A welding wire powder core, a wear-resistant submerged arc welding flux-cored wire, a preparation method and application thereof
By adding Nb to the flux core of the welding wire powder to form an NbC hard phase, the problem of easy peeling off of existing wear-resistant flux-cored welding wires is solved, the wear resistance and thermal stability of the weld layer are improved, and the service life of the rolls is extended.
Patent Information
- Application Number
- CN202410939043.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing wear-resistant flux-cored welding wires are prone to peeling off during the overlay welding repair process, leading to increased wear and affecting the service life of the rolls.
The welding wire core contains ferrochrome powder, ferroniobium powder, nickel powder, aluminum powder, activator, deoxidizer and rare earth oxides. By adding Nb element to form NbC hard phase, the wear resistance is improved and it is evenly distributed in hot rolled steel material to enhance the hardness and thermal stability of the weld layer.
It improves the wear resistance and thermal stability of the weld layer, reduces spalling, extends the service life of 60CrMnMo hot-rolled roll steel, avoids the occurrence of cracks during the welding process, and ensures a strong bond between the weld layer and the substrate.
Smart Images

Figure CN118768796B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding wire technology, and in particular to a welding wire powder core, a wear-resistant submerged arc welding flux-cored welding wire, its preparation method and application. Background Technology
[0002] As steel production grows rapidly, the consumption of rolling mill rolls is also intensifying. To meet the rolling requirements of steel products, the research and development of wear-resistant rolling mill rolls is accelerating.
[0003] 60CrMnMo is an alloy steel composed of elements such as carbon (C), chromium (Cr), manganese (Mn), and molybdenum (Mo). The addition of these elements gives 60CrMnMo good strength and wear resistance. Due to its large size and high replacement cost, 60CrMnMo roll steel can extend its service life and reduce production costs by performing surfacing repair on the rolls.
[0004] Currently, wear-resistant flux-cored welding wires used for surfacing repair generally contain alloying elements such as carbon, chromium, silicon, and manganese, with chromium accounting for a relatively high proportion, forming Cr7C3 and Cr... 23 C6 has poor high-temperature stability, becoming extremely unstable and prone to aggregation around 540℃, and easily peeling off during wear, thus exacerbating the wear process. Therefore, improving the wear resistance of flux-cored welding wire is an urgent problem to be solved. Summary of the Invention
[0005] The purpose of this invention is to provide a flux-cored welding wire powder, a wear-resistant submerged arc welding flux-cored welding wire, its preparation method and application, to solve the problem that existing wear-resistant flux-cored welding wires used for welding repair are prone to peeling off and thus aggravate wear.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0007] A welding wire powder core comprises the following raw materials in weight percentage:
[0008] The composition includes 25-46% chromium iron powder, 10.5-26.5% niobium iron powder, 0.5-1.5% nickel powder, 0.5-2% aluminum powder, 1-5% activator, 3-10% deoxidizer, 0.1-1% rare earth oxides, and 12.5-38% iron powder.
[0009] Preferably, in the above-mentioned welding wire powder core, the activator is one or both of BaF and CaF2.
[0010] Preferably, in the above-mentioned welding wire powder core, the deoxidizer is one or both of ferrosilicon and ferromanganese.
[0011] Preferably, in the above-mentioned welding wire powder core, the rare earth oxide is one or both of La2O3 and Ce2O3.
[0012] The present invention also provides a wear-resistant submerged arc welding flux-cored wire, comprising a steel strip and a welding wire powder core wrapped in the steel strip;
[0013] The welding wire powder core is the welding wire powder core described above;
[0014] The filling rate of the welding wire powder core in the steel strip is 30-50%.
[0015] Preferably, in the above-mentioned wear-resistant submerged arc welding flux-cored wire, the steel strip is made of H08A steel.
