Zirconia ceramic material and preparation method and application thereof
By adjusting the composition and preparation process of zirconia ceramic materials, introducing cerium oxide and controlling grain size, the problem of insufficient anti-aging ability of zirconia ceramics in high humidity environments was solved, and zirconia ceramic materials with high density and high strength were realized.
Patent Information
- Application Number
- CN202410858691.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing zirconia ceramic materials have poor anti-aging ability in high humidity environments, insufficient density, toughness and strength, and are prone to agglomeration during powder preparation, resulting in poor performance.
Zirconia ceramic materials are composed of zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide in a specific mass ratio. Through hydrothermal reaction and sintering processes, the grain size and distribution are controlled, cerium oxide is introduced to prevent water molecule diffusion, and dispersants and binders are used to improve density and strength.
This improved the aging resistance, density, and toughness of zirconia ceramic materials, enhanced their bending strength, and prevented grain growth at high temperatures, thus achieving high-density and high-strength zirconia ceramics.
Smart Images

Figure CN118771882B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic materials technology, specifically to a zirconia ceramic material, its preparation method, and its application. Background Technology
[0002] Zirconia ceramics, as phase transformation toughened ceramic materials, utilize the phase transformation of zirconia to achieve high fracture toughness and high flexural strength. Zirconia has three crystal structures: monoclinic, tetragonal, and cubic, which are stably present in the low-temperature, medium-temperature, and high-temperature regions, respectively. For pure zirconia ceramics, reversible transformations of these three crystal forms occur during firing; however, during cooling, zirconia undergoes volume expansion, leading to cracking. Pure zirconia ceramics obtained at room temperature and pressure have no practical value.
[0003] In related technologies, yttrium oxide is used as a stabilizer for zirconia ceramics, resulting in tetragonal zirconia ceramics with good mechanical properties. However, yttrium-stabilized zirconia ceramics have poor resistance to hydrothermal aging and cannot be used in high-humidity environments for extended periods. Furthermore, the preparation of zirconia powder often employs a co-precipitation method, which leads to severe powder agglomeration, resulting in poor density, toughness, and strength of the ceramic material.
[0004] Therefore, how to adjust and optimize zirconia ceramic materials to improve their anti-aging ability, density, toughness and strength is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] In view of this, the present invention provides a zirconia ceramic material with high anti-aging ability, high density, high toughness and high strength.
[0006] In a first aspect, the present invention provides a zirconia ceramic material, the zirconia ceramic material comprising: zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide; wherein the mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide is (90-92):(2-4):(4-8):(0.1-0.5):(0.4-0.7).
[0007] Secondly, the present invention provides a method for preparing the above-mentioned zirconia ceramic material, comprising the following steps:
[0008] (1) Dissolve zirconium salt, yttrium salt, cerium salt, aluminum salt and magnesium salt to obtain a mixed solution;
[0009] (2) Add a precipitant to the mixed solution to adjust the pH, let it stand, wash and filter to obtain a precursor mixture;
[0010] (3) The precursor mixture is subjected to a hydrothermal reaction and dried to obtain a powder;
[0011] (4) The powder is granulated, pressed and sintered to obtain the zirconium oxide ceramic material.
[0012] In one alternative embodiment, the zirconium salt includes at least one of zirconium oxychloride, zirconium nitrate, and zirconium sulfate.
[0013] In one alternative embodiment, the yttrium salt includes at least one of yttrium nitrate and yttrium chloride.
[0014] In one alternative embodiment, the cerium salt includes at least one of cerium nitrate and cerium chloride.
[0015] In one alternative embodiment, the aluminum salt includes at least one of aluminum nitrate, aluminum chloride, and aluminum sulfate.
[0016] In one alternative embodiment, the magnesium salt includes at least one of magnesium chloride, magnesium nitrate, and magnesium sulfate.
[0017] In one alternative embodiment, the zirconium salt comprises zirconium oxychloride hydrate.
[0018] In one alternative embodiment, the yttrium salt comprises yttrium nitrate hydrate.
[0019] In one alternative embodiment, the cerium salt comprises cerium nitrate hydrate.
[0020] In one alternative embodiment, the aluminum salt comprises aluminum nitrate hydrate.
[0021] In one alternative embodiment, the magnesium salt comprises magnesium chloride hydrate.
