Polyphenol composite two-dimensional material antibacterial coating and preparation method thereof

By combining polyphenols with two-dimensional materials to form an antibacterial coating and using photothermal therapy, the problem of drug resistance in the prevention of bacterial infections is solved, and efficient bacterial killing and osteogenic effects of implants are achieved.

CN118787784APending Publication Date: 2024-10-18NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411183671.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-10-18

Smart Images

  • Figure CN118787784A_ABST
    Figure CN118787784A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a poly-polyphenol composite two-dimensional material antibacterial coating. The preparation method comprises the following steps: step 1, mixing PBS (Phosphate Buffer Solution) with ammonia water to obtain a solution A; 2, polyphenol is dissolved in PBS, then the solution A is added to be stirred, the procedure of washing after centrifugation is repeated for multiple times, and polypolyphenol is obtained after sediment is subjected to freeze drying; 3, dissolving a two-dimensional material in pure water to obtain a solution B, dissolving polypolyphenol in pure water to obtain a solution C, and uniformly mixing the solution B and the solution C to obtain a polypolyphenol composite two-dimensional material solution; 4, spin-coating the surface of the implant matrix with the poly-polyphenol composite two-dimensional material solution; the invention also discloses an antibacterial coating. According to the method, polypolyphenol prepared with PBS as a medium is combined with the two-dimensional material to obtain the polypolyphenol composite two-dimensional material solution, the surface of the implant is spin-coated with the polypolyphenol composite two-dimensional material solution to form the antibacterial coating, and the antibacterial coating has good photo-thermal sterilization performance and is suitable for the technical field of antibacterial coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of antibacterial coatings, and in particular relates to an antibacterial coating of a polyphenol composite two-dimensional material and a preparation method thereof. Background Art

[0002] Infectious diseases are an important public health issue worldwide. Recent research data from authoritative institutions show that bacterial infection has become the second leading cause of death in humans after ischemic heart disease, with Staphylococcus aureus and Escherichia coli ranking first and second in infection-related deaths (both with more than 500,000 deaths). Traditional methods for preventing clinical infections include the use of aseptic techniques and antibiotic treatment, but the long-term abuse of the latter will produce some drug-resistant bacteria, which seriously threatens human health. Given my country's huge population base, the accelerated aging process of society, and the rising demand for medical services, it is crucial to control bacterial infections and develop highly effective antibacterial agents that are less likely to induce drug resistance.

[0003] Among the many methods to solve this dilemma, photothermal therapy (PTT) is a non-invasive, clinically approved and safe treatment strategy. PTT uses photosensitizers to generate sufficient heat under near-infrared light to trigger bacterial damage, biofilm degradation and possible immune response. Therefore, it is of great significance to develop a composite coating with excellent antibacterial properties to make materials implanted in the human body have bactericidal properties. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the above-mentioned prior art and provide a method for preparing a polyphenol composite two-dimensional material antibacterial coating. The preparation method prepares polyphenol using PBS as a medium, combines it with a two-dimensional material to obtain a polyphenol composite two-dimensional material solution, and then spin-coats the polyphenol composite two-dimensional material solution on the implant surface multiple times to form an antibacterial coating, so that the implant has good bactericidal performance.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing an antibacterial coating of a polyphenol composite two-dimensional material, characterized in that the preparation method comprises the following steps:

[0006] Step 1, mixing PBS and ammonia water and stirring evenly to obtain solution A;

[0007] Step 2, dissolving the polyphenol in PBS, adding the solution A obtained in step 1 and stirring, washing with PBS and pure water as media respectively after centrifugation, repeating the centrifugation and washing process for multiple times, retaining the precipitate after centrifugation again, and freeze-drying the precipitate to obtain polyphenol;

[0008] Step 3, dissolving the two-dimensional material in pure water to obtain a solution B, dissolving the polyphenol obtained in step 2 in pure water to obtain a solution C, and mixing the solution B and the solution C to obtain a polyphenol composite two-dimensional material solution;

[0009] Step 4: Spin-coat the polyphenol composite two-dimensional material solution obtained in step 3 evenly on the surface of the implant substrate multiple times to obtain an antibacterial coating.

[0010] The present invention adopts polyphenol and two-dimensional material as raw materials to prepare antibacterial coating. Since polyphenol has the characteristics of biocompatibility, free radical scavenging and light absorption, and two-dimensional material has antibacterial and biocompatibility, the combination of the two can effectively improve the antibacterial effect of antibacterial coating; by preparing polyphenol into polyphenol with rich functional groups, the polyphenol can form strong intermolecular interaction force such as hydrogen bond and closely combine with two-dimensional material; at the same time, the two-dimensional material has large specific surface area and rich surface functional groups, and can provide more Ca 2+ Binding sites are beneficial to later osteogenesis; compared with the existing technology of using antibiotics for treatment, the antibacterial coating can eradicate bacteria through physical means and prevent bacteria from developing drug resistance.