[0016] This invention also provides a method for preparing wear-resistant submerged arc welding flux-cored wire, comprising the following steps:
[0017] The raw materials for preparing welding wire powder core are mixed to obtain a dry mixture of welding wire powder core;
[0018] The steel strip is rolled into a U-shape to obtain a U-shaped steel strip;
[0019] The dry mixture of welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing welding wire powder core is rolled into an O-shape and then drawn to obtain wear-resistant submerged arc welding flux-cored wire.
[0020] The present invention also provides an application of wear-resistant submerged arc welding flux-cored wire in hot-rolled steel materials.
[0021] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0022] This invention adds Nb to the powder core. Since Nb is a strong carbide-forming element with a greater affinity for carbon than chromium, it preferentially combines with carbon to form an NbC hard phase, generating a new wear-resistant phase. This phase is uniformly dispersed within the weld overlay alloy, thereby refining the grains, reducing spalling, improving toughness, increasing the hardness of the weld overlay, and enhancing its wear resistance and thermal stability. Simultaneously, the weld layer exhibits good fusion and a strong bond with the 60CrMnMo hot-rolled roll steel base material, preventing cracks from appearing on the roll surface during welding, which could affect the roll quality and extend the service life of the 60CrMnMo hot-rolled roll steel. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0024] Figure 1This is a flowchart illustrating the preparation process of the wear-resistant submerged arc welding flux-cored wire in this invention.
[0025] Figure 2 The hardness distribution diagrams of the wear-resistant submerged arc welding flux-cored wire overlay and the base 60CrMnMo hot-rolled roll steel material after the first, second, and third overlays in Application Example 1 are shown.
[0026] Figure 3 The friction coefficient diagram of the wear-resistant submerged arc welding flux-cored wire weld overlay in Application Example 1;
[0027] Figure 4 The images show the appearance and weight loss of the wear-resistant submerged arc welding flux-cored wire overlay and the base material 60CrMnMo hot-rolled roll steel before and after wear in Application Example 1.
[0028] Figure 5 This is a microstructure diagram of the interface between the 60CrMnMo hot-rolled roll steel matrix and the wear-resistant submerged arc welding flux-cored wire weld overlay in Application Example 1.
[0029] Figure 6 This is a microstructure diagram of the weld overlay layer of the wear-resistant submerged arc welding flux-cored wire in Application Example 1. Detailed Implementation
[0030] A welding wire powder core comprises the following raw materials in weight percentage:
[0031] The composition includes 25-46% chromium iron powder, 10.5-26.5% niobium iron powder, 0.5-1.5% nickel powder, 0.5-2% aluminum powder, 1-5% activator, 3-10% deoxidizer, 0.1-1% rare earth oxides, and 12.5-38% iron powder.
[0032] In this invention, the mass percentage of the ferrochrome powder is preferably 25-46%, more preferably 28-40%, and even more preferably 35-38%.
[0033] In this invention, the mass percentage of the niobium iron powder is preferably 10.5-26.5%, more preferably 15-24%, and even more preferably 18-21%.
[0034] In this invention, the mass percentage of the nickel powder is preferably 0.5-1.5%, more preferably 0.6-1.2%, and even more preferably 0.8-1%.
[0035] In this invention, the mass percentage of the aluminum powder is preferably 0.5-2%, more preferably 0.6-1.5%, and even more preferably 1-1.2%.
[0036] In this invention, the mass percentage of the active agent is preferably 1-5%, more preferably 2-4%, and even more preferably 2.5-3%.
[0037] In this invention, the mass percentage of the deoxidizer is preferably 3-10%, more preferably 4-8%, and even more preferably 5-6%.
[0038] In this invention, the mass percentage of the rare earth oxide is preferably 0.1-1%, more preferably 0.2-0.8%, and even more preferably 0.5-0.6%.
[0039] In this invention, the mass percentage of the iron powder is preferably 12.5-38%, more preferably 15-36%, and even more preferably 20-30%.