[0022] In one optional embodiment, the molar concentration of the zirconium salt in the mixed solution is 0.2 mol / L to 0.5 mol / L.
[0023] In one optional embodiment, the molar concentration of the yttrium salt in the mixed solution is 0.005 mol / L to 0.1 mol / L.
[0024] In one optional embodiment, the molar concentration of the cerium salt in the mixed solution is 0.009 mol / L to 0.1 mol / L.
[0025] In one optional embodiment, the molar concentration of the aluminum salt in the mixed solution is 0.001 mol / L to 0.1 mol / L.
[0026] In one optional embodiment, the molar concentration of the magnesium salt in the mixed solution is 0.004 mol / L to 0.1 mol / L.
[0027] In one alternative embodiment, the solvent of the mixed solution includes deionized water.
[0028] In one optional embodiment, the hydrothermal reaction includes: first heating to 80℃-85℃ and holding at that temperature for 12h-24h, then heating to 180℃-220℃ and holding at that temperature for 8h-24h.
[0029] In an alternative embodiment, in step (2), the addition of the precipitant to the mixed solution is carried out under oscillating conditions.
[0030] In one optional implementation, in step (2), the drying temperature is room temperature and the drying time is 22h-26h.
[0031] In one optional embodiment, the sintering temperature is 1450℃-1550℃, the sintering time is 3h-6h, and the sintering atmosphere is air.
[0032] In an optional implementation, step (3) further includes adding a first dispersant and / or solvent.
[0033] In one alternative embodiment, the first dispersant includes at least one of polyethylene glycol, polyvinyl alcohol, polyvinylpyrrolidone, and polyacrylic acid.
[0034] In one alternative embodiment, the solvent includes at least one of deionized water and anhydrous ethanol.
[0035] In one alternative embodiment, the mass ratio of the precursor mixture to the first dispersant is 1:0.02-0.05.
[0036] In one optional embodiment, the mass ratio of the precursor mixture to the volume ratio of the solvent is 1:8-30, with a ratio of g / mL.
[0037] In one optional embodiment, the precipitant includes at least one selected from ammonia, sodium hydroxide solution, urea solution, and sodium carbonate solution.
[0038] In one optional embodiment, the ammonia solution has a mass fraction of 5 wt% to 25 wt%.
[0039] In one optional embodiment, the sodium hydroxide solution has a mass fraction of 3wt%-7wt%.
[0040] In one optional embodiment, the urea solution has a mass fraction of 45wt%-55wt%.
[0041] In one optional embodiment, the sodium carbonate solution has a mass fraction of 15wt%-25wt%.
[0042] In one alternative implementation, the pH is 8-12.
[0043] In one alternative implementation, the settling time is 4-8 hours.
[0044] In one alternative embodiment, the washing and filtration step continues until Cl in the filtrate is removed. - .
[0045] In one optional embodiment, the granulation step further includes a step of mixing the powder, binder solution, second dispersant, and deionized water.
[0046] In one alternative embodiment, the adhesive comprises at least one of polyvinyl alcohol, polyvinylpyrrolidone, polyethylene glycol, and water-soluble phenolic resin.
[0047] In one alternative embodiment, the polyvinyl alcohol has a molecular weight of 1000-3000.
[0048] In one alternative embodiment, the molecular weight of the polyvinylpyrrolidone is 25k-35k.
[0049] In one alternative embodiment, the polyethylene glycol has a molecular weight of 3000-5000.
[0050] In one optional embodiment, the adhesive solution contains an adhesive with a mass fraction of 2 wt% to 20 wt%.
[0051] In one alternative embodiment, the second dispersant comprises at least one of polyacrylic acid, polyammonium methacrylate, and polyacrylamide.
[0052] In one alternative embodiment, the polyacrylic acid has a molecular weight of 2000-4000.
[0053] In one alternative embodiment, the polymethacrylate has a molecular weight of 1000-3000.
[0054] In one alternative embodiment, the polyacrylamide has a molecular weight of 1000-3000.
[0055] In one optional embodiment, the ratio of the powder, the binder solution, the second dispersant, and the deionized water is 100g:(10mL-100mL):(0.5g-3g):(100g-150g).
[0056] The third invention provides an application of the above-mentioned zirconia ceramic material in new energy and medical fields.
