Self-assembled framework structure of two-dimensional material and preparation method thereof

The self-assembly technique combining quaternary ammonium salts and phenolic compounds has solved the problem of long-range ordered structures in two-dimensional materials, enabling simplified preparation and large-scale production, and improving material performance and application potential.

CN118790985BActive Publication Date: 2026-11-24FUDAN UNIVERSITY +1
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202310382728.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2026-11-24
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve long-range ordered structures in two-dimensional materials, especially the parallel arrangement structure of graphene, which prevents the full realization of material properties. Furthermore, the preparation process is complex, costly, and difficult to scale up.

Method used

By using a combination of quaternary ammonium salts RR¹R²R³NX and phenolic compounds as self-assembly aids, worm micelles were formed through self-assembly. Combined with freeze-drying technology, a two-dimensional material framework structure with a long-range ordered structure was prepared.

Benefits of technology

It achieves long-range ordered arrangement of two-dimensional materials, simplifies the preparation process, reduces costs, supports large-scale production, and is suitable for a variety of two-dimensional material applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118790985B_ABST
    Figure CN118790985B_ABST
Patent Text Reader

Abstract

A method for preparing a self-assembled framework structure of a two-dimensional material, the method comprising: 1) using a quaternary ammonium salt RR as a self-assembly aid 1 R 2 R 3 NX compound (I) is mixed with a two-dimensional material dispersion, and phenolic compound (II) is added. The mixture is stirred to form a hydrogel (A), which has a long-range ordered structure within the hydrogel; where R is C 12 -C 20 Saturated or unsaturated hydrocarbon groups, R 1 R 2 1) R3 are each independently C1-C4 alkyl groups, N is nitrogen, and X is a halogen; 2) The obtained hydrogel (A) is dried to obtain a self-assembled framework structure of a two-dimensional material, which is an aerogel (B) with a long-range highly ordered structure. Applications include, but are not limited to: preparing composite materials using the framework as a matrix, such as functionalized composites with polymers or micro / nano particles. It can be applied in various fields such as thermal conductivity and insulation, mechanical reinforcement, electromagnetic shielding, military, and aerospace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials technology and relates to the long-range ordered self-assembly arrangement of two-dimensional materials and the formation of three-dimensional framework structures. Specifically, it involves mixing a quaternary ammonium salt RR1R2R3NX compound with a dispersion of a two-dimensional material (e.g., graphene), adding a phenolic compound, and then self-assembling to obtain a hydrogel with a long-range ordered arrangement of internal two-dimensional materials. After drying the obtained hydrogel, a self-assembled three-dimensional framework structure of the corresponding two-dimensional material is obtained, resulting in an aerogel with a highly ordered long-range structure of two-dimensional materials. Background Technology

[0002] Two-dimensional materials are a cutting-edge field in materials science. Taking graphene as an example, since its first discovery in 2004, it has a wide range of applications in electronic devices, biomedical materials, functional pastes / membrane materials and composite materials due to its excellent electrical, optical and thermodynamic properties.

[0003] CN112903762A discloses a fabrication process for a carbon monoxide gas sensor based on graphene aerosol materials. The process includes: 1) combining graphene with tin dioxide nanomaterials; 2) forming a three-dimensional graphene aerosol; and 3) a printing electronics process. Step 1) involves combining graphene and tin dioxide nanomaterials using inorganic chemical synthesis. The graphene is a two-dimensional material. The tin dioxide nanomaterials are synthesized via a high-temperature, high-pressure hydrothermal method. Step 2) involves freeze-drying the product from step 1) to obtain a three-dimensional TrGO aerosol. The three-dimensional TrGO aerosol has low density and high porosity. Step 3) involves printing the three-dimensional TrGO aerosol onto the sensor using a printing electronics process to form a sensing material coating. The sensing material coating is 500 nanometers in size. PN junctions are formed between the tin dioxide nanoparticles and the graphene material.