[0011] The above-mentioned method for preparing a polyphenol composite two-dimensional material antibacterial coating is characterized in that the volume ratio of PBS to ammonia water in step one is 20 to 40:1, the stirring time is not less than 30 minutes, and the mass concentration of ammonia water is 24% to 26%.

[0012] The above-mentioned method for preparing a polyphenol composite two-dimensional material antibacterial coating is characterized in that the polyphenol in step 2 is one of dopamine, catechol, catechol, gallic acid and catechin.

[0013] The above-mentioned method for preparing a polyphenol composite two-dimensional material antibacterial coating is characterized in that the stirring time in step 2 is 12h to 30h.

[0014] The present invention uses PBS (phosphate buffered saline) as a medium and controls the stirring time to achieve self-polymerization of polyphenols with controllable morphology, including rod-shaped, spherical, conical, ellipsoidal, etc.; polyphenols of various shapes have different specific surface areas, thereby generating different photothermal properties, and the photothermal properties of the antibacterial coating are controlled by controlling the morphology of the produced polyphenols; for example, spherical polyphenols can be generated when the stirring time is 12 hours, conical polyphenols can be generated when the stirring time is 15 hours, ellipsoidal polyphenols can be generated when the stirring time is 20 hours, and rod-shaped polyphenols can be generated when the stirring time is 30 hours.

[0015] The above-mentioned method for preparing a polyphenol composite two-dimensional material antibacterial coating is characterized in that the concentration of the two-dimensional material in the solution B in step three is 0.1 mg / mL~0.2 mg / mL, the concentration of the polyphenol in the solution C is 0.2 mg / mL~0.4 mg / mL, and the volume ratio of the evenly mixed solution B and solution C is 1:1.

[0016] The present invention controls the concentration of the two-dimensional material in solution B, the concentration of the polyphenol in solution C, and the volume ratio of solution B to solution C, so as to adjust the proportion of the polyphenol components in the antibacterial coating, adjust the total surface area of ​​the polyphenol, and further adjust the photothermal properties of the antibacterial coating, so that the antibacterial coating can reach above 67°C after being irradiated with near-infrared light for 6 minutes.

[0017] The above-mentioned method for preparing a polyphenol composite two-dimensional material antibacterial coating is characterized in that the two-dimensional material in step three is one of graphene, boron nitride, molybdenum disulfide, tungsten disulfide, molybdenum diselenide and tungsten diselenide.

[0018] The above-mentioned method for preparing an antibacterial coating of a polyphenol composite two-dimensional material is characterized in that the implant described in step four is cleaned and then dried before spin coating the polyphenol composite two-dimensional material solution, and the cleaning is performed by ultrasonic cleaning using anhydrous ethanol and pure water as the medium respectively, and the ultrasonic cleaning time is not less than 15 minutes.

[0019] The present invention cleans the implant before spin coating the polyphenol composite two-dimensional material solution, thereby preventing stains and dust from existing on the implant surface and affecting the combination of the antibacterial coating and the implant surface.

[0020] The above-mentioned method for preparing a polyphenol composite two-dimensional material antibacterial coating is characterized in that the material of the implant in step four is one of titanium alloy, zinc alloy, magnesium alloy and PEEK.

[0021] The antibacterial coating prepared by the invention can chelate with the surface of implants made of titanium alloy, zinc alloy, magnesium alloy and PEEK (polyetheretherketone).

[0022] The invention also discloses a polyphenol composite two-dimensional material antibacterial coating, characterized in that the antibacterial coating is prepared by the above-mentioned preparation method.

[0023] The above-mentioned polyphenol composite two-dimensional material antibacterial coating is characterized in that the thickness of the antibacterial coating is 300nm to 1500nm, and the temperature of the antibacterial coating is greater than 67°C after being irradiated with near-infrared light for 6 minutes.

