Steel sheet having excellent bendability and high strength press hardened

CN118786236AActive Publication Date: 2024-10-15VALIN ARCELORMITTAL AUTOMOTIVE STEEL CO LTD +1

Patent Information

Application Number
CN202480001634.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-30
Filing Date
2024-04-25
Publication Date
2024-10-15
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing high-strength steel components are prone to cracking under bending loads, resulting in poor crashworthiness, making it difficult to achieve both high mechanical strength and high impact resistance, and the need for weight reduction is difficult to achieve without neglecting safety.

Method used

The steel plate is prepared through hot stamping technology, and the chemical composition and microstructure of the steel plate are controlled to ensure that it has a tensile strength higher than or equal to 1300MPa and a transverse bending angle greater than 48° after hot stamping, using a specific refining process and heat treatment process To control the inclusion group and improve the bendability and weldability of the steel plate.

Benefits of technology

High mechanical resistance and excellent energy absorption capabilities of steel components are achieved, improving vehicle safety and fuel efficiency while controlling steel plate costs and processing issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786236A_ABST
    Figure CN118786236A_ABST
Patent Text Reader

Abstract

A steel sheet having a chemical composition comprising, in weight%, C: 0.2% to 0.4%, Mn: 0.8% to 2.0%, Si: 0.1% to 0.5%, Al: 0.01% to 0.1%, Ti: 0.01% to 0.1%, B: 0.0005% to 0.005%, P < = 0.040%, Ca < = 0.01%, S < = 0.006%, N < = 0.01%, the steel sheet comprising, from the main body to the surface of the coated steel sheet, the main body and a surface layer occupying 10% of the outermost thickness on both sides of the main body, the top of such a body is a skin layer occupying 10% of the thickness of the outermost surface on both sides of the body, the density of TiN / Ti (C, N) inclusions in the skin layer being less than 240 particles / mm2, and the clustering index of MnS inclusions in the skin layer being less than 110 [mu] m / mm2. This allows the production of a hot-pressed part having a tensile strength equal to or greater than 1300 MPa and a bending angle strictly greater than 48 degrees standardized to 1.5 mm and measured in the transverse direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to steel sheets and to high strength press hardened steel parts. Background Art

[0002] High-strength press-hardened components can be used as structural elements in motor vehicles for anti-intrusion or energy absorption functions.

[0003] In this type of application, it is desirable to produce steel parts that combine high mechanical strength with high impact resistance. Furthermore, in view of global environmental protection, one of the main challenges in the automotive industry is to reduce the weight of vehicles to improve their fuel efficiency without neglecting safety requirements.

[0004] This weight reduction can be achieved in particular by using steel components with a predominantly martensitic microstructure.

[0005] It is challenging to produce very high strength steels that also have good resistance to the formation of cracks under bending. In fact, very high strength steels tend to crack at an early age when subjected to bending loads. This is detrimental to the crashworthiness of components produced with such high strength steels, because although the material is able to withstand very high loads due to its high tensile strength, once cracks start to appear in the component, these cracks will propagate rapidly under continued load and the component will fail prematurely. Summary of the invention

[0006] The object of the present invention is to solve the above challenges and to provide a press-hardened steel component having a combination of high mechanical properties: a tensile strength after hot stamping higher than or equal to 1300 MPa and a high bending angle measured in the transverse direction of more than 48° when normalized to 1.5 mm thickness.

[0007] Another object of the present invention is to provide a steel sheet which can be transformed into such a press-hardened steel component by hot forming, and to provide a method for manufacturing such a steel sheet.

[0008] The object of the invention is achieved by providing a steel sheet according to claim 1, optionally with the features of claims 2 to 4. Another object of the invention is achieved by providing a press-hardened steel component according to claim 5. The steel component may also comprise the features of claims 6 to 7. Another object of the invention is a method for manufacturing said hot stamped component according to claim 8, optionally with the features of claim 9. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The invention will now be described in detail and by way of non-limiting examples and with reference to Figure 1 To illustrate the present invention by way of example, Figure 1 is a schematic cross section of a steel plate according to the present invention. DETAILED DESCRIPTION

[0010] A steel blank is a flat steel sheet that has been cut into any shape suitable for its use. The blank has a top face and a bottom face, which are also referred to as the top side and the bottom side or as the top surface and the bottom surface. The distance between the faces is designated as the thickness of the blank. The thickness can be measured, for example, using a micrometer, the spindle and the anvil of which are placed on the top and bottom surfaces. In a similar way, the thickness can also be measured on formed parts.

[0011] Hot stamping is a forming technique that involves heating the blank to a temperature at which the microstructure of the steel is at least partially transformed into austenite, forming the blank at high temperature by stamping it, and quenching the formed part to obtain a microstructure with very high strength. Hot stamping allows very high-strength parts with complex shapes to be obtained and presents many technical advantages. It should be understood that the heat treatment to which the part is subjected not only includes the thermal cycle of the hot stamping process itself described above, but may also include other subsequent heat treatment cycles, such as a paint baking step performed after the part has been painted in order to cure the paint. The following mechanical properties of hot stamped parts are those measured after all thermal cycles (optionally including, for example, a paint baking step, where paint baking has indeed been performed).

[0012] The ultimate tensile strength is measured according to ISO standard ISO 6892-1 published in October 2009. The tensile test specimens are cut from a flat area of ​​the hot stamped part. If necessary, undersized tensile test specimens are used to fit the full available flat area on the part.

