Preparation method and application of ceramic tile hollowing binder
By using materials such as modified silane and modified phenolic resin in the ceramic tile hollowing adhesive, a highly adhesive and water-resistant adhesive is formed, which solves the problem of hollowing in the construction of ceramic tiles and floor tiles and significantly reduces the cost of wall tiles. Risk of falling off, improved bonding strength and waterproof performance.
Patent Information
- Application Number
- CN202411019689.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a preparation method and application of a tile hollowing adhesive. Background Art
[0002] Since ceramic tiles began to be widely used, especially in recent years, the trend of installing floor tiles on the wall to pursue the integration of wall and floor decoration has become popular. The problem of ceramic tiles being hollow is particularly common. Installing floor tiles on the wall is just for aesthetics and for the integration of wall and floor in the decoration system, but it is not a good choice. From the perspective of the material of the floor tiles themselves, the floor tiles do not have good water absorption, so the risk of hollowing will increase during the construction of floor tiles on the wall. The larger the tile, the greater the risk of hollowing. In essence, hollowing is an inevitable phenomenon caused by the gradual dehydration of cement or operational errors. This problem is an inevitable probability. After the ceramic tiles are hollow, there is a great risk of wall tiles and floor tiles falling off. In particular, once the wall tiles fall off, injuries caused by smashing are common. Therefore, how to avoid this phenomenon is the key to solving the problem. Summary of the invention
[0003] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a preparation method and application of a tile hollowing adhesive, which has good water resistance and adhesion.
[0004] (II) Technical solution To achieve the above object, the present invention provides the following technical solution: a method for preparing a ceramic tile hollowing adhesive, the method for preparing the ceramic tile hollowing adhesive comprising the following steps: (1) Add allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stir to dissolve, continue to add monoplatinum catalyst, heat to 80-95°C for activation for 0.6-1h, then continue to heat to 100-120°C, add heptamethyl trisiloxane dropwise at constant pressure, react at 110-115°C for 4-8h after the addition, and remove low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane; (2) Add 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst to N,N-dimethylformamide solvent in an ice water bath, react at 20-26°C for 4-8 hours, and then perform vacuum distillation, wash with petroleum ether, and dry to obtain intermediate 1; (3) Add 5-9 parts by weight of intermediate 1 and 6-12 parts by weight of tin dichloride to an ethanol solvent, stir and mix, continue to add 1-3 parts by weight of a 25-30% dilute hydrochloric acid solution, react at 80-95° C. for 6-10 hours, add 1.2-2 parts by weight of a sodium carbonate aqueous solution after cooling to control the pH of the reaction solution to 7-7.8, remove the solvent by vacuum distillation, then add ethyl acetate for extraction and separation, collect the upper ethyl acetate solution, vacuum distill, wash with petroleum ether, and dry to obtain intermediate 2; (4) adding perfluorooctanoyl chloride to tetrahydrofuran solvent to dissolve it, then continuously adding intermediate 2 and triethylamine catalyst dropwise thereto, stirring and reacting at 30-36° C. for 3-7 hours, and after the reaction, removing the solvent by rotary evaporation, washing and drying to obtain modified silane; (5) Add 5-10 parts by weight of modified silane, 4-8 parts by weight of modified phenolic resin, 15-25 parts by weight of epoxy resin, 2-4 parts by weight of powder, 1-3 parts by weight of phenyl glycidyl ether diluent, 0.8-1.5 parts by weight of DMP-30 accelerator, 2-3 parts by weight of polymethylphenylsiloxane leveling agent, 1-2 parts by weight of phenolic amine epoxy curing agent, and 3-5 parts by weight of silane coupling agent into a high-speed mixer and blend them. Blend them at 60-75°C for 20-30 minutes to obtain a tile hollowing adhesive.
[0005] Preferably, the mass ratio of allyloxy polyoxyethylene ether, monoplatinum catalyst and heptamethyl trisiloxane in (1) is 1:0.01-0.03:1.1-1.3.
[0006] Preferably, the mass ratio of 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst in (2) is 1.2-1.5:1:0.03-0.04.
[0007] Preferably, the mass ratio of perfluorooctanoyl chloride, intermediate 2, and triethylamine catalyst in (4) is 1.4-1.6:1:0.03-0.05.
[0008] Preferably, the powder in (5) is any one of talcum powder, heavy calcium sulfate, light calcium sulfate, barium sulfate and titanium dioxide.