[0004] CN101993056A discloses a porous macroscopic carbon material based on graphene and its preparation method. This material is composed of graphene and carbon derived from polyvinyl alcohol, and has a large specific surface area. The preparation method includes: mixing an aqueous solution of graphene oxide and a polyvinyl alcohol solution; placing the homogeneous mixture into a hydrothermal reactor to obtain a graphene-based hydrogel; freeze-drying the hydrogel to obtain a graphene-based aerosol; and heat-treating the aerosol under an argon atmosphere to obtain the porous macroscopic carbon material based on graphene.

[0005] CN103904313A discloses a method for preparing a tin oxide-nitrogen-graphene aerosol composite material and its application in the preparation of lithium-ion battery anodes. Concentrated ammonia, a tin source, and PVP are added to an aqueous dispersion of graphene oxide, mixed thoroughly, and subjected to a hydrothermal reaction at a temperature of 100-300℃ for 1-24 hours. After the reaction, the product is dialyzed in ultrapure water for at least one day. The sample is then frozen at -20℃ for 4 hours, followed by freeze-drying at -53℃ and -30Pa for at least 12 hours. The resulting sample is then vacuum-dried at 70℃ for 10 hours and heat-treated at 550℃ for 3 hours in an argon atmosphere. The aerosol material prepared by this invention is a self-supporting material with a certain degree of toughness. After simple cutting and pressing, it can be directly used as an electrode material for battery assembly, eliminating the need for conductive agents and binders and the cumbersome steps of traditional coating methods for electrode preparation. This improves battery assembly technology while reducing the cost of lithium-ion batteries.

[0006] CN112951455A discloses a method for improving heat transfer between fuel pellets and cladding based on graphene aerosol, comprising the following steps: (1) preparing graphene aerosol particles; (2) mixing the graphene particles prepared in step (1) with helium to form an aerosol; (3) injecting the aerosol obtained after mixing into the gap between the fuel pellets and cladding as a filling medium. Using the mixed aerosol as a filling medium for the gap between the fuel pellets and cladding significantly reduces the thermal resistance between the fuel pellets and cladding compared to the traditional method of using only helium as a filling medium, making heat dissipation from the fuel pellets more efficient and improving the safety performance of nuclear reactor operation.

[0007] CN107601463A discloses a method for preparing graphene aerosol microspheres based on microfluidic technology. First, a graphene dispersion of a certain concentration is prepared as the inner phase fluid, and an organic solvent containing a surfactant is used as the outer phase fluid. A certain flow rate is controlled so that the inner and outer phase fluids pass through a self-made glass capillary microfluidic device to form a monodisperse water / oil emulsion in the collection channel. Then, the emulsion is collected by a collection liquid placed in liquid nitrogen and frozen into graphene ice balls. Finally, the graphene ice balls produced above are filtered and freeze-dried to obtain graphene aerosol microspheres.

[0008] CN111678889A discloses a method for preparing a quantum dot and fluorescent molecule-doped graphene biosensor for detecting trace viruses, including: preparing graphene oxide / reduced graphene oxide using a modified Hummers method, and preparing a graphene oxide / reduced graphene oxide solution; preparing a silica-based graphene sensor substrate: cleaning and wiping a silica sheet, coating a layer of graphene oxide or graphene film on the silica sheet as a silica composite graphene sensor substrate; further preparing a composite film of graphene quantum dots and fluorescent molecules self-assembled on the silica composite graphene sensor substrate; preparing graphene quantum dots using a solvothermal method with graphene oxide / reduced graphene oxide, and self-assembling the graphene quantum dots with a fluorescent dye in solution to prepare a quantum dot and fluorescent molecule-doped graphene biosensor.

[0009] CN109437178A discloses a green and low-energy-consumption preparation method for high-strength graphene aerogel. The method includes: 1. Preparation and treatment of graphene hydrogel: Using graphene oxide as raw material, graphene hydrogel is prepared through a redox reaction. The prepared graphene hydrogel is evenly poured onto several evaporating dishes, and the depth of the graphene hydrogel in the evaporating dishes is controlled to be 2mm-3mm; 2. Drying treatment of graphene hydrogel: The evaporating dishes containing graphene hydrogel are placed in a room at a temperature of 20℃-30℃ and left to stand for a period of time to allow the graphene hydrogel to dry naturally at room temperature. Then, the dried graphene hydrogel in the evaporating dishes is collected together; 3. Preparation of graphene aerosol: The graphene hydrogel dried in SSO2 is freeze-dried using vacuum freeze-drying technology to obtain graphene aerosol; 4. Detection of graphene aerosol.