[0013] The bending angle is measured according to the VDA-238 bending standard. For the same material, the bending angle depends on the thickness. For simplicity, the bending angle values ​​of the present invention refer to a thickness of 1.5 mm. If the thickness is different from 1.5 mm, the bending angle values ​​need to be normalized to 1.5 mm by the following calculation, where α1.5 is the bending angle normalized at 1.5 mm, t is the thickness, and αt is the bending angle for thickness t:

[0014] α1.5=(αt×√t) / √1.5

[0015] In the present invention, the bend angle is measured in the transverse direction (i.e., transverse to the rolling direction along which the steel sheet travels during the hot rolling step). The bend angle is measured using a laser measuring device. The reported value is the value after springback. When the hot stamped part is subjected to a bend test, a sample is cut from a flat area of ​​the part. If necessary, a small size sample is used to accommodate the entire available flat area on the part. If the rolling direction on the hot stamped part is not known, it can be determined using electron backscatter diffraction (EBSD) analysis across a cross section of the sample in a scanning electron microscope (SEM). The rolling direction is determined according to a representative The strength of the orientation density function (ODF) of the main fibers under is the Euler angle as defined in "H.-J. Bunge: Texture Analysis in Materials Science-Mathematical Methods. Butterworth Co. First English Edition (Publication) 1982" (for For the definition of , see Figures 2.2 and 2.3).

[0016] The bend angle of a component represents the ability of the component to resist deformation without forming cracks.

[0017] The composition of the steel according to the invention will now be described, with the contents being expressed in weight percentages. The chemical composition is given with lower and upper limits of the composition range, which are included in the possible composition range according to the invention. Where preferred ranges for a given element are disclosed, the invention also discloses all possible combinations of these preferred ranges for the individual elements.

[0018] According to the present invention, the carbon content is in the range of 0.2% to 0.4% to ensure satisfactory strength. Above 0.4% carbon, the weldability and bendability of the steel sheet may be reduced. If the carbon content is less than 0.2%, the tensile strength will not reach the target value. In a specific embodiment, the carbon content is in the range of 0.2% to 0.3% to ensure sufficient strength while further controlling excellent weldability and bendability. In a specific embodiment, the carbon content is in the range of 0.2% to 0.25% to ensure sufficient strength while even further controlling excellent weldability and bendability.

[0019] The manganese content ranges from 0.8% to 2.0%. Adding above 2.0%, the risk of MnS formation increases, thereby impairing bendability. Below 0.8%, the hardenability of the steel sheet during the hot stamping process is reduced. In a specific embodiment, the manganese content ranges from 1.0% to 1.4% to further improve the hardenability of the steel and further limit the formation of MnS, thereby improving bendability.

[0020] The silicon content ranges from 0.1% to 0.5%. Silicon is an element that participates in the hardening of the solid solution. Silicon is added to limit carbide formation. Above 0.5%, silicon oxides are formed at the surface, which impair the paintability of the steel. In addition, the weldability of parts produced with the steel sheet may be reduced. In a specific embodiment, the silicon content ranges from 0.1% to 0.4% to further improve the paintability and weldability. In a specific embodiment, the silicon content ranges from 0.15% to 0.35% to further harden the steel and further improve the paintability and weldability.

[0021] According to the invention, the aluminum content ranges from 0.01% to 0.1% because it is a very effective element for deoxidizing the steel in the liquid phase during processing. If the titanium content is insufficient, the aluminum can protect the boron. The aluminum content is below 0.1% to avoid oxidation problems and ferrite formation during press hardening. Preferably, the aluminum content ranges from 0.02% to 0.06% to further ensure good deoxidation of the steel in the liquid phase while further avoiding oxidation problems and ferrite formation during press hardening.

[0022] According to the present invention, the titanium content ranges from 0.01% to 0.1% to protect the boron that would otherwise be trapped in the BN precipitates. The titanium content is limited to 0.1% to avoid excessive TiN formation. In a specific embodiment, the Ti content ranges from 0.02% to 0.06% to further protect the boron while further avoiding excessive TiN formation.

[0023] According to the present invention, the boron content ranges from 0.0005% to 0.005%. Boron improves the hardenability of steel. The boron content is not higher than 0.005% to avoid the problem of slab breakage during continuous casting. In a specific embodiment, the boron content ranges from 0.002% to 0.004% to further ensure the hardenability of steel and further avoid the problem of slab breakage.

[0024] Phosphorus is controlled to be less than or equal to 0.040% because it causes brittleness and weldability issues. In a specific embodiment, the P content is controlled to be less than or equal to 0.020% to further avoid brittleness and weldability issues.

[0025] Calcium is controlled to be less than or equal to 0.01% because the presence of calcium in molten steel may lead to the formation of coarse inclusions that are detrimental to bendability. In a specific embodiment, the Ca content is controlled to be less than or equal to 0.005% to further avoid the coarse inclusion problem.

[0026] Sulfur is controlled to be less than or equal to 0.006% because the presence of sulfur in the molten steel may lead to the formation of MnS precipitates that are detrimental to bendability. In a specific embodiment, the S content is controlled to be less than or equal to 0.005% to further avoid the formation of MnS precipitates.

[0027] Nitrogen is controlled to be less than 0.01%, preferably less than or equal to 0.008%, even more preferably less than 0.005%.The presence of nitrogen may lead to the formation of precipitates such as TiN or TiNbCN which are detrimental to bendability.