[0009] Preferably, the preparation method of the modified phenolic resin in (5) is: S1. Add 7-15 parts by weight of 4-aminophenol and 8-17 parts by weight of 4-vinylbenzaldehyde to N,N-dimethylformamide solvent, stir evenly, reflux at 70-95°C for 7-12h, cool to room temperature, add 5-12 parts by weight of sodium borohydride and 12-20 parts by weight of ethanol, react for 6-10h, and after completion, remove the solvent by distillation under reduced pressure, wash with petroleum ether, and recrystallize from ethanol to obtain olefinated phenol; S2. 3-4 parts by weight of sodium dodecyl sulfate emulsifier and 12-16 parts by weight of vinyl carbon nanotubes are added to deionized water, and after uniform dispersion, 10-15 parts by weight of olefinic phenol is added, nitrogen is introduced, and then 1-3 parts by weight of azobisisobutyronitrile initiator is added, and the reaction is carried out at 75-100 ° C for 2-5h, and then washed with deionized water and ethanol, and dried to obtain carbon nanotube-modified phenol; S3. Add 15-25 parts by weight of carbon nanotube-modified phenol, 80-110 parts by weight of phenol, and 40-70 parts by weight of a 38-40% formaldehyde aqueous solution into a reactor, mix well, continue to add 1-2 parts by weight of sodium hydroxide, react at 85-95°C for 2-6h, remove water by reduced pressure distillation, wash with petroleum ether, and dry to obtain a modified phenolic resin.
[0010] Preferably, the invention is used in repairing hollow tiles, hollow plaster layers, hollow foundations and various concrete cavities.
[0011] 3. Beneficial technical effects The invention provides a ceramic tile hollowing adhesive by adding modified silane, modified phenolic resin, epoxy resin, powder, phenyl glycidyl ether diluent, DMP-30 accelerator, polymethylphenylsiloxane leveling agent, phenolic amine epoxy curing agent and silane coupling agent into a high-speed mixer for blending.
[0012] The siloxane in the modified silane has good adhesion, and the (Si-O-Si) therein has good hydrophobicity and stability, which can resist the penetration of water and have a good waterproof effect; after the perfluorooctanoyl chloride reacts with the intermediate 1, its degree of substitution is increased, and the amide bonds and a large number of fluorine atoms in the modified silane will form hydrogen bonds, making it more tightly cross-linked and filling the gaps between tiles and walls, reducing the occurrence of hollowing; the carbon nanotubes in the modified phenolic resin have good mechanical properties, which can improve the tensile adhesion of the adhesive, and will entangle with the modified silane and epoxy resin to form an inorganic-organic hybrid polymer, making them denser and reducing the occurrence of tile hollowing. At the same time, the phenolic resin itself also has good adhesion and water resistance. DETAILED DESCRIPTION
[0013] The preparation process of vinyl carbon nanotubes refers to the journal "Materials Science and Engineering Plastics", Volume 23, Issue 4, "Surface Vinyl Functionalization of Multi-walled Carbon Nanotubes": 0.3g of multi-walled carbon nanotubes were added to 30mL of 98% concentrated sulfuric acid and 10mL of 70% concentrated nitric acid, refluxed at 140°C for 1h, filtered, and washed. 0.1g of the acidified carbon nanotubes obtained were weighed and dispersed in 15mL of acetone and 15mL of chloroform, 2mL of triethylamine and 5mL of acryloyl chloride were added, and the reaction was carried out at 40°C for 24h. Then 10mL of ethanol was added and stirred for 2h, filtered, and washed to obtain vinyl carbon nanotubes.