[0057] During strength testing, the ZrO2 of this invention expands by 5% in volume when it transforms from the tetragonal phase to the monoclinic phase. The resulting microcracks and residual stress can improve the toughness of the material.
[0058] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0059] 1. The zirconia ceramic material provided by this invention comprises: zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide; based on the metal oxide content, the mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide is (90-92):(2-4):(4-8):(0.1-0.5):(0.4-0.7). This invention introduces tetravalent cerium oxide into the zirconia ceramic material, simultaneously incorporating tetravalent zirconia. After doping, no oxygen vacancies are generated, and the diffusion channels of water molecules in the formed CeO2-Y2O3-ZrO2 system are blocked, effectively preventing aging and hydrolysis. Simultaneously, CeO2 and ZrO2 enter the ceramic material lattice through ion substitution, causing lattice distortion, increasing lattice defects, and reducing diffusion activation energy, thereby promoting ion diffusion and lowering the sintering temperature of the ceramic material. The Al2O3 of this invention generates second-phase particles, which is beneficial for controlling the growth of ZrO2 grains at high temperatures, stabilizing the tetragonal ZrO2 at room temperature, promoting densification, refining grains, and improving the bending strength, density, and fracture toughness of the material.
[0060] 2. The preparation method of zirconia ceramic material provided by the present invention includes a hydrothermal reaction comprising first heating to 80℃-85℃ and holding for 12h-24h, then heating to 180℃-220℃ and holding for 8h-24h, controlling the nucleation rate of the grains to make the grains tend to be more uniform and refined. The zirconia ceramic material has small particle size, narrow particle size distribution, and good crystallization. It does not require high-temperature calcination and ball milling steps, which is beneficial to improving the density of the ceramic and effectively improving the density and toughness of the zirconia ceramic material. Attached Figure Description
[0061] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0062] Figure 1 This is a schematic flowchart of the method for preparing zirconia ceramic materials according to an embodiment of the present invention;
[0063] Figure 2 This is the XRD pattern of the zirconia ceramic material prepared in Example 1 of the present invention. Detailed Implementation
[0064] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0065] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0066] The present invention will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed by the present invention.
[0067] The polyethylene glycol used in this invention was purchased from Jinan Xinshengguan Trading Co., Ltd., with a molecular weight of 4000; polyvinyl alcohol was purchased from Shanghai Xinheng New Material Technology Co., Ltd., with a molecular weight of 2000; polyvinylpyrrolidone was purchased from Shanghai Xinheng New Material Technology Co., Ltd., with a molecular weight of 30k; polyacrylic acid was purchased from Kemic Biopharmaceutical, with a molecular weight of 3000; water-soluble phenolic resin was purchased from Henan Jieyang New Material Co., Ltd., model JY water-soluble resin; polymethyl methacrylate was purchased from German Sima Chemical, with a molecular weight of 2000; and polyacrylamide was purchased from Shandong Chengda Chemical, with a molecular weight of 2000.
[0068] Example 1
[0069] like Figure 1 As shown, this embodiment provides a method for preparing zirconia ceramic material, including the following steps:
[0070] (1) Weigh 10.2g Y(NO3)3·6H2O, 12.6g Ce(NO3)3·6H2O, 238g ZrOCl2·8H2O, 1.5g Al(NO3)3·9H2O and 2.5g MgCl2·6H2O and dissolve them in 3L of deionized water to obtain a mixed solution;
[0071] (2) Under shaking conditions, 12 wt% ammonia solution was added dropwise to the above mixed solution to adjust the pH to 12. The mixture was allowed to stand for 8 hours, then filtered. The filter cake was washed successively with deionized water and anhydrous ethanol until the washing solution could not be detected with 0.1 mol / L AgNO3 solution. - The presence of [something] yields a precursor mixture;
[0072] (3) 100g of precursor mixture, 800mL of deionized water and 2g of polyethylene glycol are ultrasonically dispersed and mixed, placed in a reaction vessel, sealed and heated to 85℃, kept at the temperature for 24h, then heated to 200℃, kept at the temperature for 24h, washed with anhydrous ethanol, separated solid and liquid, dried at room temperature for 24h, and ground to obtain powder.
[0073] (4) Mix 100g of powder, 100mL of 2.5wt% polyvinyl alcohol solution, 2.5g of polyacrylic acid and 150g of deionized water evenly, then spray granulate and press, and sinter at 1520℃ for 3h in air atmosphere to obtain zirconia ceramic material. The mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide and magnesium oxide in the zirconia ceramic material is 91.01:3.01:4.99:0.20:0.49.
