A method for preparing pyrazines from polyols

By using Pt-based catalysts with doped components, the problems of high cost, difficulty in recovery, and harsh reaction conditions in the amination coupling of polyols to generate pyrazines have been solved. This has enabled the efficient, renewable, and selective preparation of pyrazines, which is applicable to a variety of alcohol substrates and has potential for industrial application.

CN118788329BActive Publication Date: 2026-11-24DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410884119.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2026-11-24
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

Existing research on the amination coupling of polyols to generate pyrazines faces challenges such as high catalyst preparation costs, susceptibility to poisoning, difficulty in catalyst recovery, harsh reaction conditions, and low product yields.

Method used

A Pt-based catalyst with doped components is used, in which the noble metal Pt is distributed in the form of clusters on Al₂O₃, and the doping component M is one or two of Ce, Fe, Mg, Mn, K, Co, and Ni. It is prepared by equal volume co-impregnation method with a loading of 0.5-5 wt%. It efficiently catalyzes the amination coupling of polyols to pyrazines under mild conditions.

Benefits of technology

It achieves high efficiency, renewability and good selectivity of catalyst, reduces the amount of precious metals used, is suitable for a variety of alcohol substrates, has mild reaction conditions, high product yield, meets green and environmental protection requirements, and has promising industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788329B_ABST
    Figure CN118788329B_ABST
Patent Text Reader

Abstract

The application provides a Pt-based catalytic system containing a doping component, and a method for efficiently catalyzing polyol compounds to prepare high-value pyrazine compounds through amination coupling. In the catalyst, the noble metal Pt is highly dispersed in the form of clusters with a size of about 1 nm. Compared with existing research and patents, the catalyst preparation method is simple, the catalyst cost is low, and the catalyst is easy to recover. Meanwhile, the reaction conditions are mild, and the target product has an observable yield. The prepared catalyst is suitable for a kettle reactor, the reaction process is green and environmentally-friendly, and the catalyst has good applicability in various types of polyols. The technical scheme of the application provides a way for synthesizing high-value pyrazine compounds from low-cost alcohol compounds, and has excellent industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic conversion of alcohols, and provides a method for efficiently catalyzing the amination coupling of polyols to prepare high-value pyrazine compounds using a Pt-based catalyst containing doped components. Background Technology

[0002] Pyrazines are an important class of chemical intermediates widely used in the synthesis of pharmaceuticals, agrochemicals, and biomolecules. In recent years, various methods for synthesizing pyrazines have been developed, including amination coupling of aldehydes, ketones, and organic amines; amination coupling of hydroxy ketones with ammonia; and intermolecular coupling of amino acids or amino alcohols. Furthermore, the amination coupling of polyols with ammonia to synthesize pyrazines is a promising method because polyols are less expensive and less toxic than other substrates, and the reaction byproduct is water. This means that alcohol amination is economically and environmentally beneficial, meeting the requirements of energy conservation and environmental protection. Currently, some progress has been made in the amination coupling of polyols to generate primary pyrazines. However, due to the presence of multiple side reactions and the complexity of the reaction pathway, existing research suffers from problems such as high catalyst preparation costs, susceptibility to poisoning, difficulty in catalyst recovery, harsh reaction conditions, and low product yields (see literature review). The amination coupling reaction of polyols includes processes such as dehydrogenation and hydrogenation, which require the synergistic action of multiple sites on the catalyst. Therefore, the development of multifunctional and highly active catalytic systems is of great significance for the amination coupling of polyols to prepare pyrazine compounds. Summary of the Invention

[0003] This invention proposes a Pt-based catalytic system containing doped components, which enables the efficient amination coupling of polyols to generate pyrazines under mild conditions. The noble metal Pt in the catalyst is in a clustered dispersion form, which improves atom utilization and significantly reduces the amount of noble metal used. The catalyst has low cost and exhibits excellent selectivity and renewability. At the same time, it has good substrate applicability in a variety of alcohol substrates and has broad application prospects.

[0004] A method for preparing pyrazine compounds from polyols uses a supported catalyst, Pt-M / Al2O3, where M is a dopant component, acting as a Pt substrate supported on Al2O3, and is one or more of Ce, Fe, Mg, Mn, K, Co, and Ni. The noble metal component is Pt, which is distributed in a clustered form on the surface of M. The loading of Pt in the catalyst is 0.5-5 wt% relative to the Al2O3 support. Within the selected range of noble metal Pt loading, the molar ratio of M to Pt is between 40 and 1. Catalyst preparation: The catalyst is prepared by equal-volume co-impregnation method: a precursor solution containing active metal Pt and dopant component M is mixed according to the required metal loading and molar ratio, and impregnated on a support Al2O3. Specifically, an equal volume of dopant component M (M = Ce, Fe, Mg, Mn, K, Co, Ni) and Pt precursor (Pt(NH3)4(NO3)2, H2PtCl6) solution is impregnated on 1-5 g Al2O3 support. The Pt loading (relative to the support) is 0.5-5 wt%, preferably 0.8-2 wt%, and the molar ratio of dopant component M to Pt is between 40 and 1, preferably in the range of 40-4. The prepared catalyst was first dried in an oven at 80-120 °C for 6-12 h, and then calcined at 400-600 °C for 2-6 h, preferably at 400-500 °C for 3-4 h, under an air atmosphere. Subsequently, it was reduced at 300-500 °C for 1-5 h, preferably at 300-400 °C for 2-3 h, under a hydrogen atmosphere. After cooling to 20-30 °C, it was passivated at 0.5-2% O2 / He for 4-12 h, finally yielding a Pt-based catalyst with doped components dispersed in clusters. For ease of writing, regardless of whether the doped component is in a metallic or oxidized state in the catalyst, it is uniformly referred to as Pt-M / Al2O3.

