Heat-resistant high-strength aluminum alloy and preparation method thereof

Through the method of combining aerosol screening and additive manufacturing, the combination of elements such as Mn, Sc, Zr and Nd is used to form intermetallic compounds, which solves the problem of low strength of existing aluminum alloys under high temperature conditions and achieves high temperature Prepared from high-strength heat-resistant high-strength aluminum alloy, ensuring the integrity and continuity of the structure.

CN118773489APending Publication Date: 2024-10-15AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410998176.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-15

Smart Images

  • Figure CN118773489A_ABST
    Figure CN118773489A_ABST
Patent Text Reader

Abstract

The invention relates to a heat-resistant high-strength aluminum alloy and a preparation method thereof, and belongs to the technical field of additive manufacturing aluminum alloys. The heat-resistant high-strength aluminum alloy comprises the following components in percentage by weight: 4.0-7.0% of Mn; 0.65% to 0.85% of Sc; zr: 0.25% to 0.45%; 0.1% to 1.0% of Nd; and Al: the balance. Through mutual cooperation of Mn, Sc, Zr, Nd and other elements, strict control of the content ratio of the elements, no Mg element, and additive manufacturing, the oxidation burning loss degree is small, the integrity and continuity of the structure in the high-strength aluminum alloy are guaranteed, and the strength is high, especially at the temperature of 300 DEG C or above. At the temperature of 300 DEG C, the tensile strength of the alloy is 220 MPa or above, and the yield strength of the alloy is 200 MPa or above; and at the temperature of 350 DEG C, the tensile strength is 145 MPa or above, and the yield strength is 139 MPa or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing of aluminum alloys, and in particular to a heat-resistant high-strength aluminum alloy and a preparation method thereof. Background Art

[0002] Additive manufacturing has good designability and can meet the needs of rapid and accurate forming of complex, thin-walled, hollow parts, etc. It has broad application prospects in the fields of aerospace, etc. As a traditional lightweight structural material, aluminum alloy has become a key material type for the development and application of additive manufacturing technology.

[0003] At present, the commonly used aluminum alloy material for additive manufacturing is AlSi10Mg, which has a low strength after stress relief annealing, only about 300MPa, and has lower high-temperature performance, making it difficult to meet the requirements of use under higher loads and higher temperatures. Studies have found that the tensile strength and yield strength of 3D printed AlSi10Mg alloy at 200°C after annealing are reduced to 180-190MPa and 150-160MPa, respectively. The tensile strength and yield strength of traditional heat-resistant cast aluminum alloys at 300°C are only about 170MPa and 130MPa, respectively. With continuous research, the Al-Mn-Sc alloy system has been gradually developed, and its additive manufacturing process has good adaptability, becoming the development direction of additive manufacturing of heat-resistant high-strength aluminum alloys. After performance testing, the tensile strength is 250MPa at 250°C. However, due to the presence of Mg elements, the oxidation and burning are serious (the burning amount is 10% to 20%), the integrity and continuity of the alloy structure are poor, especially at temperatures above 300°C, the strength is poor.

[0004] Therefore, there is an urgent need for a heat-resistant high-strength aluminum alloy with high high-temperature strength to ensure the integrity and continuity of the alloy structure. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a heat-resistant high-strength aluminum alloy and a preparation method thereof, so as to solve the problem of poor high-temperature strength of existing aluminum alloys.

[0006] On the one hand, the present invention provides a heat-resistant high-strength aluminum alloy, which includes, by weight percentage, 4.0% to 7.0% Mn; 0.65% to 0.85% Sc; 0.25% to 0.45% Zr; 0.1% to 1.0% Nd; and Al as the balance.

[0007] Furthermore, the heat-resistant high-strength aluminum alloy includes, by weight percentage, 4.8% to 7.0% Mn; 0.68% to 0.72% Sc; 0.30% to 0.36% Zr; 0.3% to 0.5% Nd; and the balance of Al.

[0008] Furthermore, the heat-resistant high-strength aluminum alloy further includes X, wherein X is selected from one or more of La and Ce.

[0009] Furthermore, the X is La, and La: 0.5% to 0.8%.

[0010] Furthermore, the X is Ce, Ce: 1.0%-1.3%.

[0011] Furthermore, the X is La and Ce, La: 0.5% to 0.8%; Ce: 1.0% to 1.3%.

