.

[0074] Based on the results of the above series of skin cleaning experiments, the paint removal parameters for the best paint removal effect are set to: the flat-top beam power density of the continuous laser part is about 52.64W / mm 2 , the Gaussian beam power density is about 56.62W / mm 2 , and the energy density of the pulse laser part is about 0.42J / mm 2 , the frequency is about 10Hz.

[0075] In the embodiment of the present invention, step S3 is specifically as follows:

[0076] S31, based on the corresponding cleaning experimental data of the optimal paint removal parameters, a power function is used to fit the relationship between the cleaning depth and the cleaning time;

[0077] S32, respectively setting a change ratio p1 of the power density of the flat-top beam in the continuous laser and a change ratio p2 of the power density of the Gaussian beam;

[0078] S33, based on the relationship between the cleaning depth and the cleaning time, and the size change ratios p1 and p2, a relationship model between the power density of the continuous laser and the cleaning depth is obtained by fitting.

[0079] In this embodiment, based on the above series of cleaning experiments and simulations, the mechanism of composite laser cleaning aircraft skin can be clearly understood. The continuous laser part of the composite laser has an ablation effect on the topcoat and primer, which makes the paint layer become an ablation that is easy to detach from the skin surface. At the same time, the pulsed laser part of the composite laser produces a stress effect on the ablation to achieve thorough cleaning of the paint layer. Therefore, we must consider the skin cleaning process in two parts, first ablating the paint layer and then removing the ablation. If the power density of the continuous laser is too high, although it will ablate all the topcoats and primers, and the removal efficiency of the paint layer will be improved on the surface, it may actually cause ablation defects on the metal substrate, thereby reducing the cleaning effect. At the same time, a continuous laser with too high power density may also cause the metal substrate to melt and merge with the primer, which also causes damage to the substrate and also reduces the cleaning effect. In addition, the continuous laser only plays a stress effect to remove the ablation residues of the paint layer, and the removal efficiency of the ablation residues has no obvious relationship with the energy density of the pulsed laser itself. In addition, in order to avoid stress damage to the substrate caused by the stress effect of the pulsed laser, try to avoid using a high energy density pulsed laser and a continuous laser to form a composite laser. Therefore, the removal of topcoat and primer on the skin surface by the composite laser is mainly based on the ablation of the paint layer by the continuous laser, while the stress effect of the pulsed laser assists in the removal of the ablated paint layer. The previous analysis shows that when the composite laser is used to clean a small circular area on the aircraft skin, the optimal cleaning parameter setting range is "the power density of the flat-top beam in the continuous laser part is 52.64W / mm 2 ~73.7W / mm 2 , the power density of the Gaussian beam is 56.62W / mm 2 ~79.26W / mm 2 , while the energy density of the pulse laser part is fixed at 0.42J / mm 2 , the frequency is fixed at 10Hz".

[0080] The ablation effect of the continuous laser part in the composite laser is the main effect, and the stress effect of the pulsed laser part is the secondary effect. The ablation effect is mainly related to the parameter setting of the continuous laser, and the basis for judging non-destructive cleaning is the cleaning depth, so the focus is on exploring the relationship between the cleaning depth and the continuous laser power density.

[0081] In step S21 of this embodiment, the relationship between the cleaning depth and the cleaning time is first explored. Figure 8 The simulation curves of the relationship between the cleaning depth l and time (0-80ms) under three composite laser parameter settings are shown. The cleaning depth l under two parameter settings reaches the base. Therefore, the simulation data under these two composite laser parameter settings are fitted with the following power function:

[0082] l=a(bt) 2 +c

[0083] The following relationship can be obtained:

[0084] When the power density of the flat-top beam in the continuous laser of the composite laser is 52.64W / mm2 and the power density of the Gaussian beam is 56.62W / mm2, the above power function becomes as follows:

[0085] l=0.404×(0.2564t) 2 +0.4991

[0086] In step S32 of this embodiment, when the flat-top beam power density is 52.64 W / mm 2 And Gaussian beam power density 56.62W / mm 2 On the basis of, when the power density of the two beams changes, let the ratio of the flat-top beam power density change be p1, and the ratio of the Gaussian beam power density change be p2, as shown in the following two formulas:

[0087]

[0088] Among them, α1 is the power density of the flat-top beam, and α2 is the power density of the Gaussian beam.

[0089] In step S33 of this embodiment, the above formula is combined to obtain the relationship model between the power density and the cleaning depth at a certain moment as follows:

[0090] l=0.404[1.6×(p1-0.2)+2×(p2-0.3)](0.2564t) 2 +0.4991

[0091] In step S4 of the embodiment of the present invention, when cleaning the aircraft skin, the aircraft skin is cleaned based on the cleaning depth requirement, according to the above relationship model, and the pulse energy density and frequency obtained when determining the optimal paint removal parameters.

[0092] Embodiment 2:

[0093] In this embodiment, the credibility of the relationship model obtained in Example 1 is tested, and specific data of the composite laser parameters are set and substituted into the above relationship model to obtain the following: Figure 8 The change curve is shown, and the specific values ​​of the cleaning depth of 50ms and 80ms are shown in Table 1.