[0005] The selected precursor solution of metallic Pt is one or both of nitrotetramineplatinum solution or chloroplatinic acid solution.

[0006] The precursor solution of the selected dopant component M is one or both of the corresponding chloride or nitrate.

[0007] In the catalyst, metallic Pt is concentratedly dispersed on the surface of dopant component M in the form of clusters, and dopant component M is dispersed on the surface of the support to form particles; the nanoparticles formed by dopant component M have a particle size between 2-24 nm.

[0008] The performance evaluation of the preparation of pyrazine compounds by amination coupling of polyols was carried out in a batch high-pressure reactor, with substrates including C4-C4 compounds. 14The substrate comprises one or more polyols with aliphatic and / or aromatic functional groups and structures. Preferably, the substrate includes polyols containing different functional groups and structures such as butanediol, propylene glycol, hexanediol, cyclohexanediol, and indanol. The reaction conditions are as follows: substrate concentration 1-10 wt%, preferably 1-5 wt%; reaction temperature 150-200 °C, preferably 170-200 °C; ammonia pressure 0.4-1 MPa, preferably 0.6-1 MPa; reaction time 1-15 h, preferably 7-12 h; alkyl-substituted benzene derivatives as solvents, such as toluene, xylene, and trimethylbenzene, preferably mesitylene; n-dodecane as an internal standard. The total liquid charge is less than or equal to 1 / 3 of the reactor volume.

[0009] This invention utilizes a Pt-based catalyst containing doped components to efficiently catalyze the amination coupling of polyols to prepare high-value pyrazine compounds. The noble metal in this catalyst is in a clustered dispersion form, resulting in high atom utilization. Compared to existing research and patents, the catalyst preparation method of this invention is simple, the catalyst cost is low, it is easy to recover, and the reaction conditions are mild, yielding considerable product yields. The method of this invention is suitable for batch reactors, the reaction process is environmentally friendly, and the catalyst has good renewability. The catalyst prepared by this invention exhibits good applicability to various types of alcohol substrates, is suitable for batch reactors, and the reaction process is environmentally friendly. The technical solution of this invention provides a route for the efficient synthesis of high-value pyrazine compounds from inexpensive alcohols, with excellent industrial application prospects.

[0010] Advantages of this invention: (1) The catalyst proposed in this invention has good dispersibility, wherein the dopant component M is dispersed on the surface of the support, and the low loading of noble metal Pt is distributed on the surface of the dopant component M in the form of clusters. The atom utilization rate of the noble metal is high, realizing the reaction of amination coupling of alcohol compounds to prepare pyrazine with high efficiency. The catalyst preparation is simple, the reaction conditions are mild, and the product yield is high, which is in line with the concept of green environmental protection.

[0011] (2) Compared with the single metal Pt / Al2O3 catalyst, the selectivity of pyrazine is significantly improved after the addition of dopant component M.

[0012] (3) Compared with existing literature and patents, the amount of precious metals used is greatly reduced, the reaction conditions are milder, the yield of pyrazine is higher, the substrate applicability of the catalyst is better, and it has industrial application prospects. Attached Figure Description

[0013] Figure 1 :0.8Pt / Al2O3(a) and 0.8Pt1-Ce 20Transmission electron microscopy (TEM) images of the Al2O3 catalyst (b, c), and corresponding elemental surface scans (d, e, f).

[0014] Figure 2 0.8Pt1-Ce 20 XAFS near-edge spectral normalization results for Al2O3 catalyst (a) and extended-edge spectral results (b).

[0015] Figure 3 0.8Pt1-Ce 20 Stability test of butanediol amination coupling to prepare tetramethylpyrazine catalyzed by Al2O3 catalyst. Solid column represents butanediol conversion, and slanted column represents tetramethylpyrazine yield. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane internal standard, 0.1 g 0.8 Pt1-Ce 20 / Al2O3, reaction temperature 180 ℃, ammonia pressure 0.7MPa, reaction time 12 h, rotation speed 600 rpm / min.

[0016] Appendix 1: 0.8Pt1-Ce 20 R-space spectral bonding fitting results of Al2O3 catalyst XAFS . Detailed Implementation

[0017] The specific embodiments of the present invention are described in detail below with reference to the technical solutions and accompanying drawings. Comparative Example 1: Preparation of the single-metal catalyst Pt / Al2O3 Taking the preparation of the single-metal catalyst 1Pt / Al2O3 as an example: an appropriate amount of nitrotetraammineplatinum solution was impregnated onto an Al2O3 support in equal volumes, with the active component Pt loaded at 1 wt% relative to the support. The catalyst was dried in an oven at 120 ℃ for 12 h, then calcined at 400 ℃ for 3 h in air, and then reduced at 400 ℃ for 2 h in hydrogen atmosphere. After cooling to room temperature, it was passivated for 5 h in an atmosphere of 1% O2 / He (1% O2 volume fraction, the same below). The resulting catalyst is denoted as 1Pt / Al2O3.

