Fluorescent gold-silver nanoclusters and preparation method and application thereof
Fluorescent gold and silver nanoclusters were synthesized in a one-pot process using dithiocarbamate as a ligand molecule and a protective agent. This solved the stability and cytotoxicity problems of existing near-infrared fluorescent materials in in vivo biological imaging, and achieved the preparation of nanoclusters with high quantum yield and good water solubility, which are suitable for in vivo biological imaging.
Patent Information
- Application Number
- CN202410742518.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing near-infrared fluorescent materials, such as organic dyes and semiconductor quantum dots, suffer from poor hydrophilicity, insufficient photostability, and high cytotoxicity in biological in vivo imaging, which limits their application. Furthermore, existing fluorescent metal nanoclusters cannot simultaneously possess near-infrared fluorescence, high quantum yield, and good stability.
Fluorescent gold-silver nanoclusters were synthesized in a one-pot method using dithiocarbamate as a ligand molecule and a protecting agent, combined with chloroauric acid and silver nitrate as metal sources. The preparation method is simple and reproducible, and the prepared nanoclusters have good stability, water solubility, near-infrared fluorescence and high quantum yield.
The fluorescent gold and silver nanoclusters exhibit excellent stability and water solubility, high quantum yield, and low cytotoxicity, making them suitable for large-scale industrial production and applicable to in vivo biological imaging.
Smart Images

Figure CN118772872B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nanomaterials technology, and in particular to a fluorescent gold-silver nanocluster, its preparation method, and its application. Background Technology
[0002] With the rapid development of nanotechnology, fluorescent nanomaterials, as emerging fluorescent materials, have attracted widespread attention and provided excellent opportunities for the design and development of nanobiosensors. Currently, the most widely studied fluorescent nanomaterials include carbon dots, graphene quantum dots, semiconductor quantum dots, and fluorescent metal nanoclusters. Among them, fluorescent metal nanoclusters possess unique optical properties, easy surface modification and functionalization, low biotoxicity, good light irradiation stability, good biocompatibility, and a large Stokes shift, making them promising for applications in small molecule sensing, biolabeling imaging, and biomedicine.
[0003] Meanwhile, biological tissues exhibit very low absorption and background fluorescence in the near-infrared spectral window (650-900 nm wavelength). Furthermore, near-infrared fluorescence can penetrate several centimeters of heterogeneous living tissue. Therefore, current technologies often employ nanoprobes such as near-infrared organic dyes and semiconductor quantum dots for in vivo biological imaging. However, organic dyes have poor hydrophilicity and photostability, and the semiconductor quantum dots currently reported to be used have high cytotoxicity and self-aggregation in living cells. This greatly limits the practical biological applications of near-infrared dyes and semiconductor quantum dots.
[0004] Therefore, combining near-infrared luminescence properties with fluorescent metal nanoclusters holds promise for applications in in vivo biological imaging. In particular, the use of near-infrared fluorescent metal nanoclusters can alleviate the limitations of traditional near-infrared organic dyes and semiconductor quantum quanta. However, currently reported fluorescent metal nanoclusters struggle to simultaneously possess the advantages of near-infrared fluorescence, high quantum yield, and good stability, which significantly restricts their application in in vivo imaging. Therefore, a solution is urgently needed to address this issue. Summary of the Invention
[0005] The purpose of this invention is to provide a fluorescent gold and silver nanocluster, its preparation method and application. The preparation method is simple to operate, has good stability and high reproducibility, which is conducive to the large-scale industrial production of fluorescent gold and silver nanoclusters. At the same time, the prepared fluorescent gold and silver nanoclusters have good stability, water solubility, near-infrared fluorescence and high quantum yield.
[0006] In the first aspect, the preparation method provided by the present invention uses dithiocarbamate as a ligand molecule and a protecting agent, and chloroauric acid and silver nitrate as metal sources. Fluorescent gold and silver nanoclusters are synthesized in a one-pot method under the action of a reducing agent. The preparation method is simple and reproducible, and the prepared fluorescent gold and silver nanoclusters have good stability, water solubility, near-infrared fluorescence, high quantum yield and low cytotoxicity.
[0007] Optionally, the preparation of the dithiocarbamate ligand includes the following steps: mixing barium hydroxide solution, carbamate solution and acetone to obtain a precursor solution; adding carbon disulfide dropwise to the precursor solution, stirring and reacting, centrifuging, washing and drying to obtain an intermediate precipitate; dissolving the intermediate precipitate in sodium carbonate solution and removing the precipitate to obtain a dithiocarbamate ligand solution.