[0028] Chromium is optionally added up to 0.4%. Chromium can be used to provide strength through solid solution hardening and improve the hardenability of the steel sheet during hot stamping. Chromium is limited to 0.4% to limit costs and avoid processing problems.

[0029] Molybdenum is optionally added up to 0.3%. Molybdenum improves the hardenability of the steel. Molybdenum is limited to 0.3% to limit costs and avoid processing problems.

[0030] Niobium is optionally added up to 0.1%. Niobium improves the ductility of the steel. Niobium is limited to 0.1% to limit costs and avoid processing problems.

[0031] Vanadium is optionally added up to 0.3%. Vanadium improves the hardenability of the steel. Vanadium is limited to 0.3% to limit costs and avoid processing problems.

[0032] In the case of adding one or more of the above elements, the following formula is further verified: Cr+Mo+Nb+V≤0.5% to limit costs and avoid processing problems.

[0033] In a specific embodiment, the chemical composition is further controlled so as to verify the following conditions:

[0034] 5.22 * (S-Ca * 32 / 40) * 10 4 +11,4 * (Ti 2* N) * 10 6 +136.5<3300

[0035] The present inventors have found that this allows further control of the inclusion population of the steel sheet and thus further improvement in bendability.

[0036] The remainder of the composition of the steel is iron and impurities resulting from the processing. The level of impurities resulting from the processing will depend on the production route used and the level of scrap used in the steel. For example, when a basic oxygen furnace route with low levels of scrap (recycled steel) is used, the level of impurities will remain very low. However, large amounts of scrap can also be added to the pig iron produced in the basic oxygen furnace in the converter, which will increase the level of impurities. In addition, when the steel is processed using an electric furnace, for example with a very high rate of recycled scrap, the level of impurities will increase significantly. When high levels of scrap are used, the level of Cu can rise to 0.25%, Ni can rise to 0.25%, Sn can rise to 0.05%, As can rise to 0.03%, Sb can rise to 0.03%, and Pb can rise to 0.03%.

[0037] The microstructure of the steel plate according to the present invention will now be described.

[0038] The steel plate has, on any analyzed section, a microstructure consisting, as a surface fraction, of:

[0039] -75% to 90% ferrite,

[0040] - The rest consists of carbides Fe3C and hard phases such as martensite and bainite.

[0041] Reference Figure 1 , the steel plate 1 according to the present invention comprises a main body portion 3 and top and bottom surface layers 2. The total thickness of the steel plate 1 is t0, and the thickness ts of the surface layer 2 is such that ts=t0 * In other words, the surface layer 2 occupies the outermost 10% of the thickness on both sides of the main body, and the main body of the steel plate occupies 80% of the thickness of the steel plate.

[0042] The present inventors have found that there is a correlation between the bending angle of the steel sheet and the inclusion group in the surface layer portion. In particular, by controlling the following two: the density of TiN / Ti(C,N) inclusions in the surface layer is less than 240 particles / mm 2 And the clustering index of MnS inclusions in the surface part of the steel is less than 110μm / mm 2 , it can be ensured that the normalized bending angle α1.5 in the transverse direction is strictly greater than 48°.

[0043] The following is a description of a method used to characterize inclusions in steel plates and steel parts. It should be understood that this is only one possible method and that others may also be implemented.

[0044] The cross section of the steel plate on which the inclusions are observed is taken in the rolling direction of the steel. In other words, the plane of the observed cross section has the transverse direction as its normal direction.

[0045] The inclusions present in the steel plates were characterized using a Scanning Electron Microscope (SEM) with a Field Effect Gun (FEG). A Tescan Mira 3SEM was used at a 14 kV power setting. This allows the detection of particles as small as 0.5 μm. Using a FEG SEM setup allows stable images to be obtained with excellent resolution over long periods of time, which may be necessary to complete image analysis over large areas - using a FEG SEM setup an image field can be obtained for up to 48 hours, which may be necessary for multiple sample analysis. In addition, the inclusions were analyzed using Energy Dispersive Spectroscopy (EDS). A 120 mm SEM with a large effective surface was used. 2 Bruker EDS probe to detect light elements (O, N) and achieve high count rates, thus allowing accurate quantification. Methods were used to obtain accurate quantification.

[0046] Based on computer-controlled scanning electron microscopy technology, the Automated Steel Cleanliness Analysis Tool (ASCAT) of the RJ Lee group is used to test the SEM and the associated EDS. Six separate samples can be analyzed in the same batch. The sample surface is divided into three regions (top surface layer, bottom surface layer, body as previously described). Each region is divided into fields. In each field, inclusions are detected. In order to detect fine particles, the scanning pixel size is set to a very low value of 0.11 μm. This is to reduce the matrix noise of the SEM image. As will be seen, only objects with a diameter exceeding 0.5 μm are actually considered. The first selection of objects referred to as particles is performed by selecting objects that form solids and have a gray level below 150 or above 220 (extreme values ​​are excluded) on a scale of 0 to 255.

[0047] Each individual particle was then magnified to capture its morphological features and subjected to EDS analysis.A database of all particles was created using ASCAT and considering the chemical and morphological features of all analyzed particles for all acquired images.

[0048] Of all the analyzed particle groups, only particles with a size greater than 0.5 μm and an iron content less than 80% were retained for subsequent analysis and were referred to as inclusions—other particles were considered part of the matrix and were not relevant for subsequent analysis.

