Eu-activated beta-sialon phosphor particles, beta-sialon phosphor powder, and light-emitting device
By controlling Eu amount distribution and annealing treatment, the problem of Eu element aggregation at grain boundaries in Eu-activated β-Sialon phosphors was solved, and its internal quantum efficiency and luminescence performance were improved.
Patent Information
- Application Number
- CN202380024616.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-07
- Filing Date
- 2023-03-01
- Publication Date
- 2024-10-15
Smart Images

Figure CN118786198A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to Eu activated β-sialon phosphor particles, β-sialon phosphor powder and a light emitting device. Background Art
[0002] There is known a light emitting device which is a combination of a light emitting element that emits primary light and a phosphor that absorbs the primary light and emits secondary light.
[0003] In recent years, as light-emitting devices have become more powerful, the heat resistance and durability of phosphors have been increasingly demanded. Therefore, β-sialon phosphors with a stable crystal structure have attracted much attention.
[0004] It is known that the crystal structure of β-sialon contains Eu 2+ The phosphor (Eu-activated β-sialon phosphor) is excited by, for example, blue light and emits green light.
[0005] Eu-activated β-Sialon is being studied as a green luminescent component of light-emitting devices such as white LEDs (Light Emitting Diodes). Eu-activated β-Sialon has a tendency to have a very sharp luminescent spectrum among phosphors containing Eu. Therefore, various studies have been conducted on β-Sialon.
[0006] As an example, Patent Document 1 describes a method for manufacturing a β-sialon phosphor, which includes the following steps: a first heat treatment step, in which a mixture comprising an aluminum compound, a first europium compound and silicon nitride is heat treated to obtain a first heat-treated product; and a second heat treatment step, in which the first heat-treated product and a second europium compound are heat treated in a rare gas atmosphere to obtain a second heat-treated product.
[0007] As another example, Patent Document 2 describes a method for producing a β-sialon phosphor, which comprises the following steps: a calcination step, in which a raw material mixture of the β-sialon phosphor is calcined at a temperature of 1820°C to 2200°C in a nitrogen atmosphere to obtain a calcined product; and an annealing step, in which the calcined product is annealed at a temperature of 1100°C or above in a reducing atmosphere.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2017-002278
[0011] Patent Document 2: International Publication No. 2010 / 143590 Summary of the invention
[0012] An object of the present invention is to provide a Eu-activated β-sialon phosphor having good internal quantum efficiency.
[0013] The present inventors have completed the invention provided below and solved the above-mentioned problems.
[0014] The present invention is as follows.
[0015] 1. A β-sialon phosphor particle, which is a Eu-activated β-sialon phosphor particle having a grain boundary,
[0016] In a cross section including the grain boundary, when a linear analysis of the elemental composition of the grain boundary and both sides thereof is performed in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the grain surface where the grain boundary exists,
[0017] On the line segment obtained by the line analysis, (i) the Eu amount at the point P where the Eu amount on the grain boundary shows a peak is set to N Eu (ii) The amount of Eu at point Q, which is 50 nm away from point P, is N' Eu When N Eu / N' Eu The value is below 3.00.
[0018] 2. The β-sialon phosphor particle according to 1, wherein the amount of oxygen at point P is N ОΟ , let the amount of oxygen at point Q be N' ОΟ When (N Eu / N O ) / (N Eu ' / N O ') is less than 2.00.
[0019] 3. The β-sialon phosphor particle according to 1 or 2, wherein the amount of oxygen at point P is N ΟО When N Eu / N O The value is below 0.70.
[0020] 4. The β-sialon phosphor particle according to any one of 1 to 3, wherein the amount of oxygen at the point P is N ΟО ,
[0021] When the element composition of the grain boundary and its both sides is linearly analyzed in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the grain surface where the grain boundary exists, the point P where the Al amount on the grain boundary shows a peak is set on the line segment obtained by the linear analysis. (Al) The amount of Al at N Al hour,
[0022] N Al / N O The value of is less than 1.00.
[0023] 5. A β-sialon phosphor particle, which is a Eu-activated β-sialon phosphor particle having a grain boundary,
[0024] In a cross section including the grain boundary, when a linear analysis of the elemental composition of the grain boundary and both sides thereof is performed in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the grain surface where the grain boundary exists,
[0025] On the line segment obtained by the line analysis, (i) the point P where the amount of O on the grain boundary shows a peak value is (O) The amount of Eu at is set to N Eu(O) , (ii) from point P (O) Leave the point Q of 50nm (O) The Eu quantity at is set to N' Eu(O) When N Eu(O) / N' Eu(O) The value is below 2.50.
[0026] 6. The β-sialon phosphor particle according to 5, wherein the point P (O) The amount of oxygen at ΟО(O) , click Q (O) The amount of oxygen at ΟО(O) When (N Eu(O) / N O(O) ) / (N' Eu(O) / N' O(O) ) is less than 1.20.
[0027] 7. The β-sialon phosphor particle according to 5 or 6, wherein the point P (O) The amount of oxygen at ΟО(O) When N Eu(O) / N O(O) The value is below 0.70.
[0028] 8. The β-sialon phosphor particle according to any one of 5 to 7, wherein the point P (O) The amount of oxygen at ΟО(O) , point P (O) The amount of aluminum at Al(O) When N Al(O) / N O(O) The value of is less than 1.00.
[0029] 9. A β-Sialon phosphor powder comprising the β-Sialon phosphor particles according to any one of 1 to 8.
[0030] 10. A light emitting device comprising a light source and a wavelength conversion component,
[0031] The wavelength conversion component includes phosphor powder.
[0032] The phosphor powder mentioned above includes the β-sialon phosphor powder described in 9.
[0033] 11. The light emitting device according to 10, wherein the light source includes an LED chip that generates light with a wavelength of 300 nm to 500 nm.
[0034] According to the present invention, a Eu-activated β-sialon phosphor having excellent internal quantum efficiency is provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a cross-sectional view schematically showing an example of the structure of a light emitting device.
[0036] Figure 2 This is a diagram for explaining the measurement positions of the line analysis in Example 1.
[0037] Figure 3 This is a diagram for explaining the measurement positions of the line analysis in Comparative Example 1. DETAILED DESCRIPTION
[0038] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0039] In this specification, Eu-activated β-sialon phosphor particles may be simply referred to as β-sialon phosphor particles.
[0040] The term "grain boundary" in this specification refers to a discontinuous boundary surface between a certain crystal and another crystal. In a grain boundary, two or more crystals (grains) are in contact with each other in a state of different orientations.
[0041] In the present specification, the "surface of the particle" of the β-sialon phosphor particle refers to at least any one of the following.
[0042] (i) The boundary between β-sialon phosphor particles in the atmosphere and the atmosphere
[0043] (ii) In the atmosphere, the boundary between the layer containing at least one of amorphous Si, Al, O, N, Eu, etc., existing on the surface of the β-sialon phosphor particle and the atmosphere
[0044] (iii) A boundary between a layer including at least one of Si, Al, O, N, Eu, etc., which exists as a crystalline phase on the surface of the β-sialon phosphor particles in the atmosphere and the atmosphere.
[0045] The “particle surface” may be referred to as a boundary between a position where at least one of Si, Al, O, N, Eu, etc. is detected and a position where at least one of them is not detected in element distribution analysis by energy dispersive X-ray spectroscopy (EDS).
[0046] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means greater than or equal to X and less than or equal to Y. For example, "1 to 5 mass %" means "1 mass % or more and 5 mass % or less".