[0012] Furthermore, at 300° C., the tensile strength is above 220 MPa, and the yield strength is above 200 MPa.

[0013] Furthermore, at 350° C., the tensile strength is above 145 MPa, and the yield strength is above 139 MPa.

[0014] On the other hand, the present invention provides a method for preparing the heat-resistant high-strength aluminum alloy, which is prepared by combining gas atomization screening and additive manufacturing, and comprises the following steps:

[0015] S1: Powder preparation, using aluminum ingots, magnesium ingots, aluminum-based master alloy ingots or alloy prefabricated ingots as alloy raw materials, smelting in a vacuum atomization furnace under inert atmosphere protection, and crushing the molten metal by high-pressure inert gas to prepare different types of alloy powders;

[0016] S2: powder processing, screening, mixing and drying the obtained alloy powder;

[0017] After sieving, the particle size of the alloy powder is ≤200μm;

[0018] S3: Additive manufacturing, using laser powder bed fusion technology to perform additive manufacturing on the processed alloy powder; the additive manufacturing process uses argon gas for protection, the oxygen content of the atmosphere is controlled to be less than 100ppm, the substrate preheating temperature is 50-250℃, and the number of repeated scans is 0-1 times;

[0019] S4: Heat-resistant and high-strength aluminum alloy is obtained after heat treatment.

[0020] Furthermore, in step S3, a strip scanning strategy is adopted, with a laser power of 230 to 295 W, a scanning rate of 1500 to 1800 mm / s, a powder layer thickness of 20 to 60 μm, and an overlap spacing of 0.1 to 0.2 mm.

[0021] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0022] 1. The present invention uses Mn, Sc, Zr and Nd to cooperate with each other, and strictly controls the content ratio of the elements, and does not contain Mg. Through additive manufacturing, the degree of oxidation and burning is small, and the integrity and continuity of the internal structure of the high-strength aluminum alloy are guaranteed. The obtained structure is relatively dense, without defects such as holes and cracks, so that the strength is higher, especially at temperatures above 300°C. At 300°C, the tensile strength is above 220MPa and the yield strength is above 200MPa; at 350°C, the tensile strength is above 145MPa and the yield strength is above 139MPa.

[0023] 2. In the present invention, the element Nd, La and / or Ce are added to form Al3Nd, Al 11 Nd3、Al 11 La3、Al 11 Ce3 heat-resistant intermetallic compounds hinder dislocation migration and exert the Orowan strengthening effect; at the same time, these intermetallic compounds have good thermal stability and can effectively inhibit the coarsening of the structure during heat treatment, which helps to ensure the high-temperature strength of the aluminum alloy obtained after additive manufacturing.

[0024] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0026] Figure 1 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 1;

[0027] Figure 2 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 2;

[0028] Figure 3 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 3;

[0029] Figure 4 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 4;

[0030] Figure 5 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 5;

[0031] Figure 6This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 6;

[0032] Figure 7 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 7;

[0033] Figure 8 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 8;

[0034] Fig. 9 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 9;

[0035] Fig.10 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 1;

[0036] Fig.11 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 2;

[0037] Fig.12 This is a metallographic photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 3;

[0038] Fig.13 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 4;

[0039] Fig.14 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 5;

[0040] Fig.15 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 6;

[0041] Fig.16 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 10;

[0042] Fig.17 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 11;

[0043] Fig.18 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 12;

[0044] Fig.19 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 13;

[0045] Fig. 20 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 14;

[0046] Fig.21 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Example 15;

[0047] Fig. 22This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 7;

[0048] Fig.23 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 8;

[0049] Fig.24 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 9;

[0050] Fig.25 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 10;

[0051] Fig.26 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 11;

[0052] Fig. 27 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 12;

[0053] Fig.28 This is a metallographic structure photograph of the heat-resistant high-strength aluminum alloy obtained in Comparative Example 13;

[0054] Fig.29 This is a metallographic structure photograph of the heat-resistant and high-strength aluminum alloy obtained in Comparative Example 14. DETAILED DESCRIPTION

[0055] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0056] Additive manufacturing has broad application prospects in aerospace and other fields. Aluminum alloy, as a traditional lightweight structural material, has become a key material type for the development and application of additive manufacturing technology. Among them, AlSi10Mg is the most widely used aluminum alloy material. Its tensile strength and yield strength at 200°C are 180-190MPa and 150-160MPa respectively. Its high temperature performance is poor and it is difficult to meet the requirements of use under higher loads and higher temperatures.