[0008] Optionally, the solute in the carbamate solution includes at least one of 3-piperidinecarboxylic acid, DL-piperidinecarboxylic acid, isoperidinecarboxylic acid, 3-methylaminopropionic acid, proline, and hydroxyproline.
[0009] Optionally, the process of mixing barium hydroxide solution, carbamate solution and acetone includes: mixing barium hydroxide solution and carbamate solution at 0-6°C, and then adding acetone and mixing.
[0010] Optionally, after stirring and mixing the barium hydroxide solution and the carbamate solution, the molar mixing ratio of barium hydroxide to carbamate is 1:1.09.
[0011] Optionally, after stirring and mixing chloroauric acid solution, silver nitrate solution, and dithiocarbamate ligand solution, a reducing agent is added, and the mixture is stirred and reacted at 50-100℃ for 1-12 hours. After separation and purification, the mixture is dialyzed and then freeze-dried at -50℃ to obtain fluorescent gold and silver nanoclusters.
[0012] Optionally, during the mixing of chloroauric acid solution, silver nitrate solution, and dithiocarbamate ligand solution, the molar mixing ratio of chloroauric acid, silver nitrate, and dithiocarbamate ligand is 4:1:40.
[0013] Optionally, the reducing agent includes ascorbic acid.
[0014] Secondly, the present invention also provides a fluorescent gold-silver nanocluster prepared using any of the above-mentioned optional preparation methods.
[0015] Thirdly, the present invention also provides an application of fluorescent gold and silver nanoclusters prepared by any of the above-mentioned optional preparation methods in fluorescent probes.
[0016] Optionally, the fluorescent gold and silver nanoclusters may be used as fluorescent probes in in vivo biological imaging. Attached Figure Description
[0017] Figure 1 The 1H NMR spectrum and 1C NMR spectrum of the dithiocarbamate ligand prepared in Example 1 of this invention;
[0018] Figure 2 The three-dimensional fluorescence spectrum, ultraviolet absorption spectrum, and emission spectrum of the fluorescent gold-silver nanoclusters prepared in Example 1 of this invention are shown below.
[0019] Figure 3 The stability spectrum of the fluorescent gold-silver nanoclusters prepared in Example 1 of this invention;
[0020] Figure 4 The anti-interference spectrum of the fluorescent gold-silver nanoclusters prepared in Example 1 of this invention;
[0021] Figure 5 This is a cytotoxicity diagram of the fluorescent gold-silver nanoclusters prepared in Example 1 of this invention. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical or scientific terms used herein should have the ordinary meaning understood by those skilled in the art. The terms "comprising" and similar expressions used herein mean that the element or object preceding the word covers the element or object listed after the word and its equivalents, but does not exclude other elements or objects.
[0023] This invention provides a method for preparing fluorescent gold and silver nanoclusters, comprising synthesizing fluorescent gold and silver nanoclusters in a one-pot process using dithiocarbamate as a ligand molecule and a protecting agent, and chloroauric acid and silver nitrate as metal sources, under the action of a reducing agent. Specifically, the method for preparing fluorescent gold and silver nanoclusters includes the following steps:
[0024] S1. Under the presence of a reducing agent, chloroauric acid solution, silver nitrate solution and dithiocarbamate ligand solution are stirred and mixed to prepare the reaction solution;
[0025] S2. After reacting the reaction solution at 50-100℃ for 1-12 hours, the solution is separated, purified, and dialyzed. Fluorescent gold and silver nanoclusters are then obtained by freeze-drying at -50℃.
[0026] In some embodiments, the reducing agent used in performing step S1 includes at least one of ascorbic acid, sodium borohydride, sodium cyanoborohydride, and hydrazine hydrate.
[0027] In some embodiments, after performing step S1 by stirring and mixing the chloroauric acid solution, silver nitrate solution and dithiocarbamate ligand, the molar mixing ratio of chloroauric acid, silver nitrate and dithiocarbamate ligand is 4:1:40.
[0028] In fact, the preparation of the dithiocarbamate ligand solution used in step S1 includes the following steps:
[0029] D1. Prepare the precursor solution by mixing barium hydroxide solution, carbamate solution and acetone.
[0030] D2. Carbon disulfide was added dropwise to the precursor solution, stirred and reacted, then centrifuged, washed and dried to obtain an intermediate precipitate.
[0031] D3. Dissolve the intermediate precipitate in sodium carbonate solution and remove the precipitate to obtain a dithiocarbamate ligand solution.
[0032] In some embodiments, the solute in the carbamate solution used in step D1 includes at least one of 3-piperidinecarboxylic acid, DL-piperidinecarboxylic acid, isoperidinecarboxylic acid, 3-methylaminopropionic acid, proline, and hydroxyproline.