[0049] Using the information from the EDS probe, the various inclusions are then classified into one of the following categories: TiN, alumina, complex oxides, oxysulfide particles, MnS, etc. For example, Table 1 details the precise rules used by the inventors to classify MnS and TiN / Ti(C,N) inclusions. A high performance EDS detector enables oxygen quantification. Oxygen levels are checked to separate TiN from TiO2 and MnS from complex oxysulfide inclusions.

[0050] Table 1 - Criteria for classifying inclusions by weight % of Ti, M, S, O, Nb

[0051]

[0052] Then for each inclusion type the following properties are calculated:

[0053] - average diameter, in micrometers,

[0054] -Density, as number of inclusions / mm 2 count,

[0055] The clustering index calculation method is based on the DBSCAN (Density-Based Spatial Clustering of Applications with Noise) algorithm, as described in the article “Adensity-based algorithm for discovering clusters in large spatial databases with noise” in Proceedings of the Second International Conference on Knowledge Discovery and Data Mining (KDD-96). AAAIPress., Ester, Martin; Kriegel, Hans-Peter; Sander, Details are given in Xu, Xiaowei (1996), pp. 226-231.

[0056] The clustering index is determined by taking 2 parameters: maximum_distance and minimum_number_of_points. Clustering is characterized by the following features:

[0057] - it contains only particles of the same type,

[0058] - in a given cluster, the distances of an inclusion to at least one other inclusion are all less than max_distance,

[0059] -It contains a number of individual inclusions equal to or greater than the minimum_number of points.

[0060] For the present invention, the inventors have found that with a maximum_distance of 30 μm maximum distance and a minimum_number of inclusions / minimum_number of points for a cluster of 4, good detection of clusters is obtained.

[0061] The length L of a given cluster is calculated as follows:

[0062] - First determine the convex hull of the cluster using known algorithms (see, for example, the chapter "Convex Hulls: Basic Algorithms" in Computational Geometry, Preparata, FP, Shamos, MI, 1985, Texts and Monographs in Computer Science, Springer, New York, NY).

[0063] - The maximum Feret diameter of the convex hull is then determined, which will be called Dmax, and also the Feret diameter taken in a direction perpendicular to Dmax, which will be called Dvert, is determined. Information on Feret diameter measurements is available, for example, in "Particle Size Measurements: Fundamentals, Practice, Quality" Springer. Henk G. Merkus (January 1, 2009).

[0064] - Calculate the length L of the cluster as

[0065]

[0066] For each type of inclusion, the average length L_mean of all clusters is calculated.

[0067] The cluster density of a given type of inclusions C_density is the number of clusters / mm 2 .

[0068] The clustering index C_index of a given type of inclusion is defined as the product of the average length of the cluster and its density, C_index = L_average * C_density. Clustering index in μm / mm 2 The inventors have found that the clustering index allows samples with different properties to be compared using a unique number and that it correlates well with the bending behavior of the samples.

[0069] The steel sheet according to the present invention can be produced by any appropriate manufacturing method, and a person skilled in the art can define a method. However, it is preferred to use the method according to the present invention including the following steps.

[0070] In the following description, the term ladle refers to a container used to hold molten steel during the refining process. The refining process is referred to as the step of adjusting the final chemical composition and temperature of the melt before casting the steel into its first solidified form, such as before casting it into a slab that will subsequently be hot rolled.

[0071] To successfully control the inclusion population of steel, for example, the following process can be implemented:

[0072] -Tapping of molten steel from a previous steelmaking process step into a ladle. For example, in the case of an electric arc furnace production route, the previous process step is the electric arc furnace process itself. For example, in the case of a blast furnace and converter process (or in the case of a direct reduced iron and converter process), the previous process step is the converter.

[0073] - measuring the sulfur content of the molten steel before the refining step, for example by taking a sample of the molten steel and analyzing it using a spark spectrometer. The sulfur content is measured, for example, by sampling the molten steel directly in a ladle or by sampling the molten steel as it is tapped into the ladle. The sulfur content before the refining step measured in wt.% will be referred to as S_start in the following description.

[0074] - Aluminium is added to the ladle at the start of the refining process to deoxidise the molten steel. The Al addition is carried out, for example, while the steel is being tapped into the ladle - advantageously this allows saving time and thus increasing productivity, and ensures that the molten steel remains sufficiently hot. The amount of Al added to the molten steel at the start of the refining process, expressed in kg aluminium per tonne of molten steel (kg / tonne), will be referred to as Al_addition in the following description.

[0075] - In a subsequent optional step, for example, if the temperature of the molten steel is too low or if it can be foreseen that the waiting time between the end of the refining step and the subsequent process (e.g. continuous casting) requires it, the molten steel is reheated by aluminothermic heating. This is done by adding a determined amount of aluminum and co-blowing a determined amount of oxygen into the molten steel, the determined amount of oxygen corresponding to the stoichiometric ratio required to form Al2O3 with the added aluminum. The strongly exothermic reaction between Al and O2 allows the temperature of the molten steel to be increased. The amount of O2 injected during this optional step will be called O2_injection and will be expressed in standard cubic meters of O2 / ton of molten steel (Nm 3 / ton). Since there is a direct stoichiometric relationship between the O2 injection for thermite reheating and the associated Al injection, the amount of Al for thermite injection will not be considered separately in the current description. It should be noted that the Al for thermite injection is different from the previously mentioned Al addition.