[0057] With continuous research, the Al-Mn-Sc alloy system has been gradually developed, and its additive manufacturing process has good adaptability, becoming the development direction of additive manufacturing of heat-resistant high-strength aluminum alloys. After performance testing, the tensile strength is 250MPa at 250°C. However, due to the presence of Mg elements, oxidation and burning are serious, and the integrity and continuity of the alloy structure are poor, especially at temperatures above 300°C, the strength is poor.

[0058] Therefore, the present invention provides a heat-resistant high-strength aluminum alloy, which comprises, by weight percentage, 4.0% to 7.0% Mn; 0.65% to 0.85% Sc; 0.25% to 0.45% Zr; 0.1% to 1.0% Nd; and Al as the balance.

[0059] Compared with the prior art, the present invention uses the mutual coordination of elements such as Mn, Sc, Zr and Nd, and strictly controls the content ratio of the elements, and does not contain Mg elements. After additive manufacturing, the degree of element oxidation and burning is small, and the integrity and continuity of the internal structure of the high-strength aluminum alloy are guaranteed, and the strength is high, especially at temperatures above 300°C. After performance testing, at 300°C, the tensile strength is above 220MPa and the yield strength is above 200MPa; at 350°C, the tensile strength is above 145MPa and the yield strength is above 139MPa.

[0060] It should be noted that the elements in the present invention have the following functions:

[0061] Mn: Manganese, as the main alloying element, ensures the adaptability and performance foundation of the forming process of heat-resistant and high-strength aluminum alloys. On the one hand, adding 4.0-7.0% of Mn elements makes the alloy near the Al-Mn eutectic composition, the solid-liquidus temperature range is narrow, and the additive manufacturing process adaptability is better. On the other hand, Mn and Al have a large lattice mismatch strain, and adding Mn can obtain a significant solid solution strengthening effect.

[0062] More importantly, the thermal diffusion coefficient of Mn in the Al matrix is ​​low, which makes the precipitation of Mn element less in the subsequent heat treatment process, which can maintain a good solid solution strengthening effect and help to obtain better high-temperature strength. Even if some Mn atoms are precipitated, they can form a quasi-crystalline phase with good stability with Al, obtain the Orowan strengthening effect, and improve the high-temperature strength.

[0063] However, too much Mn content will deteriorate the additive manufacturing process performance of the alloy and easily lead to defects such as cracks; too little Mn content will weaken the strengthening effect.

[0064] Sc: Scandium is a precipitation strengthening element in heat-resistant high-strength aluminum alloys. However, the cost of this element is high. When added in an amount of 0.65% to 0.85%, it can form a considerable volume fraction of Al3Sc intermetallic compounds in the alloy, produce heterogeneous nucleation, reduce the thermal cracking tendency of the alloy forming process, and help to achieve the addition of a higher Mn content, providing a guarantee for obtaining higher high-temperature strength.

[0065] In addition, Al3Sc intermetallic compounds also have good thermal stability. Not only can they exert precipitation strengthening effects themselves, but they can also effectively inhibit the coarsening and growth of other second phases and grains to ensure high-temperature performance.

[0066] Zr: Zirconium can form Al3Zr with Al and has L12 structure. This phase has good thermal stability. When Zr and Sc exist at the same time, Zr atoms will partially replace Sc atoms in Al3Sc intermetallic compound to form Al3(Sc 1-x ,Zr x ) pseudo binary phase, which helps to reduce the amount of Sc element added and reduce material costs. However, if the zirconium content is too high, it will reduce the Al3 (Sc 1-x ,Zr x ) The stability of the pseudo-binary phase is not conducive to obtaining a good precipitation strengthening effect. Therefore, the amount of Zr added is 0.25% to 0.45%.

[0067] Specifically, the heat-resistant high-strength aluminum alloy further includes X, wherein X is selected from one or more of La and Ce.

[0068] Specifically, the X is La, and La: 0.5% to 0.8%.

[0069] Specifically, X is Ce, Ce: 1.0%-1.3%.