[0047] <First embodiment: β-sialon phosphor particles>
[0048] The β-sialon phosphor particles according to the first embodiment have grain boundaries.
[0049] In the cross section including the grain boundary, at a depth of 200 nm from the portion of the particle surface where the grain boundary exists, the elemental composition of the grain boundary and both sides thereof was linearly analyzed in a direction perpendicular to the grain boundary.
[0050] At this time, on the line segment obtained by the line analysis, (i) the Eu amount at the point P where the Eu amount on the grain boundary shows a peak is set to N Eu (ii) The amount of Eu at point Q, which is 50 nm away from point P, is N' Eu When N Eu / N' Eu The value is below 3.00.
[0051] N Eu / N' Eu A value of 3.00 or less means that the amount of Eu at point P corresponding to the grain boundary at a shallow position such as a depth of 200 nm in the particle is 3 times or less of the amount of Eu at point Q which is sufficiently away from point P (50 nm).
[0052] According to the knowledge of the inventors and the results of previous studies, in the conventional β-sialon phosphor, the Eu element that is not completely dissolved in the crystal is concentrated in the grain boundary. Eu / N' Eu The value of is a large value exceeding 3.00 (Note: Comparative Example described later).
[0053] Eu generally functions as a luminescence center by being dissolved in a crystal. However, if Eu is concentrated at the grain boundary, unintended light absorption (light absorption that does not contribute to fluorescence) occurs at the grain boundary and its vicinity, which may deteriorate the internal quantum efficiency.
[0054] It is believed that the β-sialon phosphor particles of the first embodiment have less Eu in the portion corresponding to the grain boundary at a shallow position of 200 nm in the particle depth, so that unintended light absorption is less likely to occur at the grain boundary and its vicinity. As a result, it is believed that the β-sialon phosphor particles of the first embodiment have good internal quantum efficiency.
[0055] By the way, although point Q can have two points on both sides of point P, as long as at least one of the two points is used as point Q, N Eu / N' Eu The value of can be 3.00 or less. If the above inference mechanism is considered, it is inferred that as long as N is at least one of the two points Q on both sides of point P, Eu / N' Eu When the value of is 3.00 or less, the internal quantum efficiency can be improved.
[0056] The β-sialon phosphor particles of the first embodiment can be manufactured by using appropriate raw materials and adopting appropriate manufacturing methods and manufacturing conditions. Preferably, a small amount of titanium oxide (Ti2O3) can be added to the β-sialon phosphor and annealed to reduce the amount of Eu in the grain boundaries. The manufacturing method will be described in detail later.
[0057] N Eu / N' Eu The value of may be 3.00 or less, and is preferably 0.01 to 3.00, more preferably 0.10 to 3.00, further preferably 0.50 to 3.00, and particularly preferably 1.00 to 3.00.
[0058] Here, the line analysis, that is, the procedure of continuously performing elemental analysis on a line segment of a certain length in the cross section of the phosphor particle including the grain boundary, is described in advance. For more detailed procedures, refer to the examples described later.
[0059] (1) A sample is prepared by embedding β-sialon phosphor particles in a resin material such as epoxy resin.
[0060] (2) The sample prepared in (1) above is placed on a cross-section polisher to expose the cross-section of the embedded β-sialon phosphor particles.
[0061] (3) Observe the cross section exposed in (2) above with an electron microscope to identify a portion where a grain boundary suitable for analysis exists (grain boundary having a length of at least 200 nm from the particle surface and being approximately linear). Thin the portion and its surroundings with a focused ion beam (FIB) processing device to prepare a thin slice sample.
[0062] (4) In a thin-section sample (a cross section including a grain boundary), a line analysis is performed on the elemental composition of the grain boundary and both sides thereof in a straight line along a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the grain boundary present on the surface of the particle. The line analysis can be performed using a device that combines a scanning transmission electron microscope (STEM) with an apparatus capable of performing energy dispersive X-ray analysis (EDS).
[0063] (5) Based on the results of the line analysis, the amount of each element at each point such as point P (unit: atom%) is determined. Then, N is calculated based on the amount of each element thus determined. Eu / N' Eu The "ratio" of equal amounts of elements.
[0064] The description of the β-sialon phosphor particles according to the first embodiment will be continued.
[0065] Composition of β-sialon phosphor
[0066] β-sialon phosphors are usually composed of the general formula Si 6-z Al z O z N 8-z :Eu 2+ a (0<Z≤4.2, 0.001<a<1.0) represented by solid solution of Eu 2+ The phosphor is composed of β-sialon.
[0067] In the general formula Si 6-z Al z O z N 8-z :Eu 2+ a In the embodiment, the Z value and the content of europium are not particularly limited. The Z value is, for example, greater than 0 and less than 4.2. In addition, from the viewpoint of further improving the luminescence intensity of the β-sialon phosphor, a is 0.001 to 1.0. In addition, the content of europium is preferably 0.1 mass % to 2.0 mass %.
[0068] ·(N Eu / N O ) / (N Eu ' / N O ')
[0069] The amount of Eu generally contained in a β-sialon phosphor is relatively small compared to other main elements (Si, Al, O, and N). Therefore, by viewing the amount of Eu based on the amount of O (oxygen), it is possible to more clearly show that the amount of Eu in the grain boundaries is relatively small.
[0070] Specifically, when the amount of oxygen at point P is N00 and the amount of oxygen at point Q is N'00, (N Eu / N O ) / (N' Eu / N' O ) is preferably 2.00 or less, more preferably 0.01 to 2.00, further preferably 0.020 to 2.00, further preferably 0.03 to 1.80.
[0071] ·N Eu / N O Value
[0072] Think through N Eu / N' Eu The value is below 3.00, that is, the "ratio" of the Eu amount at point P to that at point Q is not too large, and the Eu amount on the grain boundary itself is not much compared with other elements, thereby further suppressing the unintended light absorption at the grain boundary and its vicinity, and further improving the internal quantum efficiency.
[0073] Specifically, N Eu / N O The value of , that is, the ratio of the Eu amount / O amount on the grain boundary (depth 200 nm) is preferably 0.70 or less, more preferably 0.001 to 0.70, further preferably 0.005 to 0.50, and particularly preferably 0.005 to 0.40.
[0074] ·N Al / N O Value
[0075] Since the amount of Al on the grain boundaries is not much compared to other elements, further improvement in the internal quantum efficiency can be expected.
[0076] The details are not yet clear, but based on past knowledge, there may be charge defects called aluminum oxide void centers near the grain boundaries that are believed to be in a glassy state. It is believed that the small amount of Al near the grain boundaries will reduce the number of charge defects and further improve the internal quantum efficiency.
[0077] Specifically, when the elemental composition of the grain boundary and both sides thereof is analyzed in a straight line in a direction perpendicular to the grain boundary at a depth of 200 nm from the grain boundary portion of the particle surface,
[0078] On the line segment obtained by the line analysis, the point P where the Al content on the grain boundary shows a peak is (Al) The Al content at N Al When N Al / N O The value of , that is, the ratio of the amount of Al / the amount of O near the grain boundary at a depth of 200 nm, is preferably 1.0 or less, more preferably 0.01 to 1.00, further preferably 0.01 to 0.70, and particularly preferably 0.05 to 0.50.
[0079] In addition, the amount of aluminum at point Q is N' Al When (N Al / N O ) / (N' Al / N' O ) is preferably 0.47 or less, more preferably 0.01 to 0.47 (N' ΟО is defined above).
[0080] In addition, N Al / N' Al The value of is preferably 1.10 or less, more preferably 0.10 to 1.10, further preferably 0.50 to 1.10, particularly preferably 0.75 to 1.10.