[0033] In some embodiments, after performing step D1 by stirring and mixing the barium hydroxide solution, the carbamate solution, and acetone, the molar mixing ratio of barium hydroxide to carbamate is 1:1.09.
[0034] In fact, during step D1, the barium hydroxide solution used is an aqueous solution of barium hydroxide, and the carbamate is an aqueous solution of carbamate. Specifically, a barium hydroxide solution can be prepared by stirring and dissolving barium hydroxide octahydrate in deionized water, and a carbamate solution can be prepared by stirring and dissolving the carbamate in deionized water.
[0035] In some embodiments, during step D1, barium hydroxide solution and carbamate solution are stirred and mixed at 0-6°C, and then acetone is added and stirred to obtain a precursor solution.
[0036] In some embodiments, during step D2, in which carbon disulfide is added dropwise to the precursor solution, the total time for adding carbon disulfide is controlled to be 14 min, and the mass ratio of the added carbon disulfide to the carbamate is 0.595:1.
[0037] In some embodiments, after performing step D2 and centrifuging, barium salt precipitate can be separated, and after repeatedly washing the centrifuged precipitate with acetone, reactants and impurities attached to the precipitate can be removed, and an intermediate precipitate can be obtained after vacuum drying.
[0038] In some embodiments, performing step D3 by dissolving the intermediate precipitate in a sodium carbonate solution can remove barium ions from the intermediate precipitate, thereby obtaining a dithiocarbamate ligand solution.
[0039] In practice, polyacrylamide gel electrophoresis can be used during the separation and purification process in step S2. Specifically, during the dialysis process in step S2, a MW1500D dialysis bag is used, and the dialysis time is controlled to be 10-15 days.
[0040] Preparation Example 1
[0041] Example 1 of this invention provides a method for preparing dithiocarbamate ligands, comprising the following steps:
[0042] D1. Weigh 0.7865 g of barium hydroxide hydrate and dissolve it in 4 mL of deionized water to prepare barium hydroxide solution; weigh 0.2964 g of 3-piperidinecarboxylic acid and dissolve it in 3 mL of deionized water to prepare 3-piperidinecarboxylic acid solution; at 6 °C, stir and mix the barium hydroxide solution, 3-piperidinecarboxylic acid and 18 mL of acetone to prepare precursor solution;
[0043] D2. 0.14 mL of carbon disulfide was added dropwise to the precursor solution. After stirring at 800 rpm for 2 h, the precipitate was separated by centrifugation at 12500 rpm. The precipitate was washed three times by centrifugation with acetone and then dried under vacuum to obtain the intermediate precipitate.
[0044] D3. Dissolve the intermediate precipitate in an aqueous sodium carbonate solution, stir and mix, then filter to remove the precipitate to obtain a dithiocarbamate ligand solution.
[0045] Exploration Example
[0046] This exploratory example provides a method for preparing fluorescent gold and silver nanoclusters, including the following steps:
[0047] S1. Mix 20-200 μL of chloroauric acid solution (20 mmol / L) and 10-140 μL of silver nitrate solution (10 mmol / L), then add 160-320 μL of dithiocarbamate ligand solution (100 mmol / L) and 50-300 μL of ascorbic acid solution (100 mmol / L), and add ultrapure water. Mix and bring the volume to 1000 μL to obtain the reaction solution.
[0048] S2. The reaction solution is heated in a water bath at 50-100℃ for 1-12 hours to obtain a mixed solution of fluorescent gold and silver nanoclusters. The mixed solution is separated and purified by polyacrylamide gel electrophoresis, and then dialyzed using a MW1500D dialysis bag for 10-15 days. The dialysis product is then freeze-dried under vacuum at -50℃ to obtain fluorescent gold and silver nanoclusters.
[0049] With increasing chloroauric acid solution volume, the fluorescence intensity and yield of fluorescent gold-silver nanoclusters gradually increased and then decreased, reaching an optimal volume of 120 μL; with increasing silver nitrate solution volume, the fluorescence intensity and yield of fluorescent gold-silver nanoclusters gradually increased and then gradually balanced, reaching an optimal volume of 60 μL; with increasing dithiocarbamate ligand volume, the fluorescence intensity and yield gradually increased and then decreased, with an optimal volume of 240 μL; with increasing ascorbic acid volume, the fluorescence intensity and yield gradually increased and then decreased, with an optimal volume of 150 μL; with increasing reaction temperature, the fluorescence intensity gradually increased and then gradually balanced, with an optimal reaction temperature of 80 °C; with increasing reaction time, the fluorescence intensity gradually increased and then decreased, with an optimal reaction time of 4 h.