[0074] Example 2
[0075] like Figure 1 As shown, this embodiment provides a method for preparing zirconia ceramic material, including the following steps:
[0076] (1) Dissolve 6.8g Y(NO3)3·6H2O, 15.1g Ce(NO3)3·6H2O, 238g ZrOCl2·8H2O, 1.47g Al(NO3)3·9H2O and 3.5g MgCl2·6H2O in 2L of deionized water to obtain a mixed solution;
[0077] (2) Under shaking conditions, a 5 wt% sodium hydroxide aqueous solution was added dropwise to the above mixed solution to adjust the pH to 8. After standing for 8 hours, the mixture was filtered. The filter cake was washed with deionized water and anhydrous ethanol in sequence until the washing solution could not detect Cl- in 0.1 mol / L AgNO3 solution. - The presence of [something] yields a precursor mixture;
[0078] (3) 100g of precursor mixture and 800mL of anhydrous ethanol were ultrasonically dispersed and mixed, placed in a reaction vessel, sealed and heated to 85℃, kept at the temperature for 24h, and then heated to 200℃ and kept at the temperature for 24h. After washing with anhydrous ethanol, the solid and liquid were separated, dried at room temperature for 24h, and ground to obtain powder.
[0079] (4) Mix 100g of powder, 100mL of 2.5wt% polyvinylpyrrolidone, 2.5g of polyacrylamide and 135g of deionized water, then spray granulate and press, and sinter at 1450℃ for 5h in air atmosphere to obtain zirconia ceramic material. The mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide and magnesium oxide in the zirconia ceramic material is 91.01:2.00:5.99:0.20:0.69.
[0080] Example 3
[0081] like Figure 1 As shown, this embodiment provides a method for preparing zirconia ceramic material, including the following steps:
[0082] (1) Weigh 6.8g Y(NO3)3·6H2O, 12.36g CeCl3·6H2O, 262.5g Zr(SO4)2·4H2O, 1.5g Al(NO3)3·9H2O and 2g MgSO4 and dissolve them in 3L of deionized water to obtain a mixed solution;
[0083] (2) Under shaking conditions, 50 wt% urea aqueous solution was added dropwise to the above mixed solution to adjust the pH to 10. After standing for 6 hours, the mixture was filtered. The filter cake was washed with deionized water and anhydrous ethanol in sequence until the washing solution could not detect Cl in 0.1 mol / L AgNO3 solution. - The presence of [something] yields a precursor mixture;
[0084] (3) Mix 100g of precursor mixture, 800mL of deionized water and 5g of polyvinyl alcohol, put them into a reaction vessel, seal and heat to 80℃, keep warm for 12h, then heat to 200℃ and keep warm for 8h, wash with anhydrous ethanol, separate solid and liquid, dry at room temperature for 48h, and grind to obtain powder.
[0085] (4) Mix 100g powder, 100mL 2wt% polyethylene glycol, 2g polymethyl methacrylate and 110g deionized water and spray granulation and pressing. Sinter at 1500℃ for 4h in air atmosphere to obtain zirconia ceramic material. The mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide and magnesium oxide in zirconia ceramic material is 91.01:2.00:7.01:0.20:0.66.
[0086] Example 4
[0087] like Figure 1 As shown, this embodiment provides a method for preparing zirconia ceramic material, including the following steps:
[0088] (1) Weigh 8g YCl3·6H2O, 12.6g Ce(NO3)3·6H2O, 250g Zr(NO3)4, 2.9g Al(NO3)3·9H2O and 1.8g Mg(NO3)2 and dissolve them in 2.5L of deionized water to obtain a mixed solution;
[0089] (2) Under shaking conditions, 20 wt% sodium carbonate solution was added dropwise to the above mixed solution to adjust the pH to 10. After standing for 4 hours, the mixture was filtered. The filter cake was washed with deionized water and anhydrous ethanol in sequence until the washing solution could not detect Cl- in 0.1 mol / L AgNO3 solution.- The presence of [something] yields a precursor mixture;
[0090] (3) 100g of precursor mixture, 800mL of deionized water and 5g of polyvinylpyrrolidone were ultrasonically dispersed and mixed, placed in a reaction vessel, sealed and heated to 85℃, kept at the temperature for 12h, then heated to 200℃ and kept at the temperature for 12h, washed with anhydrous ethanol, separated solid and liquid, dried at room temperature for 24h, and ground to obtain powder.