[0018] Example 1: Preparation of Pt-M / Al2O3, a Pt-based catalyst containing doped components With 0.8Pt1-Ce 20Taking the preparation of Al2O3 as an example: Equal volumes of nitrotetraammineplatinum and cobalt nitrate solutions were impregnated onto an Al2O3 support. The loading of the active component Pt relative to the support was 0.8 wt%, with subscripts indicating the molar ratio of elements (i.e., the molar ratio of Pt to Ce was 1:20). The catalyst was dried in an oven at 120 °C for 12 h, then calcined at 400 °C for 3 h in air, and then reduced at 400 °C for 2 h in hydrogen atmosphere. After cooling to room temperature, it was passivated for 5 h in an atmosphere of 1% O2 / He (1% O2 volume fraction in the mixed gas). The resulting catalyst is denoted as 0.8Pt1-Ce. 20 / Al2O3. (In the following examples, the number before Pt represents the mass fraction of Pt relative to the carrier, and the subscript number of the metal element represents the molar ratio of the two elements, i.e., the molar ratio of Pt:Ce is 1:20). From the appendix... Figure 1 Electron microscopy results of the catalyst show that in the single-metal 0.8Pt / Al₂O₃, Pt is uniformly distributed on the catalyst (support) surface, with a particle size of approximately 1.7 nm. The 0.8Pt₁₁₀Ce₃ after Ce doping... 20 On Al₂O₃, Pt is more uniformly dispersed, forming clusters of about 1 nm in size. Ce is distributed on the support surface as "nano islands" with a size of about 10 nm. Elemental surface scan results show that after Ce doping, Pt is more concentratedly distributed on the surface of the Ce nano islands. (See attached image) Figure 2 It is 0.8Pt1-Ce 20 XAFS spectra of the Al₂O₃ catalyst show that the near-edge results indicate that the valence state of Pt is close to that of the metal. Extended-edge spectra show that 0.8Pt 1-Ce 20 The peak intensity of the Pt-Pt bond in the Al2O3 catalyst is much lower than that in Pt foil, indicating a much lower Pt-Pt coordination number than in Pt foil. Appendix Table 1 shows the bonding fitting results for the extended edge spectrum, indicating a 0.8Pt1-Ce bond. 20 The coordination number of Pt-Pt in Al₂O₃ is 6, indicating that Pt is distributed in clusters of approximately 1 nm, which is similar to the results from electron microscopy. Combining the results from electron microscopy and XAFS, this confirms the presence of 0.8Pt¹⁻Ce⁻. 20 Pt on the Al2O3 catalyst is distributed in clusters of about 1 nm on the catalyst surface.

[0019] The preparation processes and conditions of Examples 2-7 in Table 1 are the same as those of Comparative Example 1, except that the amount of nitrotetraamineplatinum used in Comparative Examples 2-7 is 1 / 5, 2 / 5, 4 / 5, 2, 5, and 10 times the mass of nitrotetraamineplatinum used in Comparative Example 1, respectively. Electron microscopy results show that when the loading of Pt relative to the support in the catalyst is less than 0.4 wt%, the Pt particles are highly dispersed, forming small clusters smaller than 1 nm. With increasing loading, the Pt particle size gradually increases. At a loading of 0.8 wt%, the particle size range is approximately 1.7 ± 0.2 nm; at 1 wt%, the particle size increases to approximately 2.1 ± 0.35 nm; at 2 wt%, it increases to approximately 3.6 ± 0.16 nm; at 5 wt%, it increases to 5.8 ± 0.21 nm; and at a loading of 10 wt%, the Pt particle size increases to approximately 10.9 ± 0.46 nm.

[0020] The reaction conditions for the preparation of tetramethylpyrazine by the amination coupling of butanediol using different catalysts in Comparative Examples 1-7 were consistent (only the catalysts changed, i.e., different types of catalysts were used). Taking the catalyst prepared in Comparative Example 1 as an example, the reaction conditions are shown in Table 1: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 ℃, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL. After the reaction was completed, the reaction solution was centrifuged, and the supernatant was collected for gas chromatography and mass spectrometry analysis. As can be seen from the results in Table 1, the conversion rate of butanediol continuously increased with the increase of Pt content. When the loading increased to above 0.8 wt%, the conversion rate stabilized above 90%. However, with the increase of loading, the yield of the byproduct sec-butylamine continued to increase. It is worth noting that under the reaction conditions, polyols readily undergo intermolecular dehydration and oligomerization. These larger molecular weight products cannot be detected by gas chromatography, therefore the total yield of the detected products is lower than the conversion of the substrate. This is also why the carbon balance in the subsequent examples and comparative examples is less than 100%. For the single-metal Pt / Al₂O₃ catalyst, the main byproduct is sec-butylamine, which is a byproduct of a different reaction pathway than the target product. Therefore, it is necessary to improve the catalyst by modifying the activity of different reaction pathways within the catalyst.