[0010] CN111874892A discloses a method for preparing graphene aerogel, which includes: 1. dissolving graphene oxide and a crosslinking agent in water to form a homogeneous solution, and then subjecting the solution to a hydrothermal reaction to obtain a mixture; 2. washing and filtering the mixture with an organic solvent to obtain a black solid, immersing the black solid in the organic solvent for 0.5-12 hours, then igniting the black solid until the flame extinguishes to obtain a product with an apparent density of 1-20 mg / cm³. 3 Graphene aerogel. The mass ratio of graphene oxide to crosslinking agent is 1:0.5-1.5. The crosslinking agent is selected from one or more water-soluble sugars, including glucose, fructose, sucrose, maltose, lactose, and soluble starch. The concentration of graphene oxide in the homogeneous solution is 0.5-15 mg / ml. The hydrothermal reaction is carried out at a temperature of 140-200℃ for 3-12 hours. The organic solvent is selected from one or more of methanol, ethanol, and acetone.

[0011] CN113184832A discloses a flexible three-dimensional graphene aerogel, its preparation method and application, and a flexible three-dimensional graphene-based piezoresistive sensor and its application in flexible electronic devices. The flexible three-dimensional graphene aerogel prepared by this invention has a height on the centimeter scale and the graphene sheets therein are arranged in a long-range ordered manner, overcoming the difficulties of poor orderliness and difficulty in obtaining ultra-low detection limits in graphene active materials.

[0012] CN107311152A discloses a graphene aerogel, its preparation method, and its applications. The graphene aerogel comprises an anisotropic, ordered three-dimensional porous network structure composed of graphene sheets, and has a nanoporous structure composed of micropores, mesopores, and macropores, wherein the micropores and mesopores are mainly distributed within the pore walls of the ordered macropores. The preparation method of the graphene aerogel includes: using graphene oxide liquid crystal as a precursor, introducing a crosslinking agent into the liquid crystal system via gas-phase diffusion, then introducing a reducing agent via ion diffusion to obtain a graphene hydrogel, followed by drying to obtain the graphene aerogel. The aerogel of this invention exhibits anisotropic thermal, electrical, and mechanical properties.

[0013] CN111974320A discloses a high-temperature resistant elastic graphene aerogel and its preparation method, comprising the following steps: (1) stirring and mixing graphene oxide solution, reducing agent, surfactant and silica sol evenly to obtain precursor foam; (2) subjecting the precursor foam to hydrothermal reduction reaction to obtain graphene wet gel with silica sol suspended in the pores; (3) subjecting the graphene wet gel to directional freezing and freeze-drying steps in sequence to obtain graphene aerogel with silica nanoparticles loaded on the pore walls; (4) subjecting the graphene aerogel to high-temperature thermal annealing under an inert atmosphere to obtain a high-temperature resistant elastic graphene aerogel with a silica nanofilm covering the pore walls. The obtained high-temperature resistant and highly elastic graphene aerogel significantly improves the temperature resistance of graphene aerogel materials in an oxygen-containing environment from the generally reported no more than 600℃ to 800℃, broadening its application in the field of high temperature and high elasticity.

[0014] CN106044752A discloses a method for preparing highly oriented graphene aerogel. The method involves mixing 1g of graphene with 20-100g of water, followed by ultrasonic dispersion to obtain a graphene dispersion. This dispersion is then placed in a container with electrodes, and an external electric field is applied to orient the solution for 1-100 minutes to obtain a highly oriented graphene dispersion. The frequency of the applied alternating electric field is 10-1000Hz, and the intensity is 50-5000V / m. The highly oriented graphene dispersion is then subjected to the electric field while being freeze-dried in liquid nitrogen, followed by further freeze-drying or critical freeze-drying to obtain the highly oriented graphene aerogel. The ultrasonic dispersion time is 10-100 minutes. The highly oriented graphene aerogel can be used as an electrode material for batteries and supercapacitors, an electron field emission source, a heat insulation and heat dissipation material, an adsorbent material, a high-flux water filtration material, and a catalyst support.