[0091] (4) Mix 100g of powder, 10mL of 20wt% water-soluble phenolic resin solution, 3g of polyacrylic acid and 100g of deionized water, and then spray granulate and press. Sinter at 1530℃ for 3h in air atmosphere to obtain zirconia ceramic material. The mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide and magnesium oxide in the zirconia ceramic material is 90.80:2.98:4.99:0.39:0.49.
[0092] Example 5
[0093] This embodiment provides a method for preparing zirconia ceramic material, which is basically the same as the steps in embodiment 1. The only difference is that in step (3), 100g of precursor mixture, 800mL of deionized water and 2g of polyethylene glycol are ultrasonically dispersed and mixed, placed in a reaction vessel, sealed and heated to 200℃, kept at the temperature for 48h, washed with anhydrous ethanol, and after solid-liquid separation, dried at room temperature for 24h, and ground to obtain powder.
[0094] Comparative Example 1
[0095] This comparative example provides a method for preparing zirconia ceramic material, which is basically the same as the steps in Example 1, except that Ce(NO3)3·6H2O is replaced with the same number of moles of ZrOCl2·8H2O.
[0096] Comparative Example 2
[0097] This comparative example provides a method for preparing zirconia ceramic material, which is basically the same as the steps in Example 1, except that Y(NO3)3·6H2O is replaced with the same number of moles of ZrOCl2·8H2O.
[0098] Comparative Example 3
[0099] This comparative example provides a method for preparing zirconia ceramic material, which is basically the same as the steps in Example 1, except that Al(NO3)3·9H2O is replaced with the same number of moles of ZrOCl2·8H2O.
[0100] Experimental Example
[0101] The zirconia ceramic materials prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to hydrothermal aging resistance tests, flexural strength tests according to GB / T 6569-86, density tests according to Archimedes' displacement method, and fracture toughness tests according to the indentation method. The results are shown in the table below. The specific operation steps for the hydrothermal aging resistance test are as follows: the zirconia ceramic materials prepared in the above examples are subjected to water vapor at 134°C for 30 hours in a high-pressure reactor. The monoclinic phase volume fraction in each example and comparative example is calculated according to XRD test, which represents the hydrothermal aging resistance.
[0102] Table 1. Performance test results of zirconia ceramic materials prepared in each embodiment and comparative example.
[0103]
[0104] As can be seen from the table above, the zirconia ceramic materials prepared in Examples 1-5 of this invention have good anti-aging properties, high density, high toughness, and high flexural strength; in Comparative Example 1, replacing Ce(NO3)3·6H2O with ZrOCl2·8H2O resulted in excess Zr in the zirconia. 4+ Unable to be Ce 4+ and Y 3+ The substitution of cerium oxide with ZrOCl2·8H2O leads to a significant decrease in the material's resistance to hydrothermal aging, and a reduction in the stabilizer content results in a decrease in the density and mechanical properties of the ceramic. In Comparative Example 2, replacing Y(NO3)3·6H2O with ZrOCl2·8H2O resulted in a decrease in hydrothermal aging resistance, flexural strength, density, and fracture toughness. This was mainly because the use of cerium oxide alone reduced the stabilizer content in the ceramic sample, making it impossible to stabilize all the zirconium oxide. In Comparative Example 3, replacing Al(NO3)3·9H2O with ZrOCl2·8H2O resulted in a decrease in aging resistance, density, toughness, and high flexural strength due to the lack of alumina in the ceramic material. This was because the addition of alumina would generate second-phase particles, which would help control the growth of zirconium oxide grains and improve the mechanical properties of zirconium oxide.
[0105] The ceramic material prepared in Example 1 was subjected to XRD testing, see [see details]. Figure 2 As shown, from Figure 2 It can be seen that the tetragonal zirconia crystal form in the ceramic material is significant, with almost no monoclinic phase, indicating that the zirconia ceramic material prepared by this invention is relatively stable.