[0070] Specifically, the X is La and Ce, La: 0.5% to 0.8%; Ce: 1.0% to 1.3%.

[0071] It should be noted that in the present invention, the element Nd, La and / or Ce are added to form Al3Nd, Al 11 Nd3、Al 11 La3、Al 11 Ce3 heat-resistant intermetallic compounds hinder dislocation migration and exert the Orowan strengthening effect; at the same time, these intermetallic compounds have high melting points and good thermal stability, which can effectively inhibit the heat treatment process and the coarsening of the structure at high temperatures, and help to ensure the high-temperature strength of the aluminum alloy obtained after additive manufacturing. In order to ensure the forming process performance, reduce the tendency of hot cracking, and take into account the cost and performance improvement effect, the addition amounts are Nd: 0.1%~1.0%; La: 0.5%~0.8%; Ce: 1.0%~1.3%.

[0072] Specifically, in terms of weight percentage, the heat-resistant high-strength aluminum alloy includes Mn: 4.8% to 7.0%; Sc: 0.68% to 0.72%; Zr: 0.30% to 0.36%; Nd: 0.3% to 0.5%; and Al: the balance.

[0073] The present invention provides a method for preparing a heat-resistant high-strength aluminum alloy, which is prepared by combining gas atomization screening and additive manufacturing, and comprises the following steps:

[0074] S1: Powder preparation, using aluminum ingots, magnesium ingots, aluminum-based master alloy ingots or alloy prefabricated ingots as alloy raw materials, smelting in a vacuum atomization furnace under inert atmosphere protection, and crushing the molten metal by high-pressure inert gas to prepare different types of alloy powders;

[0075] S2: powder processing, screening, mixing and drying the obtained alloy powder;

[0076] S3: Additive manufacturing, using laser powder bed fusion technology to perform additive manufacturing on the processed alloy powder;

[0077] S4: Heat-resistant and high-strength aluminum alloy is obtained after heat treatment.

[0078] Compared with the prior art, the present invention uses the combination of alloy components, gas atomization screening and additive manufacturing methods to obtain a high-strength aluminum alloy with an internal structure of fish-scale molten pools stacked layer by layer, dense structure, and no obvious cracks, holes and other defects. After performance testing, at 300°C, the tensile strength is above 220MPa and the yield strength is above 200MPa; at 350°C, the tensile strength is above 145MPa and the yield strength is above 139MPa.

[0079] It should be noted that aluminum ingots, magnesium ingots, aluminum-based master alloy ingots or alloy prefabricated ingots are used as raw materials, smelted in a vacuum atomization furnace under the protection of an inert atmosphere, and the metal liquid is crushed by high-pressure inert gas to prepare the matrix alloy powder. The alloy powder is cooled in an inert atmosphere.

[0080] Specifically, after screening, the particle size of the alloy powder is ≤200 μm.

[0081] Preferably, after screening, the particle size of the alloy powder is ≤60 μm.

[0082] It should be noted that if the particle size of the alloy powder is too large, the power required for melting by a light source such as a high-energy laser beam or an electron beam is higher, which is more likely to cause burning or oxidation of the alloy elements. In addition, if the particle size is too large, the roughness of the formed surface is large, which is not conducive to ensuring dimensional accuracy and surface quality. In order to ensure the quality and high-temperature performance of the heat-resistant high-strength aluminum alloy, the particle size of the alloy powder needs to be controlled to be no more than 200 μm, preferably below 60 μm.

[0083] Specifically, the sieved alloy powder is mixed at a rotation speed of 1 r / min to 15 r / min for a duration of 10 min to 60 min.

[0084] It should be noted that under the above rotation speed and duration, the powders are effectively mixed, with uniform particle size and composition, and no obvious segregation. When the rotation speed is too low, sufficient mixing cannot be achieved; when the rotation speed is too high, the friction between the alloy powders is more intense, which easily causes surface oxidation. When the duration is too short, the mixing effect is insufficient; when the duration is too long, more static electricity accumulates on the powder surface, which easily causes powder agglomeration.

[0085] Specifically, during the drying process, the mixed powder is placed on a tray and spread out in a flat manner with a thickness of no more than 2 cm, and is placed in an explosion-proof drying oven and dried at 60° C. to 150° C. for 1 to 10 hours, followed by cooling in the oven.