[0015] CN103560016A discloses a method for preparing multi-level porous graphene / carbon composite materials using graphene aerogel as a three-dimensional framework and through in-situ organic-organic self-assembly via hydrothermal process. The method involves synthesizing a polymer prepolymer, mixing a dissolved surfactant with the prepolymer to synthesize spherical single micelles as subunits, hydrothermally freeze-drying graphene oxide to form graphene aerogel, and then hydrothermally heating it with the subunit solution at 100°C for 20 hours. The mass ratio of subunits to graphene aerogel is controlled at (3-8):1. The resulting solid product is dried and then the surfactant is removed by reflux extraction or high-temperature calcination under an inert atmosphere, ultimately yielding a multi-level porous and mesoporously ordered graphene / carbon composite material. The advantage of this invention is that it maintains the macroporous structure of the graphene aerogel while generating an ordered mesoporous structure on the surface of the graphene aerogel. This invention can be used in double-layer capacitors and lithium battery anode materials.

[0016] However, existing technologies do not disclose a universal technical route for preparing parallel-arranged sheet structures for two-dimensional materials (aerogels or aerosols).

[0017] Following graphene, numerous different two-dimensional materials have been discovered and prepared. Based on their varying physicochemical properties, each two-dimensional material possesses its own advantages and potential applications. For example, hexagonal boron nitride nanosheets exhibit electrical insulation, making them excellent insulating and thermally conductive materials; molybdenum disulfide nanosheets possess excellent lubricity; and MXene exhibits good electrical conductivity. Achieving long-range ordered structures in two-dimensional materials is fundamental to realizing many practical applications. For instance, achieving long-range order in graphene sheets can significantly improve the material's electrical conductivity, thermal conductivity, and mechanical properties. Furthermore, achieving long-range ordered framework structures in two-dimensional materials can play a crucial role in numerous application areas. For example, long-range ordered three-dimensional graphene frameworks can serve as matrices for composite preparation of various functional materials. However, current solutions to these two key problems face the following challenges: Taking graphene as an example, its high hydrophobicity and inertness mean that many graphene materials currently use easily dispersible graphene oxide as a precursor, which is then chemically or thermally reduced to obtain reduced graphene oxide. This results in numerous lattice defects and complex, costly processes. While methods such as liquid crystals and ice templates exist to achieve ordered structures, these methods suffer from low overall regularity, making long-range ordering and large-scale fabrication difficult. Other two-dimensional materials also exhibit similar problems, such as difficulty in uniform dispersion, further hindering the formation of highly ordered, large-scale parallel orientation structures. Existing technologies also fail to provide a unified long-range ordered arrangement solution for graphene and other two-dimensional materials. Achieving long-range ordered structures in two-dimensional materials is fundamental to constructing their three-dimensional frameworks, thus becoming a pressing issue. Summary of the Invention

[0018] To address the aforementioned problems, the present invention aims to provide a self-assembled long-range ordered framework structure of two-dimensional materials, its preparation method, and its applications.

[0019] This invention uses surfactants as self-assembly aids in combination with phenolic compounds to form worm micelles.

[0020] According to a first embodiment of the present invention, a method for preparing a self-assembled framework structure of two-dimensional (inorganic) materials (more specifically, a self-assembled long-range (height) ordered framework structure of two-dimensional materials) is provided, the method comprising the following steps:

[0021] 1) Using quaternary ammonium salt RR as a self-assembly aid 1 R 2 R 3 NX compound (I) (preferably in aqueous solution) is mixed with a dispersion of a two-dimensional material (e.g., graphene), a phenolic compound (II) is added, and the mixture is stirred to form a hydrogel (A), wherein the hydrogel has a long-range ordered structure (e.g., worm micelles) or a long-range highly ordered structure; wherein R is C 12 -C 20Saturated or unsaturated hydrocarbon groups, R 1 R 2 R 3 Each is independently a C1-C4 alkyl group, where N is nitrogen and X is a halogen (preferably chlorine or bromine);

[0022] 2) The obtained hydrogel (A) is dried (preferably freeze-dried) to obtain a self-assembled framework structure of two-dimensional material, which is an aerogel (B), wherein the aerogel has an ordered structure, a long-range ordered structure, or a long-range highly ordered structure.