[0024] The present invention sets the thickness of the antibacterial coating to 300nm-1500nm to avoid the antibacterial coating from falling off due to being too thick. At the same time, after the antibacterial coating in this thickness range kills bacteria by near-infrared light irradiation, polyphenols can be degraded into polyphenols in the body, retaining the two-dimensional material and the implant for later osteogenesis. The temperature of the antibacterial coating of the present invention is greater than 67°C after being irradiated with near-infrared light for 6 minutes, and bacteria can be killed when the temperature reaches 60°C. Therefore, the antibacterial coating can effectively kill bacteria after being irradiated with near-infrared light for 6 minutes.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] 1. The present invention combines polyphenols prepared as polyphenols with rich functional groups with two-dimensional materials, and spin-coats them on the surface of implants to prepare antibacterial coatings, which can effectively improve the antibacterial effect of implants. The photothermal properties of the antibacterial coatings can be used to eradicate bacteria, thereby preventing bacteria from developing drug resistance. At the same time, the two-dimensional materials have a large specific surface area and rich surface functional groups, and can provide more Ca 2+ The binding site is beneficial to the later implant osteogenesis.

[0027] 2. The present invention controls the morphology of polyphenols by controlling the stirring time during the preparation of polyphenols, and controls the content of polyphenols and two-dimensional materials in the antibacterial coating, so as to adjust the photothermal performance of the antibacterial coating to a level suitable for antibacterial effect; by controlling the thickness of the antibacterial coating, the antibacterial coating is prevented from being too thick and falling off, and at the same time, after the antibacterial coating is irradiated with near-infrared light to kill bacteria, the polyphenols inside can be degraded into polyphenols in the body, leaving only the two-dimensional material on the surface of the implant for later osteogenesis.

[0028] 3. The antibacterial coating prepared by the preparation method of the present invention can be coated on the surface of implants made of titanium alloy, zinc alloy, magnesium alloy and PEEK.

[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a microscopic morphology of the implant in Example 1 of the present invention.

[0031] Figure 2 This is a microscopic morphology of the catechol coating in Example 1 of the present invention.

[0032] Figure 3 This is a microscopic morphology of the polycatechol coating in Example 1 of the present invention.

[0033] Figure 4 This is a microscopic morphology of the antibacterial coating in Example 1 of the present invention.

[0034] Figure 5 This is a temperature diagram of the photothermal test in Example 1 of the present invention.

[0035] Figure 6 This is a photo of the plate of co-cultured Staphylococcus aureus under near-infrared light irradiation conditions in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] Example 1

[0037] The preparation method of the polyphenol composite two-dimensional material antibacterial coating of this embodiment comprises the following steps:

[0038] Step 1: Mix 27.5 mL of PBS and 0.75 mL of ammonia water and stir for 30 min to obtain solution A; the mass concentration of the ammonia water is 25%;

[0039] Step 2, dissolving 0.45 g of catechol in 10 mL of PBS, then adding the solution A obtained in step 1 and stirring for 30 h, centrifuging and washing with PBS and pure water respectively, centrifuging and retaining the supernatant, and freeze-drying to obtain rod-shaped polycatechol;

[0040] Step 3, dissolving 1 mg of boron nitride in 5 mL of pure water to obtain solution B, dissolving 2 mg of polycatechol obtained in step 2 in 5 mL of pure water to obtain solution C, taking 1 mL of solution B and 1 mL of solution C and mixing them evenly to obtain a polycatechol composite boron nitride solution;

[0041] Step 4: Take 10 μL of the polycatechol-complex boron nitride solution obtained in step 3 and evenly spin-coat it on the surface of the implant multiple times to obtain an antibacterial coating with a thickness of 400 nm; the implant is titanium with a mass purity of not less than 99.9%. Before spin-coating the polycatechol-complex boron nitride solution, the implant is ultrasonically cleaned with anhydrous ethanol and pure water for 15 minutes in sequence, and then vacuum dried at 80°C.

[0042] In this embodiment, catechol can also be replaced by one of dopamine, catechol, gallic acid and catechin other than catechol, boron nitride can also be replaced by one of graphene, molybdenum disulfide, tungsten disulfide, molybdenum diselenide and tungsten diselenide other than boron nitride, and titanium with a mass purity of not less than 99.9% can also be replaced by one of zinc alloy, magnesium alloy and PEEK other than titanium with a mass purity of not less than 99.9%.