[0081] Supplementation of the amount of each element
[0082] For N Eu The numerical range of itself, etc., is recorded in advance for the sake of caution.
[0083] N Eu The value is usually 0.00 atom% to 1.50 atom%, preferably 0.05 atom% to 1.00 atom%, more preferably 0.10 atom% to 0.50 atom%, further preferably 0.10 atom% to 0.30 atom%.
[0084] N' Eu The value is usually 0.01 atom % to 1.00 atom %, preferably 0.01 atom % to 0.80 atom %, more preferably 0.02 atom % to 0.50 atom %, further preferably 0.03 atom % to 0.25 atom %.
[0085] N ОΟ The value is usually 0.10 atom % to 20.00 atom %, preferably 0.30 atom % to 20.00 atom %, and more preferably 0.50 atom % to 15.00 atom %.
[0086] N' ОΟ The value is usually 0.01 atom % to 10.00 atom %, preferably 0.05 atom % to 10.00 atom %, and more preferably 0.10 atom % to 10.00 atom %.
[0087] N Al The value is usually 0.00 atom % to 10.00 atom %, preferably 0.00 atom % to 3.50 atom %.
[0088] N'Al The value is usually 0.50 atom % to 10.00 atom %, preferably 0.50 atom % to 5.00 atom %, and more preferably 1.00 atom % to 5.00 atom %.
[0089] The quantity N of the N element at point P N It is usually 5.00 atom % to 40.00 atom %, preferably 10.00 atom % to 35.00 atom %, and more preferably 10.00 atom % to 30.00 atom %.
[0090] The quantity N' of the N element at point Q N It is usually 5.00 atom % to 40.00 atom %, preferably 10.00 atom % to 35.00 atom %, more preferably 10.00 atom % to 30.00 atom %, further preferably 10.00 atom % to 25.00 atom %.
[0091] The amount of Si element N at point P Si It is usually 50.00 atom % to 85.00 atom %, preferably 60.00 atom % to 80.00 atom %.
[0092] The amount of Si element at point Q is N' Si It is usually 50.00 atom % to 85.00 atom %, preferably 60.00 atom % to 80.00 atom %, more preferably 70.00 atom % to 80.00 atom %, particularly preferably 75.00 atom % to 80.00 atom %.
[0093] Incidentally, as described later, Ti is preferably used in the production process of the β-sialon phosphor particles of the first embodiment. Ideally, Ti is used only in the production process and does not remain in the final β-sialon phosphor particles, but in practice a small amount of Ti may remain.
[0094] The amount of Ti element N at point P Ti It is preferably 0.50 atom % or less, and more preferably 0.20 atom % or less. Ti Ideally it is zero (amount below the detection limit).
[0095] The amount of Ti element N' at point Q Ti It is preferably 0.50 atom% or less, more preferably 0.20 atom% or less, and even more preferably 0.10 atom% or less. N' Ti Ideally it is zero (amount below the detection limit).
[0096] β-Sialon phosphor powder
[0097] The β-Sialon phosphor powder of the first embodiment includes the β-Sialon phosphor particles of the first embodiment.
[0098] The 50% cumulative diameter (D50) in the volume-based cumulative particle size distribution of the β-sialon phosphor powder can be adjusted according to the application of the phosphor and the like.
[0099] D50 is, for example, 0.1 μm to 50 μm, preferably 3 μm to 40 μm, and more preferably 6 μm to 30 μm. D50 can be controlled by adjusting conditions such as heating temperature and heating time during phosphor production, and by performing appropriate pulverization and classification.
[0100] D50 is defined as the particle size at which the cumulative value from the smallest particle size reaches 50% of the total in the distribution curve of the volume-based particle size measured by the laser diffraction scattering method. The distribution curve of the particle size of the phosphor can be obtained according to the particle size distribution measurement method based on the laser diffraction scattering method described in JISR 1629:1997 "Particle size distribution measurement method based on the laser diffraction scattering method for precision ceramic raw materials". The measurement can be performed using a particle size distribution measuring device.
[0101] Specifically, first, 0.1 g of the phosphor to be measured is put into 100 mL of ion exchange water, a small amount of sodium hexametaphosphate is added, and an ultrasonic homogenizer is used to perform a dispersion treatment for 3 minutes to obtain a dispersion liquid. The dispersion liquid is used as a measurement sample, and a particle size distribution measuring device is used to measure the particle size distribution. Then, D50 is determined based on the obtained particle size distribution.
[0102] As a particle size distribution measuring device, for example, "Microtrac MT3300EX II" (product name) manufactured by Microtrac BEL Co., Ltd. can be used. As an ultrasonic homogenizer, for example, "Ultrasonic Homogenizer US-150E" (product name, tip size: Amplitude: 100%, oscillation frequency: 19.5KHz, amplitude: about 31μm).
[0103] <Second embodiment: β-sialon phosphor particles>
[0104] The β-sialon phosphor particles according to the second embodiment have grain boundaries.
[0105] In a cross section including the grain boundary, when a line analysis of the elemental composition of the grain boundary and both sides thereof is performed in a straight line in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the grain boundary on the surface of the particle,
[0106] On the line segment obtained by the line analysis, (i) the point P where the amount of O on the grain boundary shows a peak (O) The amount of Eu at is set to N Eu(O) , (ii) from point P (O) Leave the point Q of 50nm (O) The Eu quantity at is set to N' Eu(O) When N Eu(O) / N' Eu(O) The value is below 2.50.
[0107] In the first embodiment, (i) the Eu amount (N) at "point P where the Eu amount shows a peak" on the grain boundary is determined. Eu ) and (ii) the amount of Eu at point Q 50 nm away from point P (N' Eu In other words, in the first embodiment, the "point P where the Eu amount shows a peak" is set as the "reference position" in the grain boundary observed with a finite width.
[0108] On the other hand, in the second embodiment, (i) the point P at which the amount of O shows a peak on the grain boundary is determined. (O) "Eu amount (N Eu(O) ) and (ii) from point P (O) Leave the point Q of 50nm (O) Eu amount at (N' Eu(O) ) is a β-sialon phosphor particle within a certain range. In other words, in the second embodiment, the point P at which the O amount shows a peak (O) ” is set as the “reference position” in the grain boundary observed with a finite width.
[0109] That is, although the position for measuring the amount of elements such as the amount of Eu is slightly different, the first embodiment is similar to the second embodiment.
[0110] Incidentally, the reason for setting different "reference positions" in the first embodiment and the second embodiment is based on the knowledge of the inventors, etc. Specifically, based on the measurement results of the inventors, etc., in the grain boundary, the point where the Eu amount shows a peak and the point where the O amount shows a peak are not necessarily consistent, and in the grain boundary observed with a limited width, they can be considered as the "center of the grain boundary".
[0111] As described in the first embodiment, it can be said that N Eu(O) / N' Eu(O) The value of 2.5 or less indicates that the amount of Eu in the shallow position of the particle, such as 200 nm in depth, corresponding to the grain boundary is small. That is, the β-sialon phosphor particles of the second embodiment are not prone to unintended light absorption at the grain boundary and its vicinity, and as a result, it is believed that the internal quantum efficiency becomes good.
[0112] N Eu(O) / N' Eu(O) The value of may be 2.50 or less, and is preferably 0 to 3.00, more preferably 0 to 2.00, and still more preferably 0 to 1.50.