[0023] Preferably, the hydrogel has a long-range (highly) ordered structure, and the aerogel has a long-range (highly) ordered structure.

[0024] Preferably, the hydrogel (A) is dried by (ordinary) freeze-drying, ice template freeze-drying, or supercritical drying.

[0025] Preferably, the two-dimensional (inorganic) material (i.e., two-dimensional material or two-dimensional inorganic material) is selected from one or more of graphene, graphene oxide, reduced graphene oxide (i.e., reduced graphene oxide), boron nitride, boron carbide, silicon carbide, silicon nitride, molybdenum disulfide, MXene, inorganic mineral nanosheets (e.g., montmorillonite nanosheets, (calcined) mica nanosheets, sheet silicate nanosheets), metal nanosheets (e.g., titanium alloy nanosheets, aluminum nanosheets, copper nanosheets), and other ceramics (e.g., conductive ceramics). More preferably, the two-dimensional (inorganic) material is selected from one or more of graphene, graphene oxide, reduced graphene oxide (i.e., reduced graphene oxide), boron nitride, boron carbide, molybdenum disulfide, and MXene.

[0026] Additionally, when graphene oxide is used as the starting two-dimensional material (e.g., to prepare an aerogel of reduced graphene oxide (two-dimensional material)), step 1) of the above method is performed as follows or includes: 1) using the quaternary ammonium salt RR as a self-assembly aid. 1 R 2 R 3 NX compound (I) (preferably in the form of an aqueous solution) is mixed with a two-dimensional material graphene oxide dispersion, a reducing agent (e.g., ascorbic acid, sodium borohydride, potassium borohydride, etc.) is added, and then a phenolic compound (II) is added, and the mixture is stirred to form a hydrogel (A).

[0027] Preferably, the reducing agent is, for example, ascorbic acid, sodium borohydride, potassium borohydride, glucose, hydroxylamine hydrochloride, L-cysteine, or formaldehyde.

[0028] Preferably, R is C 14 -C 18 Saturated or unsaturated hydrocarbon groups, preferably C 14 -C 18Saturated hydrocarbon group (i.e., alkyl group). R 1 R 2 R 3 Each is independently methyl, ethyl, n-propyl, or n-butyl; more preferably, R 1 R 2 R 3 Both are methyl groups.

[0029] Preferred, RR 1 R 2 R 3 NX compound (I) is C 12 -C 20 Alkyl triC1-C4 alkyl ammonium halide (preferably, the halogen is chlorine or bromine).

[0030] Preferred, RR 1 R 2 R 3 NX compound (I) is selected from one or more of the following compounds: hexadecyltrimethylammonium bromide (CTAB), tetradecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, hexadecyldimethylethylammonium bromide, tetradecyldimethylethylammonium bromide, octadecyldimethylethylammonium bromide, hexadecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, hexadecyldimethylethylammonium chloride, tetradecyldimethylethylammonium chloride, and octadecyldimethylethylammonium chloride.

[0031] Phenolic compounds (II) are (organic) monohydric or polyhydric phenols. For example, phenolic compounds (II) are: 1) phenols (e.g., phenol, hydroquinone, resorcinol, catechol, bisphenol A, bisphenol F, bisphenol S), 2) phenols substituted with one or two C1-C4 hydrocarbon groups, or 3) fused-ring phenols (e.g., naphthols, anthraquinones; such as naphthol, 2,3-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, anthraquinone, 1,8-dihydroxyanthracene).

[0032] Generally, quaternary ammonium salts RR 1 R 2 R 3 The NX compound (I) is in the form of an aqueous solution, and the concentration of the solution is 40-600 mg / ml, preferably 43-500 mg / ml, 45-300 mg / ml, preferably 50-250 mg / ml, preferably 55-220 mg / ml, preferably 60-200 mg / ml, preferably 65-180 mg / ml, preferably 70-150 mg / ml, for example 80, 90, 100, 110, 120, 130 or 140 mg / ml.