[0021] Table 1. Performance of Pt / Al2O3 series catalysts in catalyzing the amination coupling of butanediol to prepare tetramethylpyrazine

[0022] Table 1. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0023] Adding a certain amount of dopant to the catalyst is beneficial for adjusting its activity and selectivity. The catalysts in Examples 2-7 and Comparative Examples 8-9 in Table 2 were prepared using the same procedures and methods (processes and conditions) as the catalyst in Example 1, except that the selected dopant precursors (doping component M) were nitrates corresponding to metal M, and the molar ratio of doped atoms M to Pt was controlled at 20:1. Electron microscopy results showed that after doping different atoms onto the catalyst, the Pt particles were well dispersed, with particle sizes ranging from 1 to 1.5 nm. The dopant formed nanoislands with particle sizes of approximately 10-20 nm on the catalyst surface. Their reaction conditions and detection methods were the same as those in Comparative Example 1 (consistent with the reaction conditions for the catalytic coupling of butanediol to tetramethylpyrazine using the catalyst in Comparative Example 1). As shown in Table 2, different types of dopants have varying effects on catalyst activity and selectivity. Most doped metals inhibited the reaction that produces the sec-butylamine byproduct. In all examples, the Ce-doped Pt-based catalyst achieved the highest tetramethylpyrazine yield, approaching 80%. This is likely because Ce is a basic dopant, thus reducing the acid site density of the catalyst and inhibiting the acid-catalyzed dehydration of butanediol to sec-butanol, followed by further amination to sec-butylamine. In Examples 1-7, most byproducts were tetramethylpiperazine, which can be easily converted to the target product (also considered a p-pyrazine product) via dehydrogenation, and therefore exhibit good selectivity for p-pyrazine products. In summary, suitable dopant components include one or two of Ce, Fe, Mg, Mn, K, Co, and Ni, with Ce being preferred.

[0024] Table 2. Properties of Pt-M / Al2O3 series catalysts in the catalytic coupling of butanediol to tetramethylpyrazine

[0025] Table 2. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0026] The previous results show that the activity and selectivity of the catalyst change significantly in the presence of dopants. Therefore, we further investigated the effect of different dopant molar ratios on the preparation of tetramethylpyrazine via butanediol amination coupling. The catalyst preparation processes in Examples 8-11 and Comparative Examples 10-11 are similar to those in Example 1 (process and conditions are consistent), except that the mass content of cerium nitrate in the equal-volume impregnation solution is different. In Examples 8-11 and Comparative Examples 10-11, the amount of cerium nitrate used must meet the molar ratio of Ce to Pt of 40:1, 10:1, 4:1, 1:1, 1:2, and 60:1, respectively. Electron microscopy results confirmed that Pt was uniformly dispersed on the catalysts of Examples 8-11 and Comparative Examples 10-11 (Pt particle size range between 1-2 nm), and the size of the nanoparticles formed on the support surface gradually increased with increasing Ce content. In Example 11, the Ce particle size on the catalyst ranged from 2.3 ± 0.12 nm. Due to the similar size, it was not easy to distinguish the distribution relationship between Pt and Ce. In Example 10, the Ce particle size on the catalyst ranged from 5 ± 0.16 nm, in Example 9 it ranged from 12 ± 0.23 nm, and in Example 8 it ranged from 24 ± 0.39 nm.

[0027] The catalyst reaction conditions in Examples 8-11 and Comparative Examples 10-11 were consistent with those in Example 1 (consistent with the reaction conditions for the catalyst in Example 1 catalyzing the amination coupling of butanediol to prepare tetramethylpyrazine). As can be seen from the results in Table 3, the conversion rate of butanediol and the yield of tetramethylpyrazine showed some significant differences when the molar ratio of Ce to Pt changed. With increasing Ce content, the yield of sec-butylamine gradually decreased, which is related to the fact that Ce doping reduced the acid site density of the catalyst, thereby reducing acid-catalyzed side reactions. Meanwhile, the yield of tetramethylpyrazine gradually increased, reaching its maximum at a Ce to Pt molar ratio of 20:1. Excessive Ce doping may cover some of the Pt active sites, thereby reducing the substrate conversion and the degree of reaction. In summary, a suitable Ce / Pt molar ratio is between 40 and 1, preferably between 40 and 4, and the Ce nanoparticles formed are between 2 and 24 nm, preferably between 5 and 24 nm.

[0028] Table 3. Performance of 0.8Pt-Ce / Al2O3 series catalysts with different Ce / Pt molar ratios in catalyzing the amination coupling of butanediol to prepare tetramethylpyrazine.

[0029] Table 3. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0030] We then investigated the effect of Pt loading on the preparation of tetramethylpyrazine via butanediol amination coupling with a fixed dopant ratio in the catalyst. The catalyst preparation processes in Examples 12-14 and Comparative Examples 12-13 were similar to those in Example 1 (process and conditions were consistent), except for the different mass contents of nitrotetraammineplatinum and cerium nitrate in an equal volume of impregnation solution. With the molar ratio of Ce to Pt remaining constant at 20:1, the amounts of nitrotetraammineplatinum and cerium nitrate in Examples 12-14 and Comparative Examples 12-13 were 5 / 8, 2.5, 6.25, 0.25, and 10 times that in Example 1, respectively. Electron microscopy results confirmed that the Pt on the catalysts of Examples 12-14 and Comparative Examples 12-13 were uniformly dispersed small clusters of approximately 1-2 nm. The increase in overall content did not affect the dispersion of Pt on the Ce particle surface. Furthermore, the size of the nanoparticles formed by the Ce dopant on the support surface was positively correlated with the total loading. In Example 12, the Ce particle size on the catalyst ranged from 6 ± 0.16 nm. In Example 13, the Ce particle size on the catalyst ranged from 20 ± 0.27 nm, in Example 14 it ranged from 32 ± 0.42 nm, in Comparative Example 12 it ranged from 3 ± 0.12 nm, and in Comparative Example 13 it ranged from 50 ± 1.62 nm.