[0076] - The composition of the slag above the melt is adjusted by adding appropriate amounts of minerals to ensure that the %CaO / %Al2O3 ratio of the slag is above 1, the amount of slag / ton of liquid steel is at least 10 kg / ton of liquid steel, and the slag is kept liquid to promote chemical exchange with the steel to enable the steel to enter under the slag and to enable the steel to be tapped separately and / or the slag to be tapped (the liquid state of the slag is verified visually and / or using thermodynamic rules based on its composition and temperature).

[0077] - In a subsequent step, the molten steel is stirred by blowing an inert gas into the molten steel, for example by blowing Ar. This is done to promote the exchange between the molten steel and the slag, which will allow reducing the sulfur content of the molten steel.

[0078] - In a further step, Ca is added to the ladle in order to spheroidize inclusions present in the molten steel. For example, Ca is added in the form of silicon calcium (SiCa) or in the form of iron-calcium (FeCa) or as pure calcium. The addition is performed, for example, by adding SiCa or FeCa to the ladle in the form of a core wire - advantageously, this allows to easily control the amount of Ca added by controlling the length of the core wire inserted into the melt and the injection speed. The amount of Ca added to the molten steel (measured in wt. % in the molten steel) will be referred to as Ca_addition in the following description.

[0079] Taking into account the above process, the inventors have found that a satisfactory level of inclusions can be obtained to achieve a desired level of bending after hot stamping by controlling the above levels of sulfur measured at the start of the refining process (S_start, measured in wt. %), Al addition at the start of the refining process (Al_addition, measured in kg / ton), Ca addition during the refining process (Ca-addition, measured in kg / ton) and the volume of O2 blowing (O2_injection, measured in Nm3 / ton) to verify that the following combination (which will be referred to as C1 in the rest of the description) remains below a given cut-off value:

[0080] 217.8-315.1 * Ca_added +41.5 * O2_injection+18700 * S_Start - 40 * Al_Add(C1)

[0081] In practice, the specific cut-off value below which the combination C1 needs to be controlled will depend on the specific industrial setting for producing steel. It will depend on the production route in the steelmaking plant, the geometry of the ladle used to handle the molten steel, the equipment for adding different additives, the oxygen blowing configuration, etc.

[0082] In order to determine the relationship between these parameters for a given industrial plant and production route, it is recommended to apply the following approach:

[0083] -Several heats were performed using the chemical composition ranges described previously.

[0084] - The smelt is treated using different refining process parameters, in particular different levels of measured sulfur at the start of the refining process, Al addition at the start of the refining process, Ca addition during the refining process and the volume of O2 blowing. The range of refining process parameters tested is selected so as to represent the industrial variation of these parameters. For example, a group of 6 different smelts with 6 different sets of refining process parameters is selected. For example, a group of 8 different smelts with 8 different sets of refining process parameters is selected.

[0085] - The heat was processed according to the industrial route described below and the inclusion population of the steel was characterized using the method described above.

[0086] -The density of TiN / Ti(C,N) inclusions in the surface layer and the clustering index of MnS inclusions in the surface part of the steel and the related refining process parameters are then recorded. The combination C1 of the refining process parameters is calculated. As a general trend, it will be seen that the higher the combination C1, the higher the density of TiN / Ti(C,N) inclusions in the surface layer and the clustering index of MnS inclusions in the surface part of the steel will be.

[0087] - Using the above data set relating surface inclusion characteristics to refining process parameters, a cut-off value was determined below which not only the density of TiN / Ti(C,N) inclusions in the surface layer was less than 240 particles / mm 2 , and the clustering index of MnS inclusions in the surface part of the steel is below 110 μm / mm2. The cut-off value of the combination C1 will determine how to control the refining process of the specific industrial facility under consideration. By controlling C1 below the cut-off value, it will be possible to produce steel plates with both: less than 240 particles / mm 2 The density of TiN / Ti(C,N) inclusions in the surface layer is less than 110μm / mm 2 Clustering index of MnS inclusions in the surface part of the steel. Therefore, it will be possible to achieve an excellent bending level associated with a normalized bending angle α1.5 in the transverse direction that is strictly greater than 48°.

[0088] For example, in the case of a particular industrial facility where the inventors conducted experiments, the cut-off value was equal to 270.

[0089] After the molten steel refining step, the method for manufacturing the steel plate according to the present invention preferably comprises the following steps:

[0090] - Continuously casting the molten steel into a semi-finished product suitable for being hot rolled. During the casting step, special care should be taken to avoid oxygen absorption and, therefore, higher inclusion levels in the semi-finished product. For example, in the case of a continuous casting process, where the semi-finished product is a slab produced in a continuous sequence by casting in a mold the product of multiple melts poured into a tundish, specific refractory materials and linings can be used in the tundish, specific allocation rules can be used for the first of the sequence slabs and for the transition slabs between two different melts, etc.

[0091] The semi-finished product is then optionally reheated at a temperature of 1150°C to 1300°C.

[0092] -The steel sheet is then hot rolled at a finishing hot rolling temperature of 800°C to 950°C.

[0093] -The hot rolled steel is then cooled and heated to a temperature below 670°C 卷取 The steel is then coiled and optionally pickled to remove oxidation.