[0043] The implant was spin-coated with a 2 mg / mL catechol solution and a 2 mg / mL polycatechol solution under the same conditions as those for preparing the antibacterial coating in this example, respectively, to obtain a catechol coating and a polycatechol coating of the same thickness as the antibacterial coating; and the morphology of the implant, the catechol coating, the polycatechol coating and the antibacterial coating was observed using a scanning electron microscope. Figures 1 to 4 As shown, Figure 1 This is a microscopic morphology of the implant. The surface is relatively rough, and many parallel scratches caused by machining can be observed. Figure 2 This is the microscopic morphology of the catechol coating. There are many cracks on the surface of the coating caused by the loss of gravity water, and some parts have fallen off. Figure 3 This is the microscopic morphology of the polycatechol coating. The cracks on the coating surface are significantly reduced, and there is almost no shedding. Figure 4 This is the microscopic morphology of the antibacterial coating. The surface of the coating is dense and uniform, and it is tightly bonded to the implant. In summary, compared with the catechol coating, the polycatechol coating and the antibacterial coating can better bond with the implant and reduce the occurrence of falling off, especially the antibacterial coating, which is more tightly bonded to the implant due to the addition of two-dimensional materials.

[0044] Photothermal tests were performed on the implant and the three coatings mentioned above, and the temperatures of the implant and the three coating surfaces were measured when near-infrared light was irradiated for 1 min, 2 min, 4 min, 6 min, 8 min, and 10 min. Figure 5 As shown in the figure, the temperatures of the three coatings increased after near-infrared light irradiation. When the irradiation time was 6 minutes, the temperature of the implant was 30°C, the catechol coating was 52.8°C, and the temperatures of the polycatechol coating and the antibacterial coating were both greater than 60°C. Compared with the implant and the catechol coating, the polycatechol coating and the antibacterial coating had better photothermal properties and could effectively kill bacteria after 6 minutes of near-infrared light irradiation. Compared with the antibacterial coating, the temperature of the antibacterial coating was higher when irradiated with near-infrared light for 6 minutes, and the photothermal sterilization performance was better.

[0045] The implant and the antibacterial coating were co-cultured with Staphylococcus aureus for 1 day. Figure 6 As shown, the two culture dishes on the top have no near-infrared light, and the two culture dishes on the bottom have near-infrared light. Comparing the two dishes, under the condition of near-infrared light irradiation, the number of Staphylococcus aureus in the implants and the antibacterial coatings has decreased, especially on the culture dishes with the antibacterial coating, there are almost no colonies visible to the naked eye, indicating that the antibacterial coating has better bactericidal performance than the implant under near-infrared light irradiation.

[0046] Example 2

[0047] The preparation method of the polyphenol composite two-dimensional material antibacterial coating of this embodiment comprises the following steps:

[0048] Step 1: Mix 27 mL of PBS and 1.35 mL of ammonia water and stir for 40 min to obtain solution A; the mass concentration of the ammonia water is 24%;

[0049] Step 2, dissolving 0.43 g of catechol in 10 mL of PBS, then adding the solution A obtained in step 1 and stirring for 12 h, centrifuging and washing with PBS and pure water respectively, centrifuging and retaining the supernatant, and freeze-drying to obtain spherical polycatechol;

[0050] Step 3, dissolving 0.5 mg of molybdenum disulfide in 5 mL of pure water to obtain solution B, dissolving 1.5 mg of polycatechol obtained in step 2 in 5 mL of pure water to obtain solution C, taking 1 mL of solution B and 1 mL of solution C and mixing them evenly to obtain a polycatechol composite molybdenum disulfide solution;

[0051] Step 4: Take 10 μL of the polycatechol composite molybdenum disulfide solution obtained in step 3, and evenly spin-coat it on the surface of the implant multiple times to obtain an antibacterial coating with a thickness of 1500 nm; the implant is magnesium with a mass purity of not less than 99.9%, and the implant is ultrasonically cleaned with anhydrous ethanol and pure water for 15 minutes in sequence before the polycatechol composite molybdenum disulfide solution is applied, and then vacuum dried at 80°C.

[0052] The antibacterial coating prepared in this embodiment is irradiated with near-infrared light. When the irradiation time is 6 minutes, the temperature of the antibacterial coating is greater than 67° C., which can effectively kill bacteria.

[0053] Example 3

[0054] The difference between this embodiment and embodiment 2 is that: 0.43 g of catechol is dissolved in 10 mL of PBS, then added to solution A obtained in step 1 and stirred for 20 hours, centrifuged, washed with PBS and pure water respectively, centrifuged and retained the supernatant, and freeze-dried to obtain ellipsoidal polycatechol.

[0055] The antibacterial coating prepared in this embodiment is irradiated with near-infrared light. When the irradiation time is 6 minutes, the temperature of the antibacterial coating is greater than 67° C., which can effectively kill bacteria.