[0086] It should be noted that drying is helpful for subsequent additive manufacturing and ensures the strength and quality of the resulting aluminum alloy. When the drying temperature is too low or the duration is too short, it is impossible to effectively remove the surface adsorbed moisture or adsorbed oxygen; when the temperature is too high or the duration is too long, the alloy powder will be oxidized more seriously, resulting in relatively poor quality of the resulting aluminum alloy.

[0087] Specifically, in step S3, a strip scanning strategy is adopted, with a laser power of 230 to 295 W, a scanning rate of 1500 to 1800 mm / s, a powder layer thickness of 20 to 60 μm, and an overlap spacing of 0.1 to 0.2 mm.

[0088] Specifically, the additive manufacturing process is protected by argon gas, the oxygen content of the atmosphere is controlled to be less than 100 ppm, the substrate preheating temperature is 50 to 250° C., and the number of repeated scans is 0 to 1 times.

[0089] It should be noted that the parameters of the additive manufacturing process are closely related to the room temperature properties of the final aluminum alloy. When the laser power is too large, the scanning rate is too low, the powder layer thickness and the overlap spacing are too small, the volume energy density will be too high, and the low-boiling point elements in the melt will easily evaporate, resulting in the formation of circular holes in the organization; conversely, when the volume energy density is too small (the laser power is too low, the scanning speed is too high, or the powder layer thickness and the overlap spacing are too large), the input energy is not enough to completely remelt the alloy powder within a unit volume, resulting in defects such as irregular holes and unmelted powder.

[0090] In addition, in order to reduce oxidation and burning during the additive manufacturing process, inert gas (argon) protection is used to ensure that the oxygen content in the forming chamber is less than 100ppm. Excessive oxygen content will lead to severe oxidation and burning, destroy the continuity and integrity of the organization, and ultimately lead to a decrease in mechanical properties.

[0091] Substrate preheating can effectively control the cooling rate of the melt during the forming process and inhibit the cracking tendency of the alloy. However, too high a preheating temperature will reduce the solid solution strengthening effect. At the same time, the amount of precipitation strengthening phase after heat treatment will decrease, reducing the precipitation strengthening effect. Since the alloy has good adaptability to the forming process, in order to ensure the mechanical properties, the preheating temperature is selected to be 50-250℃.

[0092] For some key structures or parts with large stress concentration coefficients, repeated scanning can release stress or ensure the density of key structures; but too many repetitions will also cause excessive burning or oxidation. Therefore, the number of repeated scans is selected to be 0 to 1.

[0093] Specifically, the heating temperature of the heat treatment is 300-360° C., and the insulation time is 1.5-12 hours.

[0094] It should be noted that the present invention controls the heating temperature of the heat treatment to be 300-360°C and the holding time to be 1.5-12h, which is beneficial to the Al3(Sc, Zr), Al3Zr, Al3Nd or Al 11 The precipitation of Nd3 and the transformation of quasicrystalline phase AlMnSi. When the temperature is too low or the holding time is too short, the precipitation strengthening phase cannot be fully precipitated; when the temperature is too high or the holding time is too long, the precipitation phase will grow unnecessarily, weakening the precipitation strengthening effect.

[0095] In order to more clearly describe the present invention, it is further illustrated by the following examples and comparative examples.

[0096] Example 1

[0097] The preparation process of heat-resistant high-strength aluminum alloy is as follows:

[0098] S1: powder preparation, weighing alloy raw materials aluminum ingot, magnesium ingot, and aluminum-based master alloy ingot according to proportion, placing them in a crucible for melting, crushing the molten alloy liquid with nitrogen to prepare alloy powder, and cooling the alloy powder in an inert atmosphere;

[0099] S2: Powder treatment: sieve the alloy powder to obtain alloy powder of ≤53μm, then add the alloy powder into the mixer for mixing at a speed of 10r / min for 30min; spread the mixed alloy powder on a tray with a thickness of 1.5cm, and dry it in an explosion-proof drying oven at 120℃ for 1.5h, and cool it with the furnace;

[0100] S3: Additive manufacturing, using laser powder bed fusion equipment to form, using strip scanning strategy, laser power 265W, scanning rate 1600mm / s, powder layer thickness 40μm, overlap spacing 0.12mm; argon gas is used for protection during the forming process, and the oxygen content of the atmosphere is controlled to be 60ppm; the substrate preheating temperature during the forming process is 100℃; the number of repeated scans is 0 times; and it is taken out after cooling;

[0101] S4: The sample is heat treated in a heating furnace at a holding temperature of 310°C for 9 hours, and then cooled in the furnace to obtain a heat-resistant high-strength aluminum alloy.