[0040] In this invention, the composition of the ferrochrome powder is: Cr 60.0%–80.0 wt%, C ≤ 10 wt%, Si ≤ 3 wt%, with the balance being Fe. The function of the ferrochrome powder is to introduce alloying elements into the weld overlay alloy.
[0041] In this invention, the composition of the niobium-iron powder is: Nb 50.0%–70.0 wt%, C ≤ 0.1 wt%, Si ≤ 3 wt%, Al ≤ 3 wt%, with the balance being Fe. The niobium-iron powder preferentially combines with carbon in the weld overlay to form a NbC hard, wear-resistant phase.
[0042] In this invention, the nickel powder and aluminum powder are used to improve the hardenability of the weld overlay alloy.
[0043] In this invention, the activator is preferably one or both of BaF and CaF2, more preferably BaF. The activator functions to eliminate porosity in the molten pool and improve the weldability of the weld overlay alloy.
[0044] In this invention, the deoxidizer is preferably one or both of ferrosilicon and ferromanganese, more preferably ferrosilicon;
[0045] The ferrosilicon composition is Si 60.0%–80.0 wt%, C 0.01–0.1 wt%, with the balance being Fe;
[0046] The ferromanganese composition is 70-90 wt% Mn, 1-5 wt% Si, 0.1-1 wt% C, with the balance being Fe. The deoxidizer's function is to increase the strength and hardness of the weld overlay metal through deoxidation by silicon and manganese. Both silicon and manganese are strong deoxidizers; therefore, using a combined silicon-manganese deoxidation method results in a more ideal deoxidation effect.
[0047] In this invention, the rare earth oxide is preferably one or both of La2O3 and Ce2O3, more preferably La2O3. The role of the rare earth oxide is to refine the microstructure of the weld overlay alloy, making the carbides more uniformly distributed in the matrix.
[0048] In this invention, the iron powder serves to supplement the welding alloy with alloying elements.
[0049] The present invention also provides a wear-resistant submerged arc welding flux-cored wire, comprising a steel strip and a flux-cored wire powder wrapped in the steel strip;
[0050] The welding wire powder core is the welding wire powder core described above;
[0051] The filling rate of the welding wire powder core in the steel strip is 30-50%, more preferably 32-45%, and even more preferably 33-40%.
[0052] In this invention, the steel strip is preferably made of H08A steel.
[0053] In this invention, the diameter of the wear-resistant submerged arc welding flux-cored wire is preferably 2.4-4 mm, more preferably 2.5-3.8 mm, and even more preferably 3-3.5 mm.
[0054] This invention also provides a method for preparing wear-resistant submerged arc welding flux-cored wire, comprising the following steps:
[0055] The raw materials for preparing welding wire powder core are mixed to obtain a dry mixture of welding wire powder core;
[0056] The steel strip is rolled into a U-shape to obtain a U-shaped steel strip;
[0057] The dry mixture of welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing welding wire powder core is rolled into an O-shape and then drawn to obtain wear-resistant submerged arc welding flux-cored wire.
[0058] In this invention, the pretreatment of the raw materials for preparing the welding wire powder core is drying. The drying temperature is preferably 180-250°C, more preferably 190-240°C, and even more preferably 200-210°C. The drying time is 1.5-3 hours, more preferably 1.75-2.5 hours, and even more preferably 2 hours.
[0059] In this invention, the specific method of mixing is as follows: stirring and mixing in a V-type mixer; the mixing time is preferably ≥120 min, more preferably 120-200 min, and even more preferably 150 min.
[0060] The process flow diagram for preparing wear-resistant submerged arc welding flux-cored wire is as follows: Figure 1 As shown.
[0061] The present invention also provides an application of wear-resistant submerged arc welding flux-cored wire in hot-rolled steel materials.
[0062] In this invention, the hot-rolled roll steel material is preferably 60CrMnMo hot-rolled roll steel material.