[0033] Generally, the concentration of two-dimensional materials (e.g., graphene) in the dispersion is 0.01-250 mg / ml, preferably 0.1-220 mg / ml, preferably 1-200 mg / ml, preferably 2-150 mg / ml, preferably 2.5-100 mg / ml, preferably 3-70 mg / ml, preferably 4-45 mg / ml, preferably 5-40 mg / ml, preferably 7-35 mg / ml, preferably 8-32 mg / ml, preferably 10-30 mg / ml, for example 13, 15, 17, 20, 25, 28 mg / ml.

[0034] Quaternary ammonium salt RR 1 R 2 R 3 The weight ratio of NX compound (I) to the two-dimensional material is 5000-1:1, preferably 3000-2:1, preferably 1000-2.5:1, preferably 500-3:1, preferably 400-3.5:1, preferably 300-4:1, preferably 200-4.5:1, preferably 150-5:1, preferably 100-5.5:1, preferably 80-6:1, preferably 60-6.5:1, preferably 50-7:1, preferably 40-7.5:1, preferably 30-8:1, preferably 20-9:1, preferably 15-8.5:1, for example 10:1.

[0035] The phenolic compound (II) is used in an amount of 10-65 wt% (preferably 12-60 wt%, such as 20, 30, 40, 50 wt%), relative to (or based on) the quaternary ammonium salt RR. 1 R 2 R 3 The weight of NX compound (I).

[0036] In this application, the long-range (highly) ordered structure (body) of the hydrogel (i.e., long-range ordered structure or long-range highly ordered structure) refers to: a parallel layered structure.

[0037] The ordered structure, long-range ordered structure, or long-range highly ordered structure of aerogels refers to a parallel layered structure.

[0038] The (average) particle size of the two-dimensional material used in this invention is generally 100 nanometers to 600 micrometers, for example 200 nanometers, 400 nanometers, 500 nanometers, 600 nanometers, 800 nanometers, 1 micrometer, 15 micrometers, 30 micrometers, 40 micrometers, 50 micrometers, 60 micrometers, 70 micrometers, 80 micrometers, 90 micrometers, 100 micrometers, 120 micrometers, 150 micrometers, 200 micrometers, 250 micrometers, 300 micrometers, 400 micrometers, and 500 micrometers.

[0039] This invention utilizes the self-assembly structure of surfactant molecules in solution to further composite self-assemble with two-dimensional materials to form hydrogels and aerogels with long-range ordered framework structures. Framework structures formed by this technical route are collectively referred to as LOF (or LOF framework structures).

[0040] The preparation method of the present invention includes: forming a mixture of a quaternary ammonium salt (e.g., hexadecyltrimethylammonium bromide (CTAB)) and a two-dimensional material (e.g., graphene) in a solution, then adding a phenolic compound (e.g., phenol) to gel the system, and after stirring and standing, forming a hydrogel with an intrinsic long-range ordered structure, which can be freeze-dried to form the corresponding aerogel.

[0041] The principle of the technical solution of this invention is as follows: the surfactant molecule CTAB self-assembles with phenol in solution to form long-chain worm micelles, which are further compounded to form supramolecular assembly when two-dimensional materials are present, and finally form a long-range ordered arrangement structure.

[0042] Of course, the raw materials used to form worm micelles are not limited to CTAB and phenol. They can also include different combinations of CTAB and methylphenol, or worm micelles composed of other surfactant molecules (provided that they can form LOF structure worm micelles with two-dimensional materials).

[0043] Two-dimensional materials are not limited to the examples used above; they can be any two-dimensional material, or two-dimensional materials that are not strictly defined, such as montmorillonite nanosheets, etc.

[0044] The two-dimensional material raw materials used can be obtained by any preparation method, and are not limited to the method used in this invention as described above.

[0045] Extended material preparation, such as composite materials formed by adding polymers, nanoparticles, and other additives to the LOF structure.

[0046] According to a second embodiment of the present invention, a self-assembled framework structure of two-dimensional (inorganic) material is provided (more specifically, a self-assembled long-range ordered arrangement framework structure of two-dimensional material, i.e., a LOF framework structure). It is prepared by the method described above.