[0113] Hereinafter, the description of the β-sialon phosphor particles according to the second embodiment will be continued. Incidentally, as described above, since the first embodiment and the second embodiment are similar, the matters described in the first embodiment can be appropriately applied to the second embodiment.
[0114] The chemical composition of the β-sialon phosphor particles of the second embodiment is the same as that of the first embodiment, and can be composed of the general formula Si 6-z Al z O z N 8-z :Eu 2+ a (0<Z≤4.2, 0.001<a<1.0) indicates.
[0115] In the second embodiment, by viewing the Eu amount based on the O (oxygen) amount, it is possible to more clearly show that the Eu amount in the grain boundaries is small.
[0116] Specifically, point P (O) The amount of oxygen at ΟО(O) , click Q (O) The amount of oxygen at ΟО(O) When (N Eu(O) / N O(O) ) / (N' Eu(O) / N' O(O) ) is preferably 1.20 or less, more preferably 0 to 1.20, further preferably 0 to 1.00, particularly preferably 0 to 0.50, and particularly preferably 0 to 0.30.
[0117] In the second embodiment, since the amount of Eu on the grain boundaries itself is not much compared with other elements, unintended light absorption at the grain boundaries and their vicinities is further suppressed, and the internal quantum efficiency is considered to be further improved.
[0118] Specifically, point P (O) The amount of oxygen at ΟО(O) When N Eu(O) / N O(O) The value of is preferably 0.70 or less, more preferably 0 to 0.70, further preferably 0 to 0.50, particularly preferably 0 to 0.30, and particularly preferably 0 to 0.10.
[0119] In the second embodiment, since the amount of Al on the grain boundary is not much compared with other elements, further improvement of the internal quantum efficiency can be expected.
[0120] Specifically, point P (O) The amount of oxygen at ΟО(O) , point P (O) The amount of aluminum at Al(O) When N Al(O) / N O(O) The value of is preferably 1.00 or less, more preferably 0 to 1.00, and further preferably 0.01 to 1.00.
[0121] In addition, click Q (O) The amount of aluminum at Al(O) When (N Al(O) / N O(O) ) / (N' Al(O) / N' O(O) ) is preferably 0.45 or less, preferably 0 to 0.45, more preferably 0 to 0.30, and particularly preferably 0.005 to 0.25.
[0122] In addition, N Al(O) / N' Al(O) The value of is preferably 1.10 or less, more preferably 0.1 to 1.10, further preferably 0.50 to 1.10, particularly preferably 0.75 to 1.10.
[0123] N Eu(O) The value is usually 1.50 atom % or less, preferably 0 atom % to 1.00 atom %, more preferably 0 atom % to 0.50 atom %, further preferably 0 atom % to 0.30 atom %.
[0124] N' Eu(O) The value of N' Eu same.
[0125] N ΟО(O) The value is usually 1.00 atom % to 50.0 atom %, preferably 1.00 atom % to 45.0 atom %, and more preferably 1.00 atom % to 40.0 atom %.
[0126] N' ΟО(O) The value of N' ΟО same.
[0127] N Al(O) The value is usually 0.10 atom % to 10.00 atom %, preferably 0.10 atom % to 5.00 atom %, and more preferably 0.10 atom % to 3.00 atom %.
[0128] N' Al(O) The value of N' Al same.
[0129] Point P (O) The amount of N elements at N(O) It is usually 5.00 atom % to 40.00 atom %, preferably 5.00 atom % to 30.00 atom %, and more preferably 5.00 atom % to 25.00 atom %.
[0130] The β-Sialon phosphor powder of the second embodiment includes the β-Sialon phosphor particles of the second embodiment.
[0131] The 50% cumulative diameter (D50) in the volume-based cumulative particle size distribution of the β-Sialon phosphor powder of the second embodiment may be the same as that of the β-Sialon phosphor powder of the first embodiment.
[0132] <Method for producing β-sialon phosphor particles>
[0133] The β-Sialon phosphor particles of the first embodiment and the β-Sialon phosphor particles of the second embodiment can be produced by using appropriate raw materials and adopting appropriate production methods and production conditions.
[0134] A preferred production method is to add a small amount of titanium oxide (Ti2O3) to the β-sialon phosphor and perform annealing, thereby reducing the amount of Eu in the grain boundaries.
[0135] The details of this mechanism are not yet clear, but based on the past views of the present inventors, it is believed that by such annealing, a compound containing Eu and Ti is generated at the grain boundary and its vicinity of the phosphor particles. Then, it is removed by the acid treatment described later, so it is believed that the amount of Eu at the grain boundary and its vicinity is controlled.
[0136] Furthermore, since (ii) a compound containing Al and Ti is generated in addition to (i) a compound containing Eu and Ti, it is considered that the amount of Al at the grain boundary and its vicinity is also controlled.
[0137] An example of a manufacturing method may be a method comprising the following steps:
[0138] a calcination step of obtaining a calcined body containing β-sialon from a raw material composition containing a silicon source, an aluminum source, and a europium source and containing at least one of them as a nitride by one or more heat treatments; and
[0139] The annealing step is to obtain an annealed body from a mixture containing the above-mentioned calcined body and titanium oxide (Ti2O3) by performing one or more annealing treatments in an atmosphere containing at least one selected from a rare gas, a reducing gas and an inert gas.
[0140] This example is described below.
[0141] The raw material composition includes a compound having an element that is a constituent element of β-sialon including europium, and may contain at least a silicon source, an aluminum source, and a europium source.
[0142] In the raw material composition, at least one of the silicon source, the aluminum source and the europium source is a nitride. Nitride is also a nitrogen source because it contains nitrogen, which is a constituent element of β-Sialon. Silicon source refers to a compound or a single substance with silicon as a constituent element, aluminum source refers to a compound or a single substance with aluminum as a constituent element, and europium source refers to a compound or a single substance with europium as a constituent element. In this specification, compounds with silicon as a constituent element are also referred to as silicon compounds, compounds with aluminum as a constituent element are also referred to as aluminum compounds, and compounds with europium as a constituent element are also referred to as europium compounds. Silicon compounds, aluminum compounds and europium compounds can be any one of nitrides, oxides, oxynitrides and hydroxides, respectively. In addition, the raw material composition can further contain β-Sialon or β-Sialon containing europium. Here, β-Sialon or β-Sialon containing europium is a material that becomes an aggregate or a core.
[0143] As silicon compounds, for example, silicon nitride (Si3N4), silicon oxide (SiO2) and the like can be cited. As silicon nitride, it is preferred to use silicon nitride with a high α fraction. As the α fraction of silicon nitride, for example, it can be 80% by mass or more, 90% by mass or more, or 95% by mass or more. If the α fraction of silicon nitride is within the above range, primary particle growth can be promoted. As silicon nitride, it is preferred to use silicon nitride with a small oxygen content. The oxygen content of silicon nitride can be, for example, less than 3.0% by mass or less than 1.3% by mass. If the oxygen content of silicon nitride is within the above range, the generation of defects in the crystal of β-sialon can be suppressed.
[0144] Examples of the aluminum compound include aluminum nitride (AlN), aluminum oxide (Al 2 O 3 ), and aluminum hydroxide (Al(OH) 3 ).
[0145] Examples of europium compounds include europium oxides (europium oxide), europium nitrides (europium nitrides), and europium halides. Examples of europium halides include europium fluoride, europium chloride, europium bromide, and europium iodide. The europium compound preferably includes europium oxide. The valence of europium in the europium compound may be divalent or trivalent, preferably divalent.