[0063] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0064] Example 1
[0065] A wear-resistant submerged arc welding flux-cored wire includes an outer steel strip and a powder core wrapped in the steel strip; the powder core has a filling rate of 33% in the steel strip; the steel strip is made of H08A steel.
[0066] The welding wire powder core includes the following raw materials in terms of mass percentage:
[0067] 28% chromium iron powder, 21% niobium iron powder, 1% nickel powder, 1% aluminum powder, 2% activator, 10% deoxidizer, 1% rare earth oxides, and 36% iron powder;
[0068] The composition of ferrochrome powder is: Cr 70wt%, C 8.5wt%, Si 0.6wt%, with the balance being Fe;
[0069] The composition of the niobium-iron powder is: Nb 65wt%, C 0.07wt%, Si 2.6wt%, Al 1.5wt%, with the balance being Fe;
[0070] The surfactant is BaF;
[0071] The deoxidizer is a mixture of ferrosilicon and ferromanganese, with a mass ratio of ferrosilicon to ferromanganese of 1:10;
[0072] The ferrosilicon composition is 74wt% Si, 0.05wt% C, and the balance is Fe;
[0073] The composition of the ferromanganese is 80wt% Mn, 1.35wt% Si, 0.1wt% C, with the balance being Fe;
[0074] The rare earth oxides are a mixture of La2O3 and Ce2O3; the mass ratio of La2O3 to Ce2O3 is 1:1.
[0075] The preparation method of the above-mentioned wear-resistant submerged arc welding flux-cored wire includes the following steps:
[0076] The raw materials for preparing the welding wire powder core were dried at 200℃ for 2 hours, and then the dried raw materials were added to a V-type powder mixer and stirred for 150 minutes to obtain a dry mixture of welding wire powder core.
[0077] H08A steel strip is rolled into a U-shape to obtain U-shaped steel strip;
[0078] The dry mixture of welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing the powder core is rolled into an O-shape and then drawn to obtain a wear-resistant submerged arc welding flux-cored wire with a diameter of 3mm.
[0079] Application Example 1
[0080] The surface of the 60CrMnMo hot-rolled steel material was polished with coarse sandpaper, and then cleaned with anhydrous ethanol to obtain the treated 60CrMnMo hot-rolled steel material. An automatic submerged arc welding machine was used to perform the first layer of welding on the surface of the treated 60CrMnMo hot-rolled steel material with the wear-resistant submerged arc welding flux-cored wire prepared in Example 1. After the first layer was welded, the surface was kept at a certain temperature for one minute before the second layer was welded. After the second layer was welded, the surface was kept at a certain temperature for one minute before the third layer was welded. After the third layer was welded, the 60CrMnMo hot-rolled steel material and the weld alloy formed by welding were cooled to room temperature in air to complete the welding, forming a wear-resistant submerged arc welding flux-cored wire welding layer on the 60CrMnMo hot-rolled steel material. The conditions for the first layer welding, the second layer welding, and the third layer welding were as follows: welding current of 380A, voltage of 30V, welding speed of 360mm / min, and wire feed speed of 500mm / min.
[0081] Figure 2 This is a hardness distribution diagram of the wear-resistant submerged arc welding flux-cored wire overlay layer and the base 60CrMnMo hot-rolled roll steel material after the first, second, and third overlay layers in Application Example 1. Figure 2 It can be seen that the base material, 60CrMnMo hot-rolled roll steel, has the lowest hardness. As the number of weld overlay layers increases, the hardness of the wear-resistant submerged arc welding flux-cored wire weld overlay layer gradually increases, reaching its maximum hardness at the third layer. Among these, Figure 2 The horizontal axis in the figure represents the points that are drilled sequentially from the substrate to the weld overlay to measure the hardness. The first 4 points are drilled on the substrate, 5-13 are drilled on the first weld overlay, 14-21 are drilled on the second weld overlay, and 22-30 are drilled on the third weld overlay.