[0050] Example 1
[0051] Based on the optimal parameters explored in the exploratory examples, this embodiment 1 provides a method for preparing fluorescent gold and silver nanoclusters, including the following steps:
[0052] S1. Mix 120 μL of chloroauric acid solution (20 mmol / L) and 60 μL of silver nitrate solution (10 mmol / L), then add 240 μL of dithiocarbamate ligand solution (100 mmol / L) and 150 μL of ascorbic acid solution (100 mmol / L), and add ultrapure water. Mix and bring the volume to 1000 μL to obtain the reaction solution.
[0053] S2. The reaction solution was heated in an 80°C water bath for 4 hours to obtain a mixed solution of fluorescent gold and silver nanoclusters. The mixed solution was separated and purified by polyacrylamide gel electrophoresis, and then dialyzed for 13 days using a MW1500D dialysis bag. The dialysis product was freeze-dried at -50°C to obtain fluorescent gold and silver nanoclusters.
[0054] Performance testing
[0055] The dithiocarbamate ligands prepared in Preparation Example 1 were characterized by 1H NMR and 1C NMR, respectively, as follows: Figure 1 (A) and Figure 1 As shown in (B);
[0056] The fluorescent gold-silver nanoclusters prepared in Example 1 were characterized by three-dimensional excitation-emission matrix spectroscopy as follows: Figure 2 As shown in (A), the ultraviolet-visible light and absorption spectroscopy characterization was performed as follows: Figure 2 As shown in (B);
[0057] The stability of the fluorescent gold-silver nanoclusters (10 mM PBS buffered, pH 7.4) prepared in Example 1 was investigated as follows: Figure 3 As shown, the anti-interference test was conducted as follows: Figure 4 As shown; the cytotoxicity of the fluorescent gold-silver nanoclusters prepared in Example 1 was investigated as follows. Figure 5 As shown.
[0058] While embodiments of the present invention have been described in detail above, it will be apparent to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations fall within the scope and spirit of the invention as set forth in the claims. Furthermore, the invention described herein may have other embodiments and can be implemented or carried out in various ways.
Claims
1. A method for preparing fluorescent gold and silver nanoclusters, characterized in that, Fluorescent gold and silver nanoclusters were synthesized in a one-pot process using dithiocarbamate as a ligand molecule and a protecting agent, and chloroauric acid and silver nitrate as metal sources, under the action of a reducing agent. The preparation of the dithiocarbamate ligand includes the following steps: The precursor solution was prepared by mixing barium hydroxide solution, carbamate solution and acetone. Carbon disulfide was added dropwise to the precursor solution, stirred and reacted, then centrifuged, washed and dried to obtain an intermediate precipitate. The intermediate precipitate was dissolved in sodium carbonate solution and the precipitate was removed to prepare a dithiocarbamate ligand solution. The solute in the carbamic acid solution is selected from one of 3-piperidinecarboxylic acid, DL-piperidinecarboxylic acid, and isoperidinecarboxylic acid. The reducing agent is selected from ascorbic acid.
2. The preparation method according to claim 1, characterized in that, The process of mixing barium hydroxide solution, carbamate solution and acetone includes: mixing barium hydroxide solution and carbamate solution at 0-6℃, and then adding acetone and mixing; wherein, after mixing barium hydroxide solution and carbamate solution, the molar mixing ratio of barium hydroxide solution and carbamate solution is 1:1.
09.
3. The preparation method according to any one of claims 1 to 2, characterized in that, After mixing chloroauric acid solution, silver nitrate solution, and dithiocarbamate ligand solution, a reducing agent was added, and the mixture was stirred at 50-100℃ for 1-12 hours. After separation and purification, the mixture was dialyzed and then freeze-dried at -50℃ to obtain fluorescent gold and silver nanoclusters.
4. The preparation method according to claim 3, characterized in that, During the mixing of chloroauric acid solution, silver nitrate solution, and dithiocarbamate ligand solution, the molar mixing ratio of chloroauric acid, silver nitrate, and dithiocarbamate ligand is 4:1:
40.
5. A fluorescent gold-silver nanocluster prepared by the preparation method according to any one of claims 1 to 4.
6. An application of fluorescent gold-silver nanoclusters prepared by the preparation method according to any one of claims 1 to 4 in a fluorescent probe, characterized in that, The fluorescent gold and silver nanoclusters are used as fluorescent probes in in vivo biological imaging.
Citation Information
Patent Citations
Method for preparing CdTe quantum dots in aqueous phase and at low temperature
CN102191038A
Preparation method of gold-silver bimetal nanocluster capable of generating near-infrared electrochemical luminescence radiation