[0014] Example 1 (1) Add allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stir to dissolve, continue to add monoplatinum catalyst, heat to 80°C for activation for 0.6h, then continue to heat to 100°C, and add heptamethyl trisiloxane dropwise at constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, monoplatinum catalyst and heptamethyl trisiloxane is 1:0.01:1.1, react at 110°C for 4h after the addition, and remove low boiling points by reduced pressure distillation to obtain polyether modified trisiloxane; (2) adding 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst to N,N-dimethylformamide solvent in an ice water bath, wherein the mass ratio of 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst is 1.2:1:0.03, reacting at 20°C for 4 hours, and then distilling under reduced pressure, washing with petroleum ether and drying to obtain intermediate 1; (3) 5 parts by weight of intermediate 1 and 6 parts by weight of tin dichloride were added to an ethanol solvent, stirred and mixed, and 1 part by weight of a 25% dilute hydrochloric acid solution was added, and the mixture was reacted at 80° C. for 6 h. After cooling, 1.2 parts by weight of an aqueous sodium carbonate solution was added to control the pH of the reaction solution to 7, and the solvent was removed by vacuum distillation. Ethyl acetate was then added for extraction and separation, and the upper ethyl acetate solution was collected and vacuum distilled, washed with petroleum ether, and dried to obtain intermediate 2; (4) adding perfluorooctanoyl chloride to tetrahydrofuran solvent for dissolution, and then continuously adding intermediate 2 and triethylamine catalyst dropwise thereto, wherein the mass ratio of perfluorooctanoyl chloride, intermediate 2, and triethylamine catalyst is 1.4:1:0.03, stirring and reacting at 30° C. for 3 h, and after the reaction, removing the solvent by rotary evaporation, washing and drying to obtain modified silane; (5) Add 7 parts by weight of 4-aminophenol and 8 parts by weight of 4-vinylbenzaldehyde to N,N-dimethylformamide solvent, stir evenly, reflux at 70°C for 7 hours, cool to room temperature, add 5 parts by weight of sodium borohydride and 12 parts by weight of ethanol, react for 6 hours, and then remove the solvent by distillation under reduced pressure, wash with petroleum ether, and recrystallize with ethanol to obtain olefinated phenol; (6) 3 parts by weight of sodium dodecyl sulfate emulsifier and 12 parts by weight of vinyl carbon nanotubes were added to deionized water, and after being evenly dispersed, 10 parts by weight of olefinated phenol were added, and nitrogen was introduced for protection. Then, 1 part by weight of azobisisobutyronitrile initiator was added, and the mixture was reacted at 75° C. for 2 h. The mixture was washed with deionized water and ethanol in turn, and dried to obtain carbon nanotube-modified phenol; (6) 15 parts by weight of carbon nanotube-modified phenol, 80 parts by weight of phenol, and 40 parts by weight of a 38% formaldehyde aqueous solution were added to a reactor and mixed evenly. 1 part by weight of sodium hydroxide was added thereto, and the mixture was reacted at 85° C. for 2 h. Water was removed by distillation under reduced pressure, and the mixture was washed with petroleum ether and dried to obtain a modified phenolic resin. (7) Add 5 parts by weight of modified silane, 4 parts by weight of modified phenolic resin, 15 parts by weight of epoxy resin, 2 parts by weight of heavy calcium, 1 part by weight of phenyl glycidyl ether diluent, 0.8 parts by weight of DMP-30 accelerator, 2 parts by weight of polymethylphenylsiloxane leveling agent, 1 part by weight of phenolic amine epoxy curing agent, and 3 parts by weight of silane coupling agent into a high-speed mixer and blend them. Blend them at 60° C. for 20 minutes to obtain a tile hollowing adhesive.
[0015] Example 2 (1) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, adding monoplatinum catalyst thereto, heating to 95°C for activation for 1 hour, then heating to 120°C, adding heptamethyl trisiloxane thereto dropwise at a constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, monoplatinum catalyst and heptamethyl trisiloxane is 1:0.03:1.3, reacting at 115°C for 8 hours after the addition, and removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane; (2) adding 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst to N,N-dimethylformamide solvent in an ice water bath, wherein the mass ratio of 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst is 1.5:1:0.04, reacting at 26°C for 8 hours, and then distilling under reduced pressure, washing with petroleum ether