[0094] - The coiled steel sheet is then optionally cold rolled to obtain a cold rolled steel sheet. The cold rolling reduction ratio preferably ranges from 20% to 80%. Below 20%, recrystallization is not favorable during subsequent heat treatment, which may impair the ductility of the steel sheet. Above 80%, there is a risk of edge cracking during cold rolling.

[0095] - In one embodiment of the present invention, the steel sheet is heated in an annealing furnace to a soaking temperature of 700°C to 850°C and maintained at the soaking temperature for a soaking time of 10 seconds to 20 minutes.

[0096] - In one embodiment of the invention, the steel sheet thus annealed is cooled to a temperature in the range of 400° C. to 700° C. and further coated with a metal coating. The metal coating is, for example, an aluminum-based metal coating comprising at least 50% by weight of aluminum. The metal coating is, for example, a zinc-based metal coating comprising at least 50% by weight of zinc.

[0097] - In one embodiment of the invention, the steel sheet is then cooled to room temperature.

[0098] In summary, the above process preferably includes the following consecutive steps:

[0099] - producing a molten steel having the above chemical composition, wherein during the steel refining stage the level of sulfur measured at the beginning of the refining process, the Al addition at the beginning of the refining process, the Ca addition during the refining process and the volume of the O2 gas blow are controlled to verify the combination 217.8-315.1 * Ca_added +41.5 * O2_injection+18700 * S_Start - 40* The Al_addition (C1) is kept below a predetermined cut-off value. The cut-off value is determined for the specific industrial equipment being used, so that when C1 is below the cut-off value, the density of TiN / Ti(C,N) inclusions in the surface layer is less than 240 particles / mm 2 , and the clustering index of MnS inclusions in the surface part of the steel is less than 110μm / mm 2 .

[0100] - casting said molten steel to obtain semi-finished products capable of being hot rolled,

[0101] - optionally subjecting the semi-finished product to a temperature T of 1100°C to 1300°C 再加热 Reheat,

[0102] - hot rolling the semi-finished product at a finishing hot rolling temperature of 800°C to 950°C,

[0103] - The hot rolled steel sheet is coiled at a temperature T below 670°C. 卷取 Coil down to obtain the coiled steel plate,

[0104] - optionally pickling the coiled steel sheet,

[0105] - optionally, cold rolling the coiled steel sheet at a reduction ratio ranging from 20% to 80% to obtain a cold rolled steel sheet,

[0106] - optionally heating the hot-rolled steel sheet or the cold-rolled steel sheet up to a soaking temperature of 700° C. to 850° C. and keeping the steel sheet at said temperature for a soaking time of 10 seconds to 20 minutes to obtain an annealed steel sheet,

[0107] - optionally cooling the annealed steel sheet to a temperature in the range of 400° C. to 700° C.,

[0108] - optionally coating the annealed steel sheet with a metallic coating,

[0109] - Optionally cooling the coated steel sheet to room temperature.

[0110] The pressed component manufacturing process and subsequent properties of the pressed components will now be described in detail.

[0111] A steel blank is cut from the steel sheet according to the present invention and heated in an austenitizing furnace. Preferably, the steel blank is heated to a temperature of 880°C to 950°C during 10 seconds to 15 minutes to obtain a heated steel blank. The heated blank is then transferred to a press, then hot-formed and press-quenched to obtain a pressed component.

[0112] Optionally, the hot stamped component is further subjected to a paint bake step in which the component is heated to a temperature of 150° C. to 250° C. for a duration of 10 minutes to 2 hours.

[0113] The microstructure of the pressed part comprises more than 95% martensite and less than 5% bainite + ferrite as surface fraction on any analyzed section. Furthermore, the pressed part according to the invention comprises a main body portion and a top skin layer and a bottom skin layer, wherein the skin layer occupies the outermost 10% of the thickness on both sides of the main body. The skin layer has less than 240 particles / mm 2 The density of TiN / Ti(C,N) inclusions is less than 110μm / mm 2 Clustering index of MnS inclusions in the surface part of steel.

[0114] The pressed component according to the invention has a tensile strength higher than 1300 MPa, preferably higher than 1350 MPa, preferably higher than 1400 MPa, and a normalized bending angle α1.5 in the transverse direction strictly greater than 48°. Such high tensile strength and high bending angle give the component very good mechanical resistance, especially in the event of a collision. These characteristics provide very good energy absorption capacity and anti-intrusion capacity, thereby improving the safety of the vehicle.

[0115] The invention will now be illustrated by the following examples which are in no way limiting.

[0116] Eleven different samples of steel from eleven different heats A, B, C, D, E, F, G, H, I, J and K produced using the industrial production route were tested. Samples I1, I2, I3, I4, I5, I6 and I7 are according to the invention, samples R1, R2, R3 and R4 are reference samples.

[0117] All produced samples followed the same industrial production process in a steelmaking plant. All samples were coated after annealing with an AlSi based coating containing 8 to 12 wt% Si, 2 to 4 wt% Fe, the balance being Al.