[0094] Table 1: Theoretical cleaning depth table

[0095]

[0096] Table 1 shows that when α1 is 52.64 W / mm 2 , α2 is 56.62W / mm 2 The theoretical calculated cleaning depth at 80ms is 257.3242μm, which is basically consistent with the cleaning depth at 80ms in EDS analysis. In addition, when α1 is 105.28W / mm 2 , α2 is 113.23W / mm 2 And α1 is 157.92W / mm 2 , α2 is 113.23W / mm 2 The theoretically calculated cleaning depth is greater than 220μm at 50ms, which is greater than the sum of the thickness of the topcoat, primer and composite coating. This indicates that the cleaning has reached the metal substrate and caused damage to the substrate at 50ms. At 100ms, the theoretically calculated depth is far more than 220μm, indicating that the damage is greater. Figure 6 The experimental results obtained in the paper are consistent with those in the previous paper, which also indirectly verifies the objectivity and feasibility of the "relationship model between power density and cleaning depth at a certain moment" derived from this theory, and also shows that it does have guiding value for actual laser paint removal.

[0097] The present invention uses specific embodiments to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

[0098] Those skilled in the art will appreciate that the embodiments described herein are intended to help readers understand the principles of the present invention, and should be understood that the protection scope of the present invention is not limited to such specific statements and embodiments. Those skilled in the art can make various other specific variations and combinations that do not deviate from the essence of the present invention based on the technical revelations disclosed by the present invention, and these variations and combinations are still within the protection scope of the present invention.

Claims

1. A composite laser-based aircraft skin cleaning method, characterized in that: The following steps are involved: S1. Constructing a composite laser paint removal device that outputs continuous laser and pulsed laser; S2. Use a composite laser paint removal device to conduct a small circular area cleaning simulation experiment on the aircraft skin to determine the optimal paint removal parameters; S3. Based on the optimal paint removal parameters, a relationship model between the power density of the continuous laser and the cleaning depth during composite laser paint removal is obtained by fitting; S4. Clean the aircraft skin according to the relational model.

2. The aircraft skin cleaning method based on composite laser according to claim 1 is characterized in that: In step S1, the composite laser paint removal device includes a continuous laser and a pulse laser. The continuous laser and the pulse laser emitted by the continuous laser and the pulse laser respectively pass through a beam splitter and a reflector and then act on the aircraft skin through a focusing lens.

3. The aircraft skin cleaning method based on composite laser according to claim 2 is characterized in that: In the composite laser paint removal device, the angle between the continuous laser and the pulse laser when incident on the focusing lens is 20°.

4. The aircraft skin cleaning method based on composite laser according to claim 2 is characterized in that: The transmission and reflection energy ratio of the corresponding split laser beams obtained by the continuous laser and the pulse laser through the beam splitter is 8:

2.

5. The aircraft skin cleaning method based on composite laser according to claim 2 is characterized in that: The continuous laser includes a flat top beam and a Gaussian beam, and the Gaussian beam covers the center of the flat top beam.

6. The aircraft skin cleaning method based on composite laser according to claim 1 is characterized in that: In the step S2, the paint removal parameters include the flat-top beam power density and Gaussian beam power density in the continuous laser, the energy density and frequency of the pulsed laser, and the cleaning time.

7. The aircraft skin cleaning method based on composite laser according to claim 5 is characterized in that: The step S2 is specifically as follows: S21, using a continuous laser with a preset power density to clean a small circular area of ​​the aircraft skin; S22, using a pulsed laser with a preset energy density and frequency to act on the cleaning area of ​​the continuous laser to achieve composite laser cleaning; S23, analyzing the cleaning effect of the aircraft skin in the composite laser cleaning area, and setting different paint removal parameters; S24, continuously adjust the paint removal parameters and clean the aircraft skin; S25. Analyze the aircraft skin cleaning effect under different paint removal parameters, and take the paint removal parameters corresponding to the best paint removal effect as the best paint removal parameters.

8. The aircraft skin cleaning method based on composite laser according to claim 1 is characterized in that: The step S3 is specifically as follows: S31, based on the corresponding cleaning experimental data of the optimal paint removal parameters, a power function is used to fit the relationship between the cleaning depth and the cleaning time; S32, respectively setting a change ratio p1 of the power density of the flat-top beam in the continuous laser and a change ratio p2 of the power density of the Gaussian beam; S33, based on the relationship between the cleaning depth and the cleaning time, and the size change ratios p1 and p2, a relationship model between the power density of the continuous laser and the cleaning depth is obtained by fitting.

Citation Information

Patent Citations

  • Process for cleaning surface of materials and device for carrying out this process, employing focussing of pulsed laser with short pulses on surface to be cleaned

    CN1048339A

  • Pre-welding laser cleaning method and device capable of efficiently removing aluminum alloy oxidation film

    CN108031687A

  • Laser washing device

    CN109719088A

  • High-frequency laser paint removal effect detection system and method

    CN115839944A

  • Large-area aircraft skin robot laser profiling cleaning and paint removing method

    CN116060384A

Cited By

  • Nondestructive laser cleaning method and cleaning device for surface of aluminum alloy workpiece

    CN119426279A

  • Low-temperature plasma jet paint removal method

    CN121892446A