and drying to obtain intermediate 1; (3) 9 parts by weight of intermediate 1 and 12 parts by weight of tin dichloride were added to an ethanol solvent, stirred and mixed, and 3 parts by weight of a 30% dilute hydrochloric acid solution was added, and the mixture was reacted at 95° C. for 10 h. After cooling, 2 parts by weight of an aqueous sodium carbonate solution was added to control the pH of the reaction solution to 7.8, and the solvent was removed by vacuum distillation. Ethyl acetate was then added for extraction and separation, and the upper ethyl acetate solution was collected and vacuum distilled, washed with petroleum ether, and dried to obtain intermediate 2; (4) adding perfluorooctanoyl chloride to tetrahydrofuran solvent for dissolution, and then continuously adding intermediate 2 and triethylamine catalyst dropwise thereto, wherein the mass ratio of perfluorooctanoyl chloride, intermediate 2, and triethylamine catalyst is 1.6:1:0.05, stirring and reacting at 36° C. for 7 h, and after the reaction, removing the solvent by rotary evaporation, washing and drying to obtain modified silane; (5) Add 15 parts by weight of 4-aminophenol and 17 parts by weight of 4-vinylbenzaldehyde to N,N-dimethylformamide solvent, stir evenly, reflux at 95°C for 12 hours, cool to room temperature, add 12 parts by weight of sodium borohydride and 20 parts by weight of ethanol, react for 10 hours, and then remove the solvent by distillation under reduced pressure, wash with petroleum ether, and recrystallize with ethanol to obtain olefinated phenol; (6) 4 parts by weight of sodium dodecyl sulfate emulsifier and 16 parts by weight of vinyl carbon nanotubes were added to deionized water, and after being evenly dispersed, 15 parts by weight of olefinated phenol were added, and nitrogen was introduced for protection. Then, 3 parts by weight of azobisisobutyronitrile initiator were added, and the mixture was reacted at 100° C. for 5 h. The mixture was washed with deionized water and ethanol in turn, and dried to obtain carbon nanotube-modified phenol; (6) Add 25 parts by weight of carbon nanotube-modified phenol, 110 parts by weight of phenol, and 70 parts by weight of a 40% formaldehyde aqueous solution into a reactor, mix well, and continue to add 2 parts by weight of sodium hydroxide, react at 95° C. for 6 hours, remove water by reduced pressure distillation, wash with petroleum ether, and dry to obtain a modified phenolic resin; (7) Add 10 parts by weight of modified silane, 8 parts by weight of modified phenolic resin, 25 parts by weight of epoxy resin, 4 parts by weight of light calcium, 3 parts by weight of phenyl glycidyl ether diluent, 1.5 parts by weight of DMP-30 accelerator, 3 parts by weight of polymethylphenylsiloxane leveling agent, 2 parts by weight of phenolic amine epoxy curing agent, and 5 parts by weight of silane coupling agent into a high-speed mixer and blend them. Blend them at 75°C for 30 minutes to obtain a tile hollowing adhesive.
[0016] Example 3 (1) Add allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stir to dissolve, continue to add monoplatinum catalyst, heat to 87.5°C to activate for 0.8h, then continue to heat to 110°C, add heptamethyl trisiloxane dropwise at constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, monoplatinum catalyst and heptamethyl trisiloxane is 1:0.02:1.2, react at 112.5°C for 6h after the addition, and remove low boiling points by reduced pressure distillation to obtain polyether modified trisiloxane; (2) adding 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst to N,N-dimethylformamide solvent in an ice water bath, wherein the mass ratio of 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst is 1.35:1:0.035, reacting at 23° C. for 6 h, and then distilling under reduced pressure, washing with petroleum ether and drying to obtain intermediate 1; (3) 7 parts by weight of intermediate 1 and 9 parts by weight of tin dichloride were added to an ethanol solvent, stirred and mixed, and 2 parts by weight of a 27.5% dilute hydrochloric acid solution was added, and the mixture was reacted at 87.5° C. for 8 h. After cooling, 1.6 parts by weight of an aqueous sodium carbonate solution was added to control the pH of the reaction solution to 7.4, and the solvent was removed by vacuum distillation. Ethyl acetate was then added for extraction and separation, and the upper ethyl acetate solution was collected and vacuum distilled, washed with petroleum ether, and dried to obtain intermediate 2; (4) adding perfluorooctanoyl chloride to tetrahydrofuran solvent for dissolution, and then continuously adding intermediate 2 and triethylamine catalyst dropwise