[0031] The catalyst reaction conditions in Examples 12-14 and Comparative Examples 12-13 were consistent with those in Example 1 (consistent with the reaction conditions for the catalytic coupling of butanediol to tetramethylpyrazine using the catalyst in Example 1). As can be seen from the results in Table 4, when the Pt loading is low, the substrate conversion and product yield are relatively low due to the lack of sufficient active centers. While increasing the total loading results in sufficient active centers for higher substrate conversion, excessive Ce content in the catalyst affects the overall pH, thus impacting product selectivity and yield. For example, in Comparative Example 14, with a very high Pt loading, the Ce precursor feed amount is close to 100% compared to the alumina support, meaning the Pt / CeO2 catalyst is almost entirely responsible for the catalytic effect, resulting in very poor product selectivity. In summary, the Pt loading in doped catalysts should be within a suitable range, preferably 0.5-5 wt%, and more preferably 0.8-2 wt%.

[0032] Table 4: Performance of Pt-Ce / Al2O3 series catalysts with different Pt loadings in catalyzing the amination coupling of butanediol to prepare tetramethylpyrazine

[0033] Table 4. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0034] Table 5 shows the results of Examples 15-18 and Comparative Examples 14-15, which investigated the effects of different carrier loads on 0.8Pt1-Ce. 20 The performance of the catalyst in catalyzing the amination coupling of butanediol to prepare tetramethylpyrazine was assessed (under the same reaction conditions as in Example 1). The catalyst preparation, reaction process, and conditions were consistent with those in Example 1 (process and conditions were the same), except for the catalyst support used. As shown in Table 5, the substrate showed higher conversion rates when the support contained certain acidic or basic sites rather than being an inert support. The product distribution and selectivity varied with the type of support, which is related to the distribution of Pt and Ce on the support and their interaction. Overall, Al₂O₃ was the most suitable catalyst support.

[0035] Table 5. 0.8Pt1-Ce under different supports 20 Performance of the catalyst in the catalytic coupling of butanediol to prepare tetramethylpyrazine

[0036] Table 5. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0037] The Ce-doped Pt-based catalyst prepared in this invention exhibits excellent performance in the amination coupling of butanediol to prepare tetramethylpyrazine. Examples 19-24 further investigate the performance of this catalyst in the preparation of pyrazine compounds from other alcohol substrates. All catalysts were prepared from 0.8Pt1-Ce catalysts as described in Example 1. 20The Al2O3 catalyst and reaction conditions differ from those in Example 1 above in that the substrate is different (other reaction conditions are the same as those in Example 1 for the catalytic coupling of butanediol to tetramethylpyrazine). The substrates for different examples are shown in the second column of Table 6. As can be seen from the results in Table 6, for polyols without terminal hydroxyl groups, the catalyst of the present invention exhibits excellent substrate conversion and product yield (Examples 19, 20, 22). However, for substrates with terminal hydroxyl groups, the yield of the target product is very low because the terminal hydroxyl groups are more difficult to activate. The catalyst of the present invention has shown high catalytic performance for these types of polyol substrates. In summary, the catalyst of the present invention has strong substrate applicability and can provide a basis for practical production.

[0038] Table 6. Performance of amination coupling of different polyols in the preparation of tetramethylpyrazine

[0039] Table 6. Reaction conditions: 1 mmol substrate, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 210 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0040] Table 7 shows the conversion performance of butanediol amination coupling to prepare tetramethylpyrazine at different temperatures. The catalysts used in Examples 25-29 and Comparative Example 16 were the same as those prepared in Example 1. The reaction temperatures of the different examples are shown in the second column of Table 7 (consistent with the reaction conditions for butanediol amination coupling to prepare tetramethylpyrazine catalyzed by the catalyst in Example 1). The results in Table 7 show that the reaction temperature has a significant impact on the butanediol amination coupling to prepare tetramethylpyrazine. When the temperature rises above 170°C, the conversion rate of butanediol is above 90%. Continuously increasing the reaction temperature can increase the yield of tetramethylpyrazine and decrease the yield of the byproduct sec-butylamine, because the activation energy required for the acid-catalyzed formation of sec-butylamine is lower. The reason why the yield of tetramethylpyrazine cannot be continuously increased may be that butanediol is more prone to oligomerization at high temperatures, thus consuming some of the substrate. Based on the comprehensive experimental results, the reaction of butanediol amination coupling to prepare tetramethylpyrazine can achieve a considerable product yield in the temperature range of 150-200 °C, with the preferred range being 170-200 °C.