[0102] Examples 2-9, Comparative Examples 1-6

[0103] The difference between Examples 2-9 and Comparative Examples 1-6 and Example 1 lies in the alloy composition ratio, as shown in Table 1.

[0104] Table 1 Different parameters of Examples 1-9 and Comparative Examples 1-6 (unit: wt%)

[0105]

[0106]

[0107] *“-” in Table 1 means no addition.

[0108] Performance Testing

[0109] The above-mentioned Examples 1-9 and Comparative Examples 1-6 were subjected to performance tests, and the microstructure of the materials was observed and the high temperature (300°C and 350°C) tensile properties were tested according to GB / T3246.1-2012 and HB5195-1996, respectively. The test results are shown in Table 2 and Table 3, respectively.

[0110] Table 2 Performance test results (300℃)

[0111]

[0112]

[0113] In combination with Examples 1-9 and Comparative Examples 1-6 and Table 2, it can be seen that when the components and proportions provided in Examples 1-9 are used, the mutual coordination of elements such as Mn, Sc, Zr and Nd has higher high temperature strength. At 300°C, the tensile strength of the obtained aluminum alloy is above 229 MPa, the yield strength is above 217 MPa, and there are no cracks inside.

[0114] Table 3 Performance test results (350℃)

[0115] Group Tensile strength / MPa Yield strength / MPa Remark Example 1 157 144 Example 2 145 139 Example 3 187 175 Example 4 179 168 Example 5 175 163 Example 6 188 173 Example 7 182 166 Example 8 194 183 Example 9 178 173 Comparative Example 1 125 105 Comparative Example 2 122 100 Comparative Example 3 132 119 Comparative Example 4 35 21 Comparative Example 5 143 130 Comparative Example 6 - - Print cracking

[0116] In combination with Examples 1-9 and Comparative Examples 1-6 and Table 3, it can be seen that when the components and proportions provided in Examples 1-9 are used, the mutual coordination of elements such as Mn, Sc, Zr and Nd has higher high temperature strength. At 350°C, the tensile strength of the obtained aluminum alloy is above 145 MPa, the yield strength is above 139 MPa, and there are no cracks inside.

[0117] Examples 10-15, Comparative Examples 7-14

[0118] The difference between Examples 10-15 and Comparative Examples 7-14 and Example 1 is the preparation method, which is specifically shown in Table 4.

[0119] Table 4 Different parameters of Examples 10-15 and Comparative Examples 7-14

[0120]

[0121] Performance Testing

[0122] The above Examples 10-15 and Comparative Examples 7-14 were subjected to performance testing, and the microstructure and high temperature (300°C and 350°C) tensile properties of the materials were observed or tested according to GB / T 3246.1-2012 and HB5195-1996, respectively. The test results are shown in Tables 5 and 6, respectively.

[0123] Table 5 Performance test results (300℃)

[0124] Group Tensile strength / MPa Yield strength / MPa Remark Example 1 236 221 Example 10 235 223 Embodiment 11 232 220 Example 12 238 221 Embodiment 13 229 220 Embodiment 14 243 227 Embodiment 15 230 223 Comparative Example 7 198 177 Comparative Example 8 201 185 Comparative Example 9 206 189 Comparative Example 10 195 168 Comparative Example 11 - - Print cracking Comparative Example 12 207 200 Comparative Example 13 205 197 Comparative Example 14 200 193

[0125] In combination with Example 1, Examples 10-15, Comparative Examples 7-14 and Table 5, it can be seen that the heat-resistant high-strength aluminum alloy is prepared by the preparation method provided by Example 1 and Examples 10-15 of the present invention. The heat-resistant high-strength aluminum alloy has high high-temperature strength through additive manufacturing and strict control of preparation parameters. At 300°C, the tensile strength of the obtained aluminum alloy is above 229 MPa, the yield strength is above 220 MPa, and there is no crack inside.