[0146] The raw material mixture can be prepared by weighing each compound and mixing. Mixing can be performed by dry mixing or wet mixing. For example, the dry mixing method can be a method of mixing the components using a V-type mixer. For example, the wet mixing method can be a method of adding a solvent or dispersant such as water to prepare a solution or slurry, mixing the components, and then removing the solvent or dispersant.
[0147] The heating temperature in the calcining step is, for example, 1800 to 2500°C, 1800 to 2400°C, 1850 to 2100°C, 1900 to 2100°C, 1900 to 2050°C, or 1920 to 2050°C.
[0148] By setting the heating temperature in the calcining step to 1800°C or higher, the particle growth of β-Sialon can be promoted and the solid solution amount of europium can be more sufficient. By setting the heating temperature in the calcining step to 2500°C or lower, the decomposition of β-Sialon crystals can be sufficiently suppressed.
[0149] The heating time in the calcination step is preferably as long as possible from the viewpoint of promoting the primary particle growth of β-sialon, but if the heating time is too long, crystal defects may increase. Therefore, the heating time is, for example, 1 to 30 hours, 3 to 25 hours, or 5 to 20 hours.
[0150] The heating of the raw material mixture in the calcining process is carried out, for example, under a nitrogen atmosphere. By heating under conditions of high nitrogen partial pressure, the decomposition of silicon nitride at high temperatures can be suppressed. In addition, by treating at high temperatures, particle growth can be promoted. The heating of the raw material mixture in the calcining process is carried out, for example, under pressure. The pressure at this time can be, for example, 0.010 to 200 MPaG, 0.020 to 200 MPaG, 0.1 to 200 MPaG, 0.1 to 100 MPaG, 0.1 to 50 MPaG, 0.1 to 15 MPaG or 0.1 to 5 MPaG.
[0151] The number of times of heat treatment in the calcination step may be once, twice or more, 2 to 5, or 2 to 4. By performing heat treatment multiple times, a β-sialon phosphor having a higher emission intensity can be obtained.
[0152] In the calcination process, more than one heat treatment is performed. However, when multiple heat treatments are performed, they can be sequentially referred to as the first heat treatment, the second heat treatment, etc., and the processes for performing each heat treatment are sequentially referred to as the first calcination process, the second calcination process, etc. For example, when the above-mentioned manufacturing method performs two heat treatments in the calcination process, it can also be said that the calcination process includes: a process of performing a first heat treatment on the raw material composition containing nitride to obtain a first heat-treated body, and a second calcination process of performing a second heat treatment on the above-mentioned first heat-treated body to obtain a second heat-treated body. Moreover, in this case, the second heat-treated body is equivalent to a calcined body containing β-sialon. Before performing multiple heat treatments, the silicon source, aluminum source and europium source can be further mixed and heat-treated.
[0153] When the calcining process includes more than 2 heat treatments, the heating temperature, heating time, atmosphere during heating and pressure during heating of the first calcining process can be respectively applied to the heating temperature, heating time, atmosphere during heating and pressure during heating in the above-mentioned heating process. Moreover, the heating temperature, heating time, atmosphere during heating and pressure during heating after the second calcining process can be the same as or different from the first calcining process. However, even if the heating temperature, heating time, atmosphere during heating and pressure during heating after the second calcining process are different from those of the first calcining process, they are within the range of the conditions shown for the above-mentioned heating process.
[0154] The calcined body obtained in the calcining step is a crystal having β-sialon, and a solid solution of an element serving as a luminescence center is solid-dissolved in a part thereof, and the solid solution itself can emit fluorescence. The calcined body obtained by the calcining step sometimes becomes a block, so the particle size can also be adjusted by crushing or the like before the annealing step.
[0155] Next, an annealing step is performed. The annealing step in the manufacturing method of this example refers to a step of annealing a mixture containing the calcined body obtained in the above-mentioned calcining step and titanium oxide (Ti2O3). In the annealing step, an annealed body is obtained from the mixture through one or more heating treatments.
[0156] The amount of titanium oxide (Ti2O3) added may be, for example, 0.01 to 4 mass %, 0.05 to 3 mass %, or 0.1 to 3 mass % relative to the total amount of the mixture.
[0157] By setting the above-mentioned blending amount to 0.01 mass % or more, excess Eu and Al in the grain boundaries can be sufficiently removed, and the internal quantum efficiency of the obtained β-sialon phosphor can be further improved.
[0158] By setting the blending amount to 4% by mass or less, titanium oxide and various products can be easily removed by acid treatment, and degradation of the light emitting characteristics of the β-sialon phosphor can be suppressed.
[0159] The annealing step is performed in an atmosphere containing at least one selected from a rare gas, a reducing gas, and an inert gas. By performing the annealing in an atmosphere containing a rare gas, a reducing gas, or an inert gas, the ratio of divalent europium in the europium solid solution can be increased.
[0160] The above-mentioned rare gas may contain argon, helium, etc., may contain argon, or may be composed of argon. The above-mentioned reducing gas may contain ammonia, hydrocarbons, carbon monoxide, hydrogen, etc., may contain hydrogen, or may be composed of hydrogen. The inert gas may contain nitrogen, etc., or may be composed of nitrogen. The atmosphere of the annealing process may also be a mixed gas of two or more of the above-mentioned rare gas, the above-mentioned reducing gas and the inert gas. When the atmosphere of the annealing process is the above-mentioned mixed gas, the content of the above-mentioned reducing gas is based on the total volume of the mixed gas, for example, it can be 1 to 50 volume % or 4 to 20 volume %. The content of the above-mentioned inert gas is based on the total volume of the mixed gas, for example, it can be 1 to 50 volume % or 4 to 20 volume %.
[0161] The pressure during the annealing treatment may be the same as the pressure during the calcining step, but is preferably lower than the pressure during the calcining step, and more preferably atmospheric pressure.
[0162] The temperature of the annealing treatment needs to be set lower than the heating temperature in the calcining process. The upper limit of the temperature of the annealing treatment is, for example, below 1700°C, preferably below 1680°C. By setting the upper limit of the temperature of the annealing treatment within the above range, it is possible to inhibit further particle growth in the calcined body, agglomerate between solid solutions, form secondary particles, and coarsen the particles. The lower limit of the temperature of the annealing treatment is, for example, above 1000°C, above 1100°C, above 1200°C, above 1300°C, or above 1400°C. By setting the lower limit of the temperature of the annealing treatment within the above range, the crystal defect density of the β-sialon contained in the annealed body can be reduced, further improving the internal quantum efficiency. The temperature of the annealing treatment can be adjusted within the above range, for example, 1000-1700°C or 1100-1680°C.
[0163] From the viewpoint of further reducing crystal defects in the phosphor included in the annealed body, the heating time in the annealing treatment may be, for example, 1 to 30 hours, 2 to 25 hours, or 3 to 20 hours.
[0164] In the annealing process, the annealing treatment is performed more than once, but when the annealing treatment is performed multiple times, it can be sequentially referred to as the first annealing treatment, the second annealing treatment, etc., and the steps for performing each annealing treatment are sequentially referred to as the first annealing process, the second annealing process, etc. For example, when the above-mentioned manufacturing method performs two annealing treatments in the annealing process, it can also be said that the annealing process includes: a step of performing a first annealing treatment on the calcined body to obtain a first annealed body, and a second annealing process of performing a second annealing treatment on the first annealed body to obtain a second annealed body. Moreover, in this case, the second annealed body is equivalent to the above-mentioned annealed body.