[0041] Table 7. Conversion performance of tetramethylpyrazine prepared by butanediol amination coupling at different reaction temperatures

[0042] Table 7. Reaction conditions: 1 mmol substrate, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0043] Ammonia, as the sole ammonia source in the reaction system, is crucial in its pressure for the amination coupling of butanediol to prepare tetramethylpyrazine. Examples 30-33 and Comparative Examples 17-18 in Table 8 investigated the effect of different ammonia pressures on the reaction results. The catalysts used in Examples 30-33 and Comparative Examples 17-18 were the same as those prepared in Example 1 above. The ammonia pressures for the reaction conditions differed, as shown in the second column of Table 8 (consistent with the reaction conditions for the amination coupling of butanediol to prepare tetramethylpyrazine catalyzed by the catalyst in Example 1 above). The results in Table 8 show that at lower ammonia pressures, the conversion rate of butanediol and the yield of tetramethylpyrazine were both lower, while the selectivity of the two byproducts was relatively higher. This is related to the smaller reaction extent when the ammonia pressure decreased. At higher ammonia pressures (0.8 MPa, 1 MPa), the conversion rate of butanediol decreased, which may be related to the competitive adsorption of ammonia and the substrate, thereby inhibiting the conversion of some substrates. In summary, the product yield is considerable when the ammonia pressure is in the range of 0.4-1 MPa, and the preferred ammonia pressure is (0.6-1 MPa).

[0044] Table 8. Effect of ammonia pressure on the conversion performance of butanediol amination coupling to prepare tetramethylpyrazine

[0045] Table 8. Reaction conditions: 1 mmol substrate, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0046] Table 9 shows Examples 34-37, which investigated the effect of butanediol concentration on the reaction performance for the preparation of tetramethylpyrazine. The catalyst and reaction conditions used in Examples 34-37 were the same as those in Example 1 (consistent with the reaction conditions for the butanediol amination coupling to tetramethylpyrazine catalyzed by the catalyst in Example 1). The difference lay in the substrate concentration, which is shown in the second column of Table 9. The results show that a reduction in substrate concentration (half that in Example 1) in Example 34 resulted in a significant decrease in substrate conversion. This is because the butanediol-to-tetramethylpyrazine reaction is a multi-stage reaction, and a lower substrate concentration slows down the reaction rate. While an increase in substrate concentration, insufficient catalyst input still caused a certain degree of decrease in substrate conversion, the conversion rate remained above 50% when the substrate concentration increased to 10 wt%, indicating that the catalyst remained applicable over a wide range of substrate concentrations, which is beneficial for practical applications. The preferred range is 1-5 wt%.

[0047] Table 9. Effect of substrate concentration on the conversion performance of butanediol amination coupling to prepare tetramethylpyrazine

[0048] Table 9. Reaction conditions: 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0049] Table 10 shows Examples 38-42, which investigated the effect of reaction time on the conversion performance of butanediol amination coupling to tetramethylpyrazine. The catalyst and reaction conditions used in Examples 38-42 were the same as those in Example 1 (the reaction conditions for the butanediol amination coupling to tetramethylpyrazine catalyzed by the catalyst in Example 1 were consistent), except for the reaction time. The substrate concentrations in Examples 38-42 are shown in the second column of Table 10. The results in the table show that when the reaction time was only one hour, most of the substrate was converted. As the reaction time increased, tetramethylpiperazine gradually dehydrogenated to tetramethylpyrazine. When the reaction time exceeded seven hours, the yield of tetramethylpyrazine became very considerable. Overall, the preferred reaction time is in the range of 7-12 hours.

[0050] Table 10. Effect of reaction time on the conversion performance of butanediol amination coupling to prepare tetramethylpyrazine

[0051] Table 10. Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0052] Table 11 shows the effects of the reaction solvent on the reaction performance of butanediol to tetramethylpyrazine in Examples 43-44 and Comparative Example 19. The catalysts and reaction conditions used in Examples 43-44 and Comparative Example 19 were the same as those in Example 1 (consistent with the reaction conditions for the amination coupling of butanediol to tetramethylpyrazine catalyzed by the catalyst in Example 1), except for the reaction solvents. In Examples 43-44 and Comparative Example 19, the solvents were toluene, p-xylene, and methanol, respectively. The results in Table 11 show that when the reaction solvent is a less polar alkyl-substituted benzene, both the substrate conversion and the yield of tetramethylpyrazine are considerable. However, when the solvent is changed to a highly polar methanol solution, the substrate is not converted at all. Therefore, a less polar solvent is more suitable for this reaction. Trimethylbenzene is preferred as the solvent among alkyl-substituted benzenes.

[0053] Table 11. Effect of reaction solvent on the conversion performance of butanediol to tetramethylpyrazine

[0054] Table 11 Reaction conditions: 1 mmol butanediol, 5 mL solvent, 0.5 mmol internal standard n-dodecane, 0.1 g catalyst, reaction temperature 180 ℃, ammonia pressure 0.7 MPa, reaction time 12 h, rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0055] The effects of catalyst calcination temperature on 0.8Pt1-Ce were investigated in Examples 45-46 and Comparative Examples 20-21 in Table 12. 20The effect of Al2O3 on the reaction performance of butanediol to tetramethylpyrazine. The calcination temperature affects the interaction between the metal and the support, significantly impacting metal dispersion. The catalyst preparation process and reaction conditions in Examples 45-46 and Comparative Examples 20-21 were the same as in Example 1 (consistent with the reaction conditions for the catalyst-catalyzed butanediol amination coupling to tetramethylpyrazine in Example 1), except for the calcination temperature. The calcination temperatures of the catalysts in Examples 45-46 and Comparative Examples 20-21 are shown in the second column of Table 12. The results in Table 12 show that at a lower calcination temperature (300℃), the butanediol conversion rate is less than 50%. At lower calcination temperatures, the interaction between metal particles and the support is not favorable, making metal aggregation more likely during subsequent reduction, thus reducing the substrate conversion rate. When the calcination temperature exceeds 600℃, the excessively high calcination temperature affects the interaction between the dopant and the active metal, potentially causing the active component to be covered, leading to a decrease in product yield. The preferred calcination temperature is 400-500℃.