[0082] Figure 3 This is a graph showing the friction coefficient of the weld overlay layer from the wear-resistant submerged arc welding flux-cored wire in Application Example 1. Figure 3 It can be seen that in the initial stage of wear, the coefficient of friction increases sharply, and after 1 minute it tends to stabilize at a coefficient of friction of 0.35. In the subsequent wear process, the coefficient of friction remains basically unchanged.
[0083] Figure 4 This image shows the appearance and weight loss of the wear-resistant submerged arc welding flux-cored wire surfacing layer and the base material of the 60CrMnMo hot-rolled roll steel before and after wear, as well as the wear-related weight loss figures, in Application Example 1. Figure 4 It can be seen that after the wear test, the wear loss of the weld overlay alloy is very small, only 0.0001 grams, while the wear loss of the substrate is relatively high.
[0084] Figure 5 This is a microstructure image of the interface between the 60CrMnMo hot-rolled roll steel matrix and the wear-resistant submerged arc welding flux-cored wire weld overlay in Application Example 1. Figure 5 It can be seen that the left side is the 60CrMnMo hot-rolled steel plate substrate, and the right side is the weld overlay layer. The interface is well bonded and there is no cracking.
[0085] Figure 6 This is a microstructure diagram of the weld overlay layer of the wear-resistant submerged arc welding flux-cored wire used in Application Example 1. Figure 6 It can be seen that a large amount of black precipitate was precipitated in the microstructure, which was identified as NbC.
[0086] Based on the above results, it can be seen that the wear-resistant submerged arc welding flux-cored wire of the present invention has good welding process performance, the surface hardness of the weld layer is uniformly distributed, the average hardness is 650HV, and the wear resistance is 15 times that of the substrate.
[0087] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A welding wire powder core, characterized in that, The raw materials include the following ingredients in weight percentage: Iron chromium powder 25-46%, iron niobium powder 18-26.5%, nickel powder 0.5-1.5%, aluminum powder 0.5-2%, activator 1-5%, deoxidizer 3-10%, rare earth oxides 0.1-1%, iron powder 12.5-38%; The composition of the ferrochrome powder is: Cr 60.0%~80.0wt%, C≤10wt%, Si≤3wt%, with the balance being Fe; The composition of the niobium-iron powder is: Nb 50.0%~70.0wt%, C≤0.1wt%, Si≤3wt%, Al≤3wt%, with the balance being Fe; The active agent is one or both of BaF and CaF2; The deoxidizer is one or both of ferrosilicon and ferromanganese; The ferrosilicon composition is Si 60.0%~80.0wt%, C 0.01%~0.1wt%, with the balance being Fe; The composition of the ferromanganese is Mn 70~90wt%, Si 1~5wt%, C 0.1~1wt%, with the balance being Fe; The rare earth oxide is one or both of La2O3 and Ce2O3.
2. A wear-resistant submerged arc welding flux-cored wire, characterized in that, Includes a steel strip and a welding wire powder core wrapped in the steel strip; The welding wire powder core is the welding wire powder core as described in claim 1; The filling rate of the welding wire powder core in the steel strip is 30-50%.
3. The wear-resistant submerged arc welding flux-cored wire according to claim 2, characterized in that, The steel strip is made of H08A steel.
4. The method for preparing the wear-resistant submerged arc welding flux-cored wire according to claim 2 or 3, characterized in that, Includes the following steps: The raw materials for preparing welding wire powder core are mixed to obtain a dry mixture of welding wire powder core; The steel strip is rolled into a U-shape to obtain a U-shaped steel strip; The dry mixture of welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing welding wire powder core is rolled into an O-shape and then drawn to obtain wear-resistant submerged arc welding flux-cored wire.
5. The application of the wear-resistant submerged arc welding flux-cored wire as described in claim 2 or 3 in hot-rolled steel materials.
Citation Information
Patent Citations
Niobium enhanced wear-resisting submerged arc bead weld flux-cored wire
CN101856776A