[0165] When the annealing process includes more than two annealing processes, the temperature, heating time and pressure of the annealing process in the first annealing process can be respectively applied to the temperature, heating time and pressure of the annealing process in the above annealing process. Moreover, the temperature, heating time and pressure of the annealing process after the second annealing process can be the same as or different from the first annealing process. Among them, even if the temperature, heating time and pressure of the annealing process after the second annealing process are different from those of the first annealing process, they are within the range of the conditions shown for the above annealing process.
[0166] The number of annealing treatments in the annealing step may be 1, for example, 2, 2 to 5, or 2 to 4. By performing multiple annealing treatments, the crystal defect density of β-sialon contained in the annealed body can be reduced, and a europium-containing β-sialon phosphor with better internal quantum efficiency can be obtained.
[0167] When multiple annealing treatments are performed in the annealing process, titanium oxide (Ti2O3) can be combined in the first annealing process, or it can be combined in batches in the multiple annealing processes. Among them, it is preferably combined in the first annealing process. By the way, when these compounds are combined in batches, the description of the amount of titanium oxide (Ti2O3) is replaced by the total amount of titanium oxide (Ti2O3) combined in the multiple annealing processes. In the annealing process, the compound of the constituent element of the β-type sialon phosphor can be added together with titanium oxide (Ti2O3).
[0168] The method for manufacturing a β-sialon phosphor may include other steps in addition to the calcining step and the annealing step. As other steps, for example, a step of treating the annealed body obtained in the annealing step with at least one of an acid and an alkali, a classification step of adjusting the particle size of the annealed body or the annealed body treated with an acid, etc. The step of treating the annealed body with an acid is referred to as an acid treatment step, and the step of treating the annealed body with an alkali is referred to as an alkali treatment step.
[0169] Through the acid treatment step or the alkali treatment step, for example, it is expected that the crystal defect density in the phosphor contained in the annealed body is further reduced, silicon existing on the surface of the solid solution generated by thermal decomposition of β-sialon is removed, and pseudo-polymorphs of aluminum nitride (AlN), i.e., AlN polytypes (Polytipoid), etc., which are by-produced during the preparation of the first calcined body, are removed. The acid includes, for example, hydrofluoric acid and nitric acid. The acid may be a mixed acid of hydrofluoric acid and nitric acid. The alkali includes, for example, sodium hydroxide.
[0170] The classification process may be performed by, for example, a wet classification method or a dry classification method. As wet classification, for example, an elutriation classification method in which the annealed body is added to a mixed solvent containing ion exchange water and a dispersant (e.g., sodium hexametaphosphate, etc.), or a mixed solvent containing ion exchange water and ammonia water, and stirred and then allowed to stand to remove particles with a small particle size may be cited.
[0171] <Light-emitting device>
[0172] The light emitting device of this embodiment is a light emitting device including a light source and a wavelength conversion component. The wavelength conversion component includes a phosphor. Moreover, the phosphor includes the β-sialon phosphor powder of the first embodiment and / or the β-sialon phosphor powder of the second embodiment.
[0173] Figure 1 2 is a cross-sectional view schematically showing an example of the structure of the light emitting device 10 .
[0174] Figure 1 The light emitting device 10 shown is composed of an LED chip as a light source 12, a first lead frame 13 carrying the light source 12, a second lead frame 14, a wavelength conversion component 15 covering the light source 12, a bonding wire 16 electrically connecting the light source 12 and the second lead frame 14, and a cover 19 made of synthetic resin covering them. The wavelength conversion component 15 has a phosphor 18 and a sealing resin 17 in which the phosphor 18 is dispersed.
[0175] A recess 13b for mounting a light emitting diode chip as the light emitting source 12 is formed on the upper portion 13a of the first lead frame 13. The recess 13b has a substantially funnel shape with a diameter gradually expanding from its bottom surface toward the top, and the inner surface of the recess 13b is a reflective surface. An electrode on the lower surface side of the light emitting source 12 is chip-bonded to the bottom surface of the reflective surface. Another electrode formed on the upper surface of the light emitting source 12 is connected to the surface of the second lead frame 14 via a bonding wire 16.
[0176] Various LED chips can be used as the light source 12. In particular, an LED chip that generates light with a wavelength of 300 nm to 500 nm as near-ultraviolet to blue light is preferred.
[0177] The phosphor 18 of the wavelength conversion component 15 for the light emitting device 10 includes the β-Sialon phosphor powder of the first embodiment and / or the β-Sialon phosphor powder of the second embodiment. In addition, from the perspective of controlling the wavelength of light of the light emitting device 10, the phosphor 18 may further include phosphors such as α-Sialon phosphor, KSF-based phosphor, CaAlSiN3, and a monomer or mixture of YAG in addition to the β-Sialon phosphor powder of the first embodiment and / or the β-Sialon phosphor powder of the second embodiment. As elements dissolved in these phosphors, for example, europium (Eu), cerium (Ce), strontium (Sr), calcium (Ca), manganese (Mn), etc. can be cited. These phosphors can be used alone or in combination of two or more.
[0178] Among these, as a phosphor used in combination with the β-sialon phosphor powder of the first embodiment and / or the β-sialon phosphor powder of the second embodiment, a KSF-based phosphor having manganese dissolved therein is preferred. By using a β-sialon phosphor that displays green and a KSF-based phosphor that displays red in combination, for example, it can be appropriately used as a backlight LED suitable for a high color rendering television or the like.
[0179] By combining the luminescent light source 12 with the wavelength conversion member 15, light having high luminous intensity can be emitted.
[0180] If we record it for the sake of caution, the KSF series phosphor with manganese solid solution can be represented by the general formula: A2M (1-n) F6:MN 4+ n In the general formula, element A is one or more alkali metal elements including K, element M is Si single substance, Ge single substance, or a combination of Si and one or more elements selected from Ge, Sn, Ti, Zr and Hf, and 0<n≤0.1.
[0181] In the case of the light emitting device 10 using a β-sialon phosphor, near-ultraviolet light or visible light having a wavelength of 300nm to 500nm is used as an excitation source as the light emitting light source 12, thereby having a green light emitting characteristic having a peak at a wavelength in the range of 520nm to 560nm. Therefore, by using a near-ultraviolet LED chip or a blue LED chip and the β-sialon phosphor of the present embodiment as the light emitting light source 12, and further combining a single body or a mixed body of a red light emitting phosphor, a blue light emitting phosphor, a yellow light emitting phosphor, or an orange light emitting phosphor having a wavelength of 600nm to 700nm, white light can be formed.
[0182] The embodiments of the present invention have been described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above-mentioned embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are included in the present invention.
[0183] Example
[0184] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, it is to be noted that the present invention is not limited to the Examples.
[0185] <Production of β-sialon phosphor particles>
[0186] [Example 1]
[0187] The following steps (1) to (4) were carried out.
[0188] (1) Raw material mixing process
[0189] Each raw material was weighed in a container so that silicon nitride (Si3N4) was 95.7 mass%, aluminum nitride (AlN) was 2.6 mass%, aluminum oxide (Al2O3) was 1.0 mass%, and europium oxide (Eu2O3) was 0.7 mass%, and mixed using a V-type mixer (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.) to obtain a mixture. The obtained mixture was completely passed through a sieve with a mesh of 250 μm to remove agglomerates, thereby obtaining a raw material composition. The agglomerates that did not pass through the sieve were crushed and the particle size was adjusted so as to pass through the sieve.