[0118] Table 2 – Sample composition

[0119] The compositions tested are summarized in the following table, where the element contents are expressed in weight percentages, the remainder of the composition being iron and unavoidable impurities resulting from the processing:

[0120]

[0121] Table 3 – Process parameters of steelmaking plant, density of TiN / Ti(C,N) inclusions in the surface layer and MnS inclusions in the surface layer Clustering index of debris

[0122] The following process parameters were applied in a steelmaking plant and the following density of TiN / Ti(C,N) inclusions in the surface layer and clustering index of MnS inclusions in the surface part of the steel were observed - underlined values ​​are not according to the invention:

[0123]

[0124]

[0125] * C1=217.8-315.1 * Ca_added +41.5 * O2_injection+18700 * S_Start - 40 * Al_Add

[0126] As can be seen, under the industrial conditions tested, the density of TiN / Ti(C,N) inclusions in the surface layer can be controlled to less than 240 particles / mm by ensuring that the refining process parameters are properly controlled to keep C1 below 270. 2 The clustering index of MnS inclusions in the surface layer of steel can be controlled to be less than 110 μm / mm. 2 As previously explained, the cutoff value of 270 is specific to the industrial setting in which the experiment is conducted, and the appropriate cutoff factor for a given industrial setting will need to be determined, for example by following the method described above.

[0127] Table 4 - Additional process conditions

[0128] The following process parameters are applied along the production route:

[0129]

[0130] Table 5 - Microstructure, bending angle and tensile strength

[0131] The following microstructure (in terms of surface fraction), bend angle, bend angle anisotropy and tensile strength were measured on the samples, the underlined values ​​are not according to the invention:

[0132]

[0133]

[0134] Table 5 shows that the samples according to the invention have a tensile strength in the transverse direction higher than 1300 MPa, while having a normalized bending angle α1.5 measured in the transverse direction strictly greater than 48°. On the other hand, the reference samples, despite having a comparable tensile strength level higher than 1300 MPa, all have a normalized bending angle α1.5 measured in the transverse direction equal to or lower than 48°.

[0135] The inventors have found that this very good bendability level is correlated to the density of TiN / Ti(C,N) inclusions in the surface layer and the clustering index of the MnS inclusions in the surface part of the steel.

[0136] When the clustering index of MnS inclusions in the surface layer is equal to or greater than 110 μm / mm 2 When the bending angle decreases, for example, in the case of reference samples R1, R2 and R3, all reference samples R1, R2 and R3 have a bending angle greater than or equal to 110 μm / mm 2 The clustering index of MnS inclusions in the surface layer and the normalized bending angle of 1.5 mm in the transverse direction are equal to or less than 48°.

[0137] When the density of TiN / Ti(C,N) inclusions in the surface layer is equal to or greater than 240μm / mm 2 When the bending angle decreases, for example, in the case of reference sample R1, the reference sample R1 has a bending angle of 246 μm / mm 2 The density of TiN / Ti(C,N) inclusions in the surface layer is reduced, and a bending angle normalized to 1.5 mm in the lateral direction is exhibited of 46° or less.

[0138] By controlling the surface inclusion group within the above range, the produced steel sheet allows the production of hot stamped parts with very good, robust and stable crash resistance for use in, for example, the automotive industry.

Claims

1. A steel plate made of steel having the following composition, wherein the composition comprises by weight percentage: C: 0.2% to 0.3% Mn: 0.8% to 2.0% Si: 0.1% to 0.5% Al: 0.01% to 0.1% Ti: 0.01% to 0.1% B: 0.0005% to 0.005% P≤0.040% Ca≤0.01% S≤0.006% N≤0.01% and optionally contains: Cr≤0.4% Mo≤0.3% Nb≤0.1% V≤0.3% Where Cr+Mo+Nb+V≤0.5% The remainder of the composition is iron and unavoidable impurities resulting from the processing. The steel sheet has a microstructure comprising, by surface fraction, 75% to 90% of ferrite, the remainder of which is a microstructure consisting of Fe3C and hard phases such as martensite and bainite, The steel plate includes, from the main body to the surface of the steel plate: - a body accounting for 80% of the thickness of the steel plate, - the top of such a body is a top and bottom skin layer occupying the outermost 10% of the thickness on both sides of the body, the density of TiN / Ti(C,N) inclusions in the skin layer being strictly lower than 240 particles / mm 2 , and the clustering index of the MnS inclusions in the surface layer is strictly lower than 110 μm / mm 2 .

2. The steel plate according to claim 1, wherein: C: 0.2% to 0.25%, and / or Mn: 1.0% to 1.4%, and / or Si: 0.1% to 0.4%, preferably 0.15% to 0.35%, and / or Al: 0.02% to 0.06%, and / or Ti: 0.02% to 0.06%, and / or B: 0.002% to 0.004%, and / or P ≤ 0.020%, and / or Ca≤0.005%, and / or S ≤ 0.005%, and / or N≤0.008%, preferably N≤0.005%.

3. The steel sheet according to claim 1 or 2, wherein the steel sheet is coated with a metal coating comprising at least 50% by weight of Al.

4. The steel sheet according to claim 1 or 2, wherein the steel sheet is coated with a metal coating comprising at least 50% by weight of Zn.

5. The steel sheet according to any one of claims 1 to 4, wherein the chemical composition further complies with the following conditions, all elements are expressed in weight %: 5.22 * (S-Ca * 32 / 40) * 10 4 +11,4 * (Ti 2* N) * 10 6 +136.5<280.