thereto, wherein the mass ratio of perfluorooctanoyl chloride, intermediate 2, and triethylamine catalyst is 1.5:1:0.04, stirring and reacting at 33° C. for 5 h, and after the reaction, removing the solvent by rotary evaporation, washing and drying to obtain modified silane; (5) Add 11 parts by weight of 4-aminophenol and 12.5 parts by weight of 4-vinylbenzaldehyde to N,N-dimethylformamide solvent, stir evenly, reflux at 82.5°C for 9.5 hours, cool to room temperature, add 8.5 parts by weight of sodium borohydride and 16 parts by weight of ethanol, react for 8 hours, and then remove the solvent by distillation under reduced pressure, wash with petroleum ether, and recrystallize with ethanol to obtain olefinated phenol; (6) 3.5 parts by weight of sodium dodecyl sulfate emulsifier and 14 parts by weight of vinyl carbon nanotubes were added to deionized water, and after being evenly dispersed, 12.5 parts by weight of olefinic phenol were added, and nitrogen was introduced for protection. Then, 2 parts by weight of azobisisobutyronitrile initiator were added, and the reaction was carried out at 87.5° C. for 3.5 hours. The mixture was washed with deionized water and ethanol in turn, and dried to obtain carbon nanotube-modified phenol; (6) Add 20 parts by weight of carbon nanotube-modified phenol, 95 parts by weight of phenol, and 55 parts by weight of a 39% formaldehyde aqueous solution into a reactor, mix them evenly, and continue to add 1.5 parts by weight of sodium hydroxide, react at 90° C. for 4 hours, remove water by reduced pressure distillation, wash with petroleum ether, and dry to obtain a modified phenolic resin; (7) Add 7.5 parts by weight of modified silane, 6 parts by weight of modified phenolic resin, 20 parts by weight of epoxy resin, 3 parts by weight of titanium dioxide, 2 parts by weight of phenyl glycidyl ether diluent, 1.15 parts by weight of DMP-30 accelerator, 2.5 parts by weight of polymethylphenylsiloxane leveling agent, 1.5 parts by weight of phenolic amine epoxy curing agent, and 4 parts by weight of silane coupling agent into a high-speed mixer and blend them. Blend them at 67.5° C. for 25 minutes to obtain a tile hollowing adhesive.
[0017] Comparative Example 1 (1) 6 parts by weight of modified phenolic resin, 20 parts by weight of epoxy resin, 3 parts by weight of titanium dioxide, 2 parts by weight of phenyl glycidyl ether diluent, 1.15 parts by weight of DMP-30 accelerator, 2.5 parts by weight of polymethylphenylsiloxane leveling agent, 1.5 parts by weight of phenolic amine epoxy curing agent, and 4 parts by weight of silane coupling agent were added into a high-speed mixer for blending, and blended at 67.5° C. for 25 minutes to obtain a tile hollowing adhesive.
[0018] Comparative Example 2 (1) 7.5 parts by weight of modified silane, 20 parts by weight of epoxy resin, 3 parts by weight of titanium dioxide, 2 parts by weight of phenyl glycidyl ether diluent, 1.15 parts by weight of DMP-30 accelerator, 2.5 parts by weight of polymethylphenylsiloxane leveling agent, 1.5 parts by weight of phenolic amine epoxy curing agent, and 4 parts by weight of silane coupling agent were added into a high-speed mixer and blended. The mixture was blended at 67.5° C. for 25 minutes to obtain a tile hollowing adhesive.
[0019] The above-mentioned tile hollow adhesive was applied to the back of the tile for bonding strength test. The bonding strength test method between tiles and concrete walls: the reverse production process is adopted. The tiles are first laid in the mold, and then the tile hollow adhesive is applied to the back of the tile. After the tile adhesive is dried for 24 hours, concrete is poured on the back of the tile for prefabrication of the wallboard. Finally, the mold is removed for maintenance. After the maintenance reaches the age, the sample is cut and tested. The tensile bonding strength test is carried out according to the test method of JC / T 547-2017 "Ceramic Tile Adhesive". The test results of various performances are shown in Table 1.
[0020] Table 1: Bond strength test.
[0021] project Tensile bond strength (MPa) Tensile bond strength after immersion in water (MPa) Tile and concrete wall status (30 days) Example 1 0.93 0.8 No warping, no hollowing Example 2 1.1 0.9 No warping, no hollowing Example 3 1.0 0.8 No warping, no hollowing Comparative Example 1 0.6 0.5 There are warping edges, no hollows Comparative Example 2 0.5 0.4 There are warping edges, no hollows It can be seen from Table 1 that compared with Comparative Example 1-2, Examples 1-3 of the present invention have better viscosity and no warping; Examples 1-3 and Comparative Example 1-2 have no hollowing.