[0190] (2) Calcination process
[0191] 200 g of the above-mentioned raw material composition is placed in a cylindrical boron nitride container with a lid (manufactured by Denka Co., Ltd., a molded product with boron nitride (trade name: Denka Boron Nitride N-1) as the main component, inner diameter: 10 cm, height: 10 cm). Then, the container is placed in an electric furnace equipped with a carbon heater, heated to 2020°C under a nitrogen atmosphere (pressure: 0.90 MPaG), and heated at a heating temperature of 2020°C for 8 hours (calcination process). After heating, the sample that slowly condenses in the above-mentioned container into a block is collected in a mortar and crushed. After crushing, it is passed through a sieve with a mesh of 250 μm and strongly crushed. In this way, a first calcined body in powder form is obtained.
[0192] (3) Annealing process
[0193] The first calcined body was mixed with titanium oxide (Ti2O3) to obtain a mixture for annealing treatment. The amount of titanium oxide was 0.1 parts by mass when the total amount of the first calcined body and titanium oxide was 100 parts by mass.
[0194] Then, the mixture for annealing treatment is filled into a cylindrical boron nitride container. The container is placed in an electric furnace equipped with a carbon heater. The temperature is raised to 1450°C under an argon atmosphere (pressure: 0.025 MPaG), and heating is performed at a temperature of 1450°C for 3 hours (annealing process). After heating, the lumps slowly condensed in the container are crushed with mortar particles and passed through a 250 μm sieve to obtain a powder.
[0195] (4) Acid treatment, fine powder removal and other processes
[0196] The obtained powder is added to a mixed acid (acid in which hydrofluoric acid and nitric acid are mixed in a volume ratio of 1:1) of hydrofluoric acid (concentration: 50% by mass) and nitric acid (concentration: 70% by mass), and the acid treatment is performed for 30 minutes while stirring at a temperature of 75°C. After the acid treatment, the stirring is stopped to allow the powder to settle, and the supernatant and the fine powder purified by the acid treatment are removed. Then, distilled water is further added and stirred again. The stirring is stopped to allow the powder to settle, and the supernatant and fine powder are removed. Repeat this operation until the supernatant becomes transparent when the pH of the aqueous solution is below 8, and the obtained precipitate is filtered and dried.
[0197] Through the above operation, β-Sialon phosphor powder including Eu-activated β-Sialon phosphor particles was obtained.
[0198] [Example 2]
[0199] A β-sialon phosphor powder was obtained in the same manner as in Example 1 except that the final pulverization in the calcination step (2) was performed with weak pulverization instead of strong pulverization.
[0200] [Example 3]
[0201] (3) In the annealing step, the β-sialon phosphor powder was obtained in the same manner as in Example 1 except that the amount of titanium oxide added was changed from 0.1 part by mass to 0.2 part by mass.
[0202] [Comparative Example 1]
[0203] In the (3) annealing step, titanium oxide was not used and only the first calcined body was heated for annealing. A β-sialon phosphor powder was obtained in the same manner as in Example 1.
[0204] [Comparative Example 2]
[0205] A β-sialon phosphor powder was obtained in the same manner as in Example 1 except that an equal amount of europium oxide was added instead of titanium oxide to perform annealing in the annealing step (3).
[0206] [Comparative Example 3]
[0207] In the (3) annealing step, titanium oxide was not used and only the first calcined body was heated for annealing. A β-sialon phosphor powder was obtained in the same manner as in Example 2.
[0208] <Line Analysis>
[0209] Proceed through the following steps.
[0210] (1) A sample was prepared in which β-sialon phosphor powder was embedded in epoxy resin.
[0211] (2) The sample prepared in (1) above was placed in a cross-section polisher (SM-09010 manufactured by JEOL Ltd.) and processed at an accelerating voltage of 6 kV. This exposed the cross-section of the embedded β-sialon phosphor particles.
[0212] (3) The cross section exposed in (2) above is observed using a SEM (field emission type, accelerating voltage 5 kV) to identify a portion where a grain boundary suitable for analysis exists (grain boundary having a length of at least 200 nm from the particle surface and being approximately linear). This portion and its surroundings are sliced using a focused ion beam (FIB) processing device to prepare a thin slice sample.
[0213] (4) In the thin-section sample (including the cross section of the grain boundary), the elemental composition of the grain boundary and both sides thereof was analyzed in a straight line in a direction perpendicular to the grain boundary at a depth of 200 nm from the grain boundary portion of the surface of the particle. The line analysis was performed using JEM-ARM200F (a device that combines a scanning transmission electron microscope (STEM) with an apparatus capable of performing energy dispersive X-ray analysis (EDS)) manufactured by JEOL Ltd. The accelerating voltage was 200 kV.
[0214] (5) Based on the results of line analysis, the amount of each element at each point such as point P (unit: atom%) is determined. The amount of each element (unit: atom%) is determined by analysis using the software attached to JEM-ARM200F, namely "NORAN System 7" manufactured by Thermo Fisher Scientific. In this analysis, Si, N, Al, O, Ti (K-ray), and Eu (L-ray) are specified as the elements to be considered. In addition, the Cliff-Lorimer (absorption-free) model is specified as a semi-quantitative model.
[0215] Then, calculate N based on the amount of each element found. Eu / N' Eu The "ratio" of equal amounts of elements.
[0216] For reference, the position where the line analysis of (4) was performed in the flake sample obtained by flake-forming the β-sialon phosphor particles of Example 1 as described in (1) to (3) above is shown in FIG. Figure 2 Similarly, in the thin-sheet sample obtained by thinning the β-sialon phosphor particles of Comparative Example 1 as described in (1) to (3), the position where the line analysis (4) was performed is shown in FIG. Figure 3 .
[0217] The amount of each element at each point (unit: atom%) and N Eu / N' Eu The ratios of the elements are summarized in Table 1.
[0218] It should be noted that in a region sufficiently away from the grain boundary (about 50 nm), even if the measurement point is offset by a few nm, there is no significant difference in the elemental composition. (O) The amount of each element measured at the position is regarded as the amount of each element at point Q.
[0219] [Table 1]
[0220]
[0221] <Evaluation of internal quantum efficiency, etc.>
[0222] The β-sialon phosphors obtained in the examples and comparative examples were evaluated for absorptivity, internal quantum efficiency, external quantum efficiency, and chromaticity X when irradiated with excitation light of a wavelength of 455 nm. In addition, absorptivity when irradiated with excitation light of a wavelength of 600 nm was also evaluated. The specific evaluation method is as follows.
[0223] [Absorption rate, internal quantum efficiency and external quantum efficiency]
[0224] The absorptivity (excitation light absorptivity), internal quantum efficiency, and external quantum efficiency of the fluorescent body when irradiated with an excitation light of a wavelength of 455 nm are calculated by the following steps. First, the fluorescent body to be measured is filled in a concave cell in a manner that makes the surface smooth, and is installed in the opening of an integrating sphere. Monochromatic light with a wavelength of 455 nm split by a Xe lamp as a light source is introduced into the above-mentioned integrating sphere using an optical fiber as the excitation light for the fluorescent body. The fluorescent body to be measured is irradiated with the monochromatic light as the excitation light, and the fluorescence spectrum is measured. The measurement is performed using a spectrophotometer (manufactured by Otsuka Electronics Co., Ltd., trade name: MCPD-7000).
[0225] The luminous intensity of the phosphor is determined based on the data of the obtained fluorescence spectrum. In addition, the number of excitation reflected light photons (Qref) and the number of fluorescence photons (Qem) are calculated based on the data of the obtained fluorescence spectrum. The number of excitation reflected light photons is calculated within the same wavelength range as the number of excitation light photons, and the number of fluorescence photons is calculated within the range of 465 to 800 nm. In addition, using the same device, a standard reflector with a reflectivity of 99% (manufactured by Labsphere, Spectralon (registered trademark)) is installed at the opening of the integrating sphere to measure the spectrum of the excitation light with a wavelength of 455 nm. At this time, the number of excitation light photons (Qex) is calculated based on the spectrum in the wavelength range of 450 to 465 nm.