[0106] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A zirconia ceramic material, characterized in that, The zirconia ceramic material comprises: zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide; the mass ratio of zirconia, yttrium oxide, cerium oxide, aluminum oxide, and magnesium oxide is (90-92):(2-4):(4-8):(0.1-0.5):(0.4-0.7). The method for preparing the zirconia ceramic material includes the following steps: (1) Dissolve zirconium salt, yttrium salt, cerium salt, aluminum salt, and magnesium salt to obtain a mixed solution; (2) Add a precipitant to the mixed solution to adjust the pH, let it stand, filter and wash to obtain a precursor mixture; (3) The precursor mixture is subjected to a hydrothermal reaction and dried to obtain a powder; (4) The powder is granulated, pressed, and sintered to obtain the zirconium oxide ceramic material; The hydrothermal reaction includes: first heating to 80℃-85℃ and holding for 12h-24h, then heating to 180℃-220℃ and holding for 8h-24h.
2. The zirconia ceramic material according to claim 1, characterized in that, The raw materials for the zirconia ceramic material include: zirconium salts, yttrium salts, cerium salts, aluminum salts, and magnesium salts; The zirconium salt includes at least one of zirconium oxychloride, zirconium nitrate, and zirconium sulfate; And / or, the yttrium salt includes at least one of yttrium nitrate and yttrium chloride; And / or, the cerium salt includes at least one of cerium nitrate and cerium chloride; And / or, the aluminum salt includes at least one of aluminum nitrate, aluminum chloride, and aluminum sulfate; And / or, the magnesium salt includes at least one of magnesium chloride, magnesium nitrate, and magnesium sulfate.
3. The zirconia ceramic material according to claim 1 or 2, characterized in that, The zirconium salt includes zirconium oxychloride hydrate; And / or, the yttrium salt includes yttrium nitrate hydrate; And / or, the cerium salt includes cerium nitrate hydrate; And / or, the aluminum salt includes aluminum nitrate hydrate; And / or, the magnesium salt includes magnesium chloride hydrate.
4. The zirconia ceramic material according to claim 1, characterized in that, In the mixed solution, the molar concentration of the zirconium salt is 0.2 mol / L to 0.5 mol / L; And / or, the molar concentration of the yttrium salt is 0.005 mol / L to 0.1 mol / L; And / or, the molar concentration of the cerium salt is 0.009 mol / L to 0.1 mol / L; And / or, the molar concentration of the aluminum salt is 0.001 mol / L to 0.1 mol / L; And / or, the molar concentration of the magnesium salt is 0.004 mol / L to 0.1 mol / L.
5. The method for preparing zirconia ceramic material according to claim 1, characterized in that, The sintering temperature is 1450℃-1550℃, the sintering time is 3h-6h, and the sintering atmosphere is air.
6. The zirconia ceramic material according to claim 1, characterized in that, Step (3) further includes adding a first dispersant and / or solvent; The first dispersant includes at least one of polyethylene glycol, polyvinyl alcohol, polyvinylpyrrolidone, and polyacrylic acid; And / or, the solvent includes at least one of deionized water and anhydrous ethanol; And / or, the mass ratio of the precursor mixture to the first dispersant is 1:0.02-0.05; And / or, the ratio of the precursor mixture to the solvent is 1 g : (8 mL - 30 mL).
7. The zirconia ceramic material according to claim 1, characterized in that, The precipitant includes at least one of ammonia water, sodium hydroxide solution, urea solution, and sodium carbonate solution; And / or, the pH is 8-12; And / or, the settling time is 4h-8h; And / or, in the filtration and washing step, until chloride ions are removed from the filtrate.
8. The zirconia ceramic material according to claim 1, characterized in that, The granulation step also includes the step of mixing the powder, binder solution, second dispersant and deionized water; The adhesive includes at least one of polyvinyl alcohol, polyvinylpyrrolidone, polyethylene glycol, and water-soluble phenolic resin; And / or, in the adhesive solution, the mass fraction of the adhesive is 2wt%-20wt%; And / or, the second dispersant comprises at least one of polyacrylic acid, polyammonium methacrylate, and polyacrylamide; And / or, the ratio of the powder, the binder solution, the second dispersant and the deionized water is 100g:(10mL-100mL):(0.5g-3g):(100g-150g).
9. The application of the zirconia ceramic material according to any one of claims 1-8 in new energy and medical fields.
Citation Information
Patent Citations
Yttria-stabilized zirconia powder and preparation method thereof
CN103708831A