[0056] Table 12. Effect of catalyst calcination temperature on the conversion performance of butanediol to tetramethylpyrazine

[0057] Table 12 Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0058] The effects of calcination time of the catalyst at 400 °C on 0.8Pt1-Ce were investigated in Examples 47-49 and Comparative Example 22 in Table 13. 20 The effect of Al2O3 on the reaction performance of butanediol to tetramethylpyrazine. The catalyst preparation process and reaction conditions in Examples 47-49 and Comparative Example 22 were the same as in Example 1 (consistent with the reaction conditions for the butanediol amination coupling to tetramethylpyrazine catalyzed by the catalyst in Example 1), the difference being the calcination time of the catalyst. The calcination times of the catalysts in Examples 47-49 and Comparative Example 22 are shown in the second column of Table 13. The results in Table 13 show that both excessively long and short calcination times are detrimental to obtaining a high tetramethylpyrazine yield. This is because a longer calcination time may cause some active sites to be covered, while a shorter calcination time is not conducive to the interaction between the active component and the substrate, resulting in a large accumulation during the reduction process. Overall, the catalyst performance is relatively good when the calcination time is in the range of 2-6 h, with a preferred calcination time of 3-4 h.

[0059] Table 13. Effect of calcination time of catalyst at 400℃ on the conversion performance of butanediol to tetramethylpyrazine.

[0060] Table 13 Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0061] The reduction temperature of the catalyst on 0.8Pt1-Ce was investigated in Examples 50-51 and Comparative Examples 23-24 in Table 14. 20 The effect of Al₂O₃ on the reaction performance of butanediol to tetramethylpyrazine. Changes in reduction temperature affect the valence state and dispersion of the metal, thus influencing the reaction. The catalyst preparation process and reaction conditions in Examples 50-51 and Comparative Examples 23-24 were the same as in Example 1 (consistent with the reaction conditions for the catalyst-catalyzed amination coupling of butanediol to tetramethylpyrazine in Example 1), the difference being the reduction temperature of the catalyst. The reduction temperatures in Examples 50-51 and Comparative Examples 23-24 are shown in the second column of Table 14. The results in the table show that at lower reduction temperatures, the metal is in a positive valence state, which is unfavorable for the dehydrogenation of butanediol, thus affecting the conversion rate. Simultaneously, a positive valence metal is beneficial for acid-catalyzed side reactions, resulting in a higher yield of sec-butylamine. Increasing the reduction temperature causes metal agglomeration, reducing the active sites on the catalyst and also causing a decrease in conversion rate. Considerable performance can be obtained at reduction temperatures in the range of 300-500 °C, preferably 300-400 °C.

[0062] Table 14. Effect of catalyst reduction temperature on the conversion performance of butanediol to tetramethylpyrazine

[0063] Table 14 Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0064] In Examples 52-55 of Table 15, the reduction time of the catalyst at 400 °C was investigated for 0.8 Pt1-Ce. 20The effect of Al2O3 on the reaction performance of butanediol to tetramethylpyrazine preparation. The catalyst preparation process and reaction conditions in Examples 52-55 were the same as in Example 1 (consistent with the reaction conditions for the butanediol amination coupling to tetramethylpyrazine catalyzed by the catalyst in Example 1), the difference being the reduction time of the catalyst. The reduction times of the catalysts in Examples 52-55 are shown in the second column of Table 15. The results in the table show that a shorter reduction time results in insufficient reduction of the metal, affecting the butanediol dehydrogenation process and promoting the formation of the byproduct sec-butylamine. Increasing the reduction time increases the degree of metal aggregation, reducing the active sites of the metal on the catalyst, which also leads to a decrease in conversion rate. The preferred reduction time is 2-3 h.

[0065] Table 15. Effect of reduction time of catalyst at 350 °C on the performance of butanediol amination coupling to prepare tetramethylpyrazine

[0066] Table 15 Reaction conditions: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. The reaction was carried out in a batch reactor with a total volume of 50 mL.

[0067] Figure 3 It is 0.8Pt1-Ce 20 Stability test of the Al2O3 catalyst catalyzing the amination coupling of butanediol to prepare tetramethylpyrazine. The reaction procedure was as follows: 1 mmol butanediol, 5 mL mesitylene, 0.5 mmol n-dodecane (internal standard), 0.1 g catalyst, reaction temperature 180 °C, ammonia pressure 0.7 MPa, reaction time 12 h, and rotation speed 600 rpm / min. After the reaction, the reaction solution was centrifuged, and the supernatant was collected for gas chromatography and mass spectrometry analysis. Examples 56-60 are activity tests of the recovered catalyst. The catalyst in Example 56 was obtained by washing and centrifuging the catalyst after the reaction in Example 1 with solvent, and the remaining reaction conditions were the same as in Example 1. The catalyst in Example 57 was obtained by washing and centrifuging the catalyst after the reaction in Example 56, and so on up to the catalyst in Example 60. The reaction results of the recovery experiment are as follows. Figure 3As shown in the figure, after four cycles of recovery testing, the catalyst maintained stable substrate conversion and product yield. However, compared to the fresh catalyst, the product yield decreased. Thermogravimetric analysis revealed significant weight loss of the recovered catalyst in the 400-500 °C range. The exhaust gas contained CO2 and NO2, suggesting that C and N-containing products adsorbed onto the catalyst surface, resulting in the covering of active sites and thus the decrease in yield. Overall, however, the optimal 0.8Pt1-Ce catalyst in this invention... 20 The Al2O3 catalyst exhibits good cycle stability.