[0226] From the above calculation results, the absorptivity of the 455 nm excitation light, the internal quantum efficiency, and the external quantum efficiency of the phosphor to be measured were determined based on the calculation formula shown below.
[0227] Absorption rate of 455nm excitation light = ((Qex-Qref) / Qex) × 100
[0228] Internal quantum efficiency = (Qem / (Qex-Qref))×100
[0229] External quantum efficiency = (Qem / Qex) × 100
[0230] In addition, based on the above formula, the relationship between the external quantum efficiency, the absorptivity of the excitation light of 455 nm, and the internal quantum efficiency can be expressed as follows.
[0231] External quantum efficiency = 455nm light absorption rate × internal quantum efficiency
[0232] [Chroma X, Chroma Y]
[0233] Chromaticity X and chromaticity Y are obtained by calculating the CIE chromaticity coordinate x value (chromaticity X) and y value (chromaticity Y) in the XYZ colorimetric system specified in JIS Z8781-3:2016 based on spectral data in the wavelength range of 465 to 780 nm of the fluorescence spectrum in accordance with JIS Z8724:2015.
[0234] [600nm light absorption rate]
[0235] A standard reflector plate with a reflectivity of 99% (Spectralon (registered trademark) manufactured by Labsphere) was set at the side opening of the integrating sphere. Monochromatic light with a wavelength of 600 nm from a light source (Xe lamp) was introduced into the integrating sphere through an optical fiber, and the reflected light spectrum was measured using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.). At this time, the number of incident light photons (Qex(600)) was calculated based on the spectrum in the wavelength range of 590 to 610 nm.
[0236] Next, the β-sialon phosphor is filled in a concave cell in a manner that the surface becomes smooth, and is set at the opening of an integrating sphere. Then, monochromatic light with a wavelength of 600nm is irradiated, and the incident reflected light spectrum is measured using a spectrophotometer. The incident reflected light photon number (Qref(600)) is calculated based on the obtained spectral data. The incident reflected light photon number (Qref(600)) is calculated within the same wavelength range as the incident light photon number (Qex(600)). Based on the two obtained photon numbers, the 600nm light absorptivity is calculated based on the following formula.
[0237] 600nm light absorption rate = ((Qex(600) - Qref(600)) / Qex(600)) × 100
[0238] <Determination of D50>
[0239] The D50 of the β-sialon phosphor of each example and comparative example was measured. The specific procedure and conditions of the measurement are as described above.
[0240] Table 2 shows the evaluation and measurement results in summary.
[0241] [Table 2]
[0242]
[0243] As shown in Tables 1 and 2, N Eu / N' Eu The value is 3.00 or less and / or N Eu(O) / N' Eu(O) The internal quantum efficiency of Examples 1 to 3 with a value of 2.50 or less is N Eu / N' Eu The value of N is greater than 3.00 and / or Eu(O) / N' Eu(O) The internal quantum efficiency of Comparative Examples 1 to 3 in which the value of is larger than 2.50 is good.
[0244] In addition, from the difference in the manufacturing method between the embodiment and the comparative example, it can be understood that the annealing treatment using titanium oxide is used to obtain N Eu / N' Eu The value is 3.00 or less and / or NEu(O) / N' Eu(O) A preferred method for producing β-sialon phosphor particles having a value of 2.50 or less.
[0245] This application claims the benefit of priority based on Japanese patent application No. 2022-034169, filed on March 7, 2022, the disclosure of which is incorporated herein in its entirety.
[0246] Explanation of symbols
[0247] 10 Lighting device
[0248] 12 Light source (LED chip)
[0249] 13 1st lead frame
[0250] 13a upper part
[0251] 13b recess
[0252] 14 2nd lead frame
[0253] 15. Wavelength conversion components
[0254] 16 Bonding wire
[0255] 17 Sealing resin
[0256] 18 Phosphor (β-sialon phosphor particles)
[0257] 19 Hood
Claims
1. A β-sialon phosphor particle, which is a Eu-activated β-sialon phosphor particle having a grain boundary, In a cross section including the grain boundary, when a linear analysis of the elemental composition of the grain boundary and both sides thereof is performed in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the particle surface where the grain boundary exists, On the line segment obtained by the line analysis, (i) the Eu amount at the point P where the Eu amount on the grain boundary shows a peak is set to N Eu (ii) The amount of Eu at point Q, which is 50 nm away from point P, is N' Eu When N Eu / N' Eu The value is below 3.
00.
2. The β-sialon phosphor particle according to claim 1, wherein The amount of oxygen at point P is N ΟО , let the amount of oxygen at point Q be N' ΟО When (N Eu / N O ) / (N Eu ' / N O ') is less than 2.
00.
3. The β-sialon phosphor particle according to claim 1 or 2, wherein The amount of oxygen at point P is N ОΟ When N Eu / N O The value is below 0.
70.
4. The β-sialon phosphor particle according to any one of claims 1 to 3, wherein The amount of oxygen at point P is N ΟО , When the elemental composition of the grain boundary and its both sides is linearly analyzed in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the particle surface where the grain boundary exists, the point P where the Al amount on the grain boundary shows a peak is set on the line segment obtained by the linear analysis. (Al) The Al content at N Al hour, N Al / N O The value of is less than 1.
00.
5. A β-sialon phosphor particle, which is a Eu-activated β-sialon phosphor particle having a grain boundary, In a cross section including the grain boundary, when a linear analysis of the elemental composition of the grain boundary and both sides thereof is performed in a direction perpendicular to the grain boundary at a depth of 200 nm from the portion of the particle surface where the grain boundary exists, On the line segment obtained by the line analysis, (i) the point P where the amount of O on the grain boundary shows a peak value is (O) The amount of Eu at is set to N Eu(O) , (ii) from point P (O) Leave the point Q of 50nm (O) The Eu quantity at is set to N' Eu(O) When N Eu(O) / N' Eu(O) The value is below 2.
50.
6. The β-sialon phosphor particle according to claim 5, wherein Point P (O) The amount of oxygen at ΟО(O) , click Q (O) The amount of oxygen at ΟО(O) When (N Eu(O) / N O(O) ) / (N' Eu(O) / N' O(O) ) is less than 1.
20.
7. The β-sialon phosphor particle according to claim 5 or 6, wherein Point P (O) The amount of oxygen at ΟО(O) When N Eu(O) / N O(O) The value is below 0.
70.
8. The β-sialon phosphor particle according to any one of claims 5 to 7, wherein Point P (O) The amount of oxygen at ΟО(O) , point P (O) The amount of aluminum at Al(O) When N Al(O) / N O(O) The value of is less than 1.
00. 9 . A β-Sialon phosphor powder comprising the β-Sialon phosphor particles according to claim 1 .
10. A light emitting device comprising a light source and a wavelength conversion component, The wavelength conversion component includes phosphor powder, The phosphor powder includes the β-sialon phosphor powder according to claim 9.
11. The light emitting device according to claim 10, wherein: The light source includes an LED chip that generates light with a wavelength of 300 nm to 500 nm.
Citation Information
Patent Citations
Europium-activated beta-sialon phosphor and light-emitting device
CN116018388A
Europium-activated beta-sialon phosphor and light-emitting device
CN118995205A