6. A press-hardened steel component, the steel component having the following composition, the composition comprising by weight percentage: C: 0.2% to 0.3% Mn: 0.8% to 2.0% Si: 0.1% to 0.5% Al: 0.01% to 0.1% Ti: 0.01% to 0.1% B: 0.0005% to 0.005% P≤0.040% Ca≤0.01% S≤0.006% N≤0.01% and optionally contains: Cr≤0.4% Mo≤0.3% Nb≤0.1% V≤0.3% Where Cr+Mo+Nb+V≤0.5% The remainder of the composition is iron and unavoidable impurities resulting from the processing. The steel component has a microstructure comprising, by surface fraction, more than 95% of martensite and up to 5% of bainite or ferrite, The steel component includes, from the body to the surface of the steel component: -main body, - the top of such a body is a top surface layer and a bottom surface layer occupying the outermost 10% of the thickness on both sides of the body, the density of TiN / Ti(C,N) inclusions in the surface layer is less than 240 particles / mm 2 , and the clustering index of the MnS inclusions in the surface layer is less than 110 μm / mm 2 .

7. The press-hardened steel component according to claim 6, wherein: C: 0.2% to 0.25%, and / or Mn: 1.0% to 1.4%, and / or Si: 0.1% to 0.4%, preferably 0.15% to 0.35%, and / or Al: 0.02% to 0.06%, and / or Ti: 0.02% to 0.06%, and / or B: 0.002% to 0.004%, and / or P ≤ 0.020%, and / or Ca≤0.005%, and / or S ≤ 0.005%, and / or N≤0.008%, preferably N≤0.005%.

8. A press-hardened steel component according to claim 6 or 7, wherein the chemical composition further complies with the following conditions, all elements expressed in weight %: 5.22 * (S-Ca * 32 / 40) * 10 4 +11,4 * (Ti 2* N) * 10 6 +136.5<300.

9. A press-hardened steel component according to any one of claims 6 to 8, wherein the press-hardened steel component has a tensile strength TS measured in the transverse direction of at least 1300 MPa and a bending angle normalized to 1.5 mm and measured in the transverse direction of strictly greater than 48°.

10. A method for manufacturing a steel plate according to any one of claims 1 to 5, comprising the following consecutive steps: -Providing molten steel having the following chemical composition, wherein the chemical composition comprises, by weight percentage: C: 0.2% to 0.3% Mn: 0.8% to 2.0% Si: 0.1% to 0.5% Al: 0.01% to 0.1% Ti: 0.01% to 0.1% B: 0.0005% to 0.005% P≤0.040% Ca≤0.01% S≤0.006% N≤0.01% and optionally contains: Cr≤0.4% Mo≤0.3% Nb≤0.1% V≤0.3% Where Cr+Mo+Nb+V≤0.5% The remainder of the composition is iron and unavoidable impurities, - casting said molten steel to obtain semi-finished products capable of being hot rolled, - hot rolling the semi-finished product at a finishing hot rolling temperature of 800° C. to 950° C., - The hot rolled steel sheet is coiled at a temperature T below 670°C. 卷取 The steel plate is then coiled to obtain a coiled steel plate.

11. The method according to claim 10, wherein: C: 0.2% to 0.25%, and / or Mn: 1.0% to 1.4%, and / or Si: 0.1% to 0.4%, preferably 0.15% to 0.35%, and / or Al: 0.02% to 0.06%, and / or Ti: 0.02% to 0.06%, and / or B: 0.002% to 0.004%, and / or P ≤ 0.020%, and / or Ca≤0.005%, and / or S ≤ 0.005%, and / or N≤0.008%, preferably N≤0.005%.

12. The method according to claim 10 or 11, wherein the step of providing the molten steel comprises a stage of refining the molten steel, during which the sulfur level measured at the start of the refining, the Al addition at the start of the refining, the Ca addition during the refining and the volume of the O2 blowing are controlled to verify the combination C1 = 217.8-315.1 * Ca_added +41.5 * O2_injection+18700 * S_Start - 40 * Al_addition remains below a predetermined cut-off value, Al_added is the Al added at the beginning of the refining, in kg aluminum / ton of molten steel, S_start is the sulfur content before said refining, in % by weight, O2_injection is the amount of O2 injected during the optional step of thermite heating, expressed in Nm3 O2 / t molten steel, Ca_addition is the amount of Ca added to the molten steel, measured as wt% in the molten steel.

13. A method for manufacturing a press-hardened steel component according to any one of claims 6 to 9, comprising the following consecutive steps: - providing a steel sheet according to any one of claims 1 to 5, - cutting the steel plate into a predetermined shape in order to obtain a steel blank, - heating the steel blank to a temperature of 880° C. to 950° C. during 10 seconds to 15 minutes to obtain a heated steel blank, - transferring the heated blank to a forming press, - thermoforming the heated blank in the press to obtain a shaped part, - press-hardening the shaped part.

14. The method according to claim 13, further comprising a paint baking step in which the molded part is heated to a temperature of 150°C to 250°C for a duration of 10 minutes to 2 hours.

Citation Information

Patent Citations

  • Niobium and vanadium composite microalloying thermoforming steel and production and hot stamping forming method thereof

    CN111235483A

  • 1900MPa-grade high-strength and high-toughness aluminum-silicon coated steel plate for hot stamping and preparation method thereof

    CN111893377A

  • Steel sheet for manufacturing a press hardened component, press hardened component with a combination of high strength and

    CN114934238A

  • High strength steel sheet excellent in moldability and manufacturing method of the same

    JP2014047395A

  • Hot-pressed member and method for manufacturing same, and cold-rolled steel sheet for hot pressing and method for manufacturing same

    US20200370140A1

Cited By

  • Steel sheet having excellent bendability and high strength press hardened

    CN120905591A