[0126] Table 6 Performance test results (350℃)

[0127] Group Tensile strength / MPa Yield strength / MPa Remark Example 1 157 144 Example 10 156 142 Embodiment 11 155 141 Example 12 149 140 Embodiment 13 151 143 Embodiment 14 156 149 Embodiment 15 152 147 Comparative Example 7 103 97 Comparative Example 8 112 101 Comparative Example 9 109 100 Comparative Example 10 105 98 Comparative Example 11 - - Print cracking Comparative Example 12 119 110 Comparative Example 13 121 114 Comparative Example 14 125 117

[0128] In combination with Example 1, Examples 10-15, Comparative Examples 7-14 and Table 5, it can be seen that the heat-resistant high-strength aluminum alloy is prepared by the preparation method provided by Example 1 and Examples 10-15 of the present invention. The heat-resistant high-strength aluminum alloy has high high-temperature strength through additive manufacturing and strict control of preparation parameters. At 350°C, the tensile strength of the obtained aluminum alloy is above 149 MPa, the yield strength is above 140 MPa, and there is no crack inside.

[0129] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A heat-resistant high-strength aluminum alloy, characterized in that: According to weight percentage, it includes Mn: 4.0% to 7.0%; Sc: 0.65%~0.85%; Zr: 0.25%~0.45%; Nd: 0.1%~1.0%; Al: balance.

2. The heat-resistant high-strength aluminum alloy according to claim 1, characterized in that: According to weight percentage, it includes Mn: 4.8% to 7.0%; Sc: 0.68%~0.72%; Zr: 0.30%~0.36%; Nd: 0.3%~0.5%; Al: balance.

3. The heat-resistant high-strength aluminum alloy according to claim 1 or 2, characterized in that: It also includes X, wherein X is selected from one or more of La and Ce.

4. The heat-resistant high-strength aluminum alloy according to claim 1 or 2, characterized in that: The X is La, and La: 0.5% to 0.8%.

5. The heat-resistant high-strength aluminum alloy according to claim 1 or 2, characterized in that: The X is Ce, Ce: 1.0%-1.3%.

6. The heat-resistant high-strength aluminum alloy according to claim 1 or 2, characterized in that: The X is La and Ce, La: 0.5% to 0.8%; Ce: 1.0%-1.3%.

7. The heat-resistant high-strength aluminum alloy according to claim 1 or 2, characterized in that: At 300°C, the tensile strength is above 220MPa and the yield strength is above 200MPa.

8. The heat-resistant high-strength aluminum alloy according to claim 1 or 2, characterized in that: At 350°C, the tensile strength is above 145MPa and the yield strength is above 139MPa.

9. A method for preparing the heat-resistant high-strength aluminum alloy according to any one of claims 1 to 8, characterized in that: The preparation is carried out by combining gas atomization screening and additive manufacturing, including the following steps: S1: Powder preparation, using aluminum ingots, magnesium ingots, aluminum-based master alloy ingots or alloy prefabricated ingots as alloy raw materials, smelting in a vacuum atomization furnace under inert atmosphere protection, and crushing the molten metal by high-pressure inert gas to prepare different types of alloy powders; S2: powder processing, screening, mixing and drying the obtained alloy powder; After sieving, the particle size of the alloy powder is ≤200μm; S3: Additive manufacturing, using laser powder bed fusion technology to perform additive manufacturing on the processed alloy powder; the additive manufacturing process uses argon gas for protection, the oxygen content of the atmosphere is controlled to be less than 100ppm, the substrate preheating temperature is 50-250℃, and the number of repeated scans is 0-1 times; S4: Heat-resistant and high-strength aluminum alloy is obtained after heat treatment.

10. The method for preparing the heat-resistant high-strength aluminum alloy according to claim 9, characterized in that: In step S3, a strip scanning strategy is adopted, with a laser power of 230 to 295 W, a scanning rate of 1500 to 1800 mm / s, a powder layer thickness of 20 to 60 μm, and an overlap spacing of 0.1 to 0.2 mm.

Citation Information

Cited By

  • Heat-resistant high-strength aluminum alloy material for additive manufacturing and preparation method of heat-resistant high-strength aluminum alloy material

    CN119162494A

  • Heat-resistant aluminum alloy material as well as preparation method and application thereof

    CN120796786A

  • A heat-resistant aluminum alloy material and a preparation method and application thereof

    CN120796786B