[0022] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a tile hollowing adhesive, characterized in that: The preparation method of the tile hollowing adhesive comprises the following steps: (1) Add allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stir to dissolve, continue to add monoplatinum catalyst, heat to 80-95°C for activation for 0.6-1h, then continue to heat to 100-120°C, add heptamethyl trisiloxane dropwise at constant pressure, react at 110-115°C for 4-8h after the addition, and remove low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane; (2) Add 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst to N,N-dimethylformamide solvent in an ice water bath, react at 20-26°C for 4-8 hours, and then perform vacuum distillation, wash with petroleum ether, and dry to obtain intermediate 1; (3) Add 5-9 parts by weight of intermediate 1 and 6-12 parts by weight of tin dichloride to an ethanol solvent, stir and mix, continue to add 1-3 parts by weight of a 25-30% dilute hydrochloric acid solution, react at 80-95° C. for 6-10 hours, add 1.2-2 parts by weight of a sodium carbonate aqueous solution after cooling to control the pH of the reaction solution to 7-7.8, remove the solvent by vacuum distillation, then add ethyl acetate for extraction and separation, collect the upper ethyl acetate solution, vacuum distill, wash with petroleum ether, and dry to obtain intermediate 2; (4) adding perfluorooctanoyl chloride to tetrahydrofuran solvent to dissolve it, then continuously adding intermediate 2 and triethylamine catalyst dropwise thereto, stirring and reacting at 30-36° C. for 3-7 hours, and after the reaction, removing the solvent by rotary evaporation, washing and drying to obtain modified silane; (5) Add 5-10 parts by weight of modified silane, 4-8 parts by weight of modified phenolic resin, 15-25 parts by weight of epoxy resin, 2-4 parts by weight of powder, 1-3 parts by weight of phenyl glycidyl ether diluent, 0.8-1.5 parts by weight of DMP-30 accelerator, 2-3 parts by weight of polymethylphenylsiloxane leveling agent, 1-2 parts by weight of phenolic amine epoxy curing agent, and 3-5 parts by weight of silane coupling agent into a high-speed mixer and blend them. Blend them at 60-75°C for 20-30 minutes to obtain a tile hollowing adhesive.
2. The method for preparing a hollow tile adhesive according to claim 1, characterized in that: The mass ratio of allyloxy polyoxyethylene ether, monoplatinum catalyst and heptamethyl trisiloxane in (1) is 1:0.01-0.03:1.1-1.
3.
3. The method for preparing a hollow tile adhesive according to claim 1, characterized in that: The mass ratio of 3,5-dinitrobenzoyl chloride, polyether-modified trisiloxane and triethylamine catalyst in (2) is 1.2-1.5:1:0.03-0.
04.
4. The method for preparing a hollow tile adhesive according to claim 1, characterized in that: The mass ratio of perfluorooctanoyl chloride, intermediate 2 and triethylamine catalyst in (4) is 1.4-1.6:1:0.03-0.
05.
5. The method for preparing a hollow tile adhesive according to claim 1, characterized in that: The powder in (5) is any one of talcum powder, heavy calcium, light calcium, barium sulfate, and titanium dioxide.
6. The method for preparing a hollow tile adhesive according to claim 1, characterized in that: The preparation method of the modified phenolic resin in (5) is: S1. Add 7-15 parts by weight of 4-aminophenol and 8-17 parts by weight of 4-vinylbenzaldehyde to N,N-dimethylformamide solvent, stir evenly, reflux at 70-95°C for 7-12h, cool to room temperature, add 5-12 parts by weight of sodium borohydride and 12-20 parts by weight of ethanol, react for 6-10h, and after completion, remove the solvent by distillation under reduced pressure, wash with petroleum ether, and recrystallize from ethanol to obtain olefinated phenol; S2. 3-4 parts by weight of sodium dodecyl sulfate emulsifier and 12-16 parts by weight of vinyl carbon nanotubes are added to deionized water, and after uniform dispersion, 10-15 parts by weight of olefinic phenol is added, nitrogen is introduced, and then 1-3 parts by weight of azobisisobutyronitrile initiator is added, and the reaction is carried out at 75-100 ° C for 2-5h, and then washed with deionized water and ethanol, and dried to obtain carbon nanotube-modified phenol; S3. Add 15-25 parts by weight of carbon nanotube-modified phenol, 80-110 parts by weight of phenol, and 40-70 parts by weight of a 38-40% formaldehyde aqueous solution into a reactor, mix well, continue to add 1-2 parts by weight of sodium hydroxide, react at 85-95°C for 2-6h, remove water by reduced pressure distillation, wash with petroleum ether, and dry to obtain a modified phenolic resin.
7. A method for preparing a tile hollow adhesive according to any one of claims 1 to 6, characterized in that: The invention is applied in repairing hollow tiles, hollow plaster layers, hollow foundations and various concrete cavities.