[0056] Example 4

[0057] The preparation method of the polyphenol composite two-dimensional material antibacterial coating of this embodiment comprises the following steps:

[0058] Step 1: Mix 28 mL of PBS and 0.7 mL of ammonia water and stir for 30 min to obtain solution A; the mass concentration of the ammonia water is 26%;

[0059] Step 2, dissolving 0.5 g of gallic acid in 10 mL of PBS, then adding solution A obtained in step 1 and stirring for 20 h, washing with PBS and pure water respectively after centrifugation, retaining the supernatant by centrifugation, and freeze-drying to obtain ellipsoidal polygallic acid;

[0060] Step 3: dissolving 0.7 mg of graphene in 5 mL of pure water to obtain solution B, dissolving 1 mg of polygallic acid obtained in step 2 in 5 mL of pure water to obtain solution C, taking 1 mL of solution B and 1 mL of solution C and mixing them evenly to obtain a polygallic acid composite graphene solution;

[0061] Step 4: Take 10 μL of the polygallic acid composite graphene solution obtained in step 3 and evenly spin-coat it on the surface of the implant multiple times to obtain an antibacterial coating with a thickness of 300 nm; the implant is magnesium with a mass purity of not less than 99.9%, and the implant is ultrasonically cleaned with anhydrous ethanol and pure water for 15 minutes in sequence before the polygallic acid composite graphene solution is applied, and then vacuum dried at 80°C.

[0062] The antibacterial coating prepared in this embodiment is irradiated with near-infrared light. When the irradiation time is 6 minutes, the temperature of the antibacterial coating is greater than 67° C., which can effectively kill bacteria.

[0063] Example 5

[0064] The difference between this embodiment and embodiment 4 is that: in step 2, 0.5 g of gallic acid is dissolved in 10 mL of PBS, then added to solution A obtained in step 1 and stirred for 15 h, and then washed with PBS and pure water respectively after centrifugation, the supernatant is retained by centrifugation, and freeze-dried to obtain conical polygallic acid.

[0065] The antibacterial coating prepared in this embodiment is irradiated with near-infrared light. When the irradiation time is 6 minutes, the temperature of the antibacterial coating is greater than 67° C., which can effectively kill bacteria.

[0066] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a polyphenol composite two-dimensional material antibacterial coating, It is characterized in that The preparation method comprises the following steps: Step 1, mixing PBS and ammonia water and stirring evenly to obtain solution A; Step 2, dissolving polyphenol in PBS, adding the solution A obtained in step 1 and stirring, washing with PBS and pure water as media respectively after centrifugation, repeating the centrifugation and washing process for multiple times, retaining the precipitate after centrifugation again, and freeze-drying the precipitate to obtain polyphenol; Step 3, dissolving the two-dimensional material in pure water to obtain a solution B, dissolving the polyphenol obtained in step 2 in pure water to obtain a solution C, and mixing the solution B and the solution C to obtain a polyphenol composite two-dimensional material solution; Step 4: Spin-coat the polyphenol composite two-dimensional material solution obtained in step 3 evenly on the surface of the implant substrate multiple times to obtain an antibacterial coating.

2. A method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that In step 1, the volume ratio of PBS to ammonia water is 20-40:1, the stirring time is not less than 30 minutes, and the mass concentration of ammonia water is 24%-26%.

3. The method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that The polyphenol in step 2 is one of dopamine, catechol, catechol, gallic acid and catechin.

4. The method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that The stirring time in step 2 is 12 h to 30 h.

5. The method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that In step 3, the concentration of the two-dimensional material in solution B is 0.1 mg / mL to 0.2 mg / mL, the concentration of polyphenol in solution C is 0.2 mg / mL to 0.4 mg / mL, and the volume ratio of the uniformly mixed solution B to solution C is 1:

1.

6. The method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that The two-dimensional material in step three is one of graphene, boron nitride, molybdenum disulfide, tungsten disulfide, molybdenum diselenide and tungsten diselenide.

7. The method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that In step 4, the implant is cleaned and dried before spin coating the polyphenol composite two-dimensional material solution, and the cleaning is performed by ultrasonic cleaning using anhydrous ethanol and pure water as the medium, and the ultrasonic cleaning time is not less than 15 minutes.

8. The method for preparing a polyphenol composite two-dimensional material antibacterial coating according to claim 1, It is characterized in that The implant in step 4 is made of one of titanium alloy, zinc alloy, magnesium alloy and PEEK.

9. A polyphenol composite two-dimensional material antibacterial coating, It is characterized in that The antibacterial coating is prepared by the preparation method as claimed in any one of claims 1 to 8.

10. The polyphenol composite two-dimensional material antibacterial coating according to claim 9, It is characterized in that The thickness of the antibacterial coating is 300nm-1500nm, and the temperature of the antibacterial coating is greater than 67°C after being irradiated with near-infrared light for 6 minutes.