Claims

1. A method for preparing pyrazine compounds from polyols, characterized in that: the catalyst used is a supported catalyst Pt-M / Al2O3, wherein M is a doping component, which is supported on Al2O3 as a substrate of Pt, is one or more than two of Ce, Fe and Mn, the noble metal component is Pt, and which is distributed in the form of clusters on the surface of M; the loading of metal Pt in the catalyst is 0.5-5 wt % of Pt relative to the carrier Al2O3, the molar ratio of M to Pt is between 40-1 within the selected loading range of noble metal Pt, the reaction is carried out in a batch autoclave reactor, and the reaction process is as follows: the concentration of alcohol compound substrate is 1-10 wt %, the reaction temperature is 160-200 ℃, the ammonia pressure is 0.4-1 MPa, the reaction time is 1-15 h, and the alkyl-substituted benzene is used as the solvent, which is selected from one or more than two of toluene, xylene and mesitylene.

2. The method according to claim 1, characterized in that: M in the supported catalyst Pt-M / Al2O3 is Ce; the loading of metal Pt in the catalyst is 0.8-2 wt % of Pt relative to the carrier Al2O3; the molar ratio of M to Pt is between 40-4 within the selected loading range of noble metal Pt, the reaction is carried out in a batch autoclave reactor, and the reaction process is as follows: the concentration of alcohol compound substrate is 1-5 wt %; the reaction temperature is 180-200 ℃; the ammonia pressure is 0.6-1 MPa; the reaction time is 7-12 h; and the solvent is mesitylene.

3. The method according to claim 1 or 2, characterized in that: the metal Pt is dispersed in the form of clusters on the surface of the doping component M, and the doping component M is dispersed on the surface of the carrier to form particles; the particle size of the nanoparticles formed by the doping component M is between 2-24 nm.

4. The method according to claim 1 or 2, characterized in that: the particle size of the metal Pt clusters is between 1-2 nm.

5. The method according to claim 1 or 2, characterized in that: the particle size of the nanoparticles formed by the doping component M is between 5-24 nm.

6. The method according to claim 1 or 2, characterized in that: the particle size of the metal Pt clusters is between 1-1.5 nm.

7. The method according to claim 1 or 2, characterized in that: the preparation method of the catalyst is an equal-volume co-impregnation method, and the specific process is as follows: precursor solutions containing active metal Pt and doping component M are mixed according to the required loading and molar ratio of the metals, impregnated on the carrier Al2O3, and the prepared catalyst is first dried, then calcined at 400-600 ℃ for 2-6 h in an air atmosphere, then reduced at 300-500 ℃ for 1-5 h in a hydrogen atmosphere, and finally passivated at 0.5-2 % O2 / He for 4-12 h after being reduced to 20-30 ℃, to obtain a Pt-based catalyst containing a doping component in the form of clusters, which is uniformly denoted as Pt-M / Al2O3 regardless of the valence state of the doping component in the catalyst.

8. The method according to claim 7, characterized in that:

3. The method of claim 1, wherein: ​ ​ 4. The method of claim 3, wherein: ​ ​ ​ ​ ​ The catalyst was prepared by an equal-volume co-impregnation method. The specific process was as follows: a precursor solution containing active metal Pt and dopant component M was mixed according to the required metal loading and molar ratio and impregnated on a support Al2O3. The prepared catalyst was first dried and then calcined at 400-500 °C for 3-4 h in an air atmosphere. Subsequently, it was reduced at 300-400 °C for 2-3 h in a hydrogen atmosphere. After cooling to 20-30 °C, it was passivated at 0.5-2% O2 / He atmosphere for 4-12 h to finally obtain a Pt-based catalyst containing dopant component dispersed in a cluster form. For convenience, regardless of the valence state of the dopant component in the catalyst, it was uniformly referred to as Pt-M / Al2O3.

7. The method according to claim 5, characterized in that: The selected precursor solution of metallic Pt is one or both of nitrotetramineplatinum solution or chloroplatinic acid solution; The precursor solution of the selected dopant component M is one or both of the corresponding chloride or nitrate; The catalyst was first dried in an oven at 80-120 ℃ for 6-12 h.

8. The method according to claim 1, characterized in that: Substrates include C4-C 14 aliphatic and / or aromatic functional groups and structures, one or more of which are polyols, which are dihydric or higher alcohols.

9. The method of claim 1, wherein: n-Dodecane was used as an internal standard; the total liquid charge was less than or equal to 1 / 3 of the reactor volume.

Citation Information

Patent Citations

  • Production of pyrazines

    JP1996225543A