[0047] That is, the present invention provides a self-assembled framework structure of two-dimensional materials, which is composed of an ordered structure of aerogel of two-dimensional materials, wherein the ordered structure refers to a parallel-arranged sheet structure; wherein the ordered structure of the aerogel includes two-dimensional materials and a quaternary ammonium salt RR as a self-assembly aid. 1 R 2 R 3 NX compound (I) and phenolic compound (II), where R is C 12 -C 20 Saturated or unsaturated hydrocarbon groups, R 1R 2 R 3 Each is independently a C1-C4 alkyl group, N is nitrogen, and X is a halogen (preferably chlorine or bromine).

[0048] Alternatively, the ordered structure of aerogels consists of two-dimensional materials and quaternary ammonium salts (RR) acting as self-assembly aids. 1 R 2 R 3 It consists of three compounds: NX compound (I) and phenolic compound (II).

[0049] Two-dimensional (inorganic) materials, RR 1 R 2 R 3 NX compound (I) and phenolic compound (II) are as described above.

[0050] In the self-assembled framework structure of two-dimensional materials, two-dimensional (inorganic) materials, RR 1 R 2 R 3 The contents of NX compound (I) and phenolic compound (II) correspond to the (relative) amounts used in the above preparation method. Because only drying (lyophilization) is used in the preparation method, and the product is not separated or purified, the (relative) amounts of the components used in the preparation method directly correspond to the contents of the components in the product.

[0051] That is, in the self-assembled framework structure of two-dimensional materials, the quaternary ammonium salt RR 1 R 2 R 3 The weight ratio of NX compound (I) to the two-dimensional material is 5000-1:1, preferably 3000-2:1, preferably 1000-2.5:1, preferably 500-3:1, preferably 400-3.5:1, preferably 300-4:1, preferably 200-4.5:1, preferably 150-5:1, preferably 100-5.5:1, preferably 80-6:1, preferably 60-6.5:1, preferably 50-7:1, preferably 40-7.5:1, preferably 30-8:1, preferably 20-9:1, preferably 15-8.5:1, for example 10:1.

[0052] In the self-assembled framework structure of two-dimensional materials, the percentage of phenolic compound (II) is 10-65 wt% (preferably 12-60 wt%, such as 20, 30, 40, 50 wt%), relative to or based on quaternary ammonium salt RR. 1 R 2 R 3 Weight of NX compound (I).

[0053] The long-range ordered framework (LOF) structure prepared in this invention has potential applications in major material fields. Its uses include, but are not limited to, thermal conductivity and insulation, mechanical reinforcement, electromagnetic shielding and electromagnetic absorption, military applications, and aerospace.

[0054] Advantages of the present invention

[0055] 1. A long-range ordered arrangement structure of two-dimensional materials was realized.

[0056] 2. The technical route for preparing framework structures is universally applicable to two-dimensional materials.

[0057] 3. The technical route is simple to operate, can achieve large-scale preparation, and has low cost. Attached Figure Description

[0058] Figure 1 This is a scanning electron microscope image of the internal long-range ordered structure (i.e., the three-dimensional framework structure of graphene LOF) of a sample of graphene LOF aerogel from Example 1.

[0059] Figure 2 This is a scanning electron microscope image of the internal long-range ordered structure (i.e., the three-dimensional framework structure of graphene LOF) of another sample of the graphene LOF aerogel of Example 1.

[0060] Figure 3 This is a scanning electron microscope image of the long-range ordered structure inside the graphene LOF hydrogel of Example 1.

[0061] Figure 4 The images show the appearance of the graphene LOF hydrogel (left center) and graphene LOF aerogel (right) from Example 1. Detailed Implementation

[0062] The present invention will be further described in detail through the following embodiments, but the present invention is not limited to these embodiments.

[0063] The devices used in the embodiments are all commonly used in the art and commercially available, unless otherwise specified.

[0064] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be understood that one or more steps mentioned in the present invention do not preclude the existence of other methods and steps before or after the combined steps, or that other methods and steps may be inserted between these explicitly mentioned steps. It should also be understood that these examples are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise stated, each method step is for the purpose of identifying the method steps only, and not for limiting the order of each method or limiting the scope of the invention. Changes or adjustments to their relative relationships, without substantial changes to the technical content, should also be considered within the scope of the invention.

[0065] Raw materials used in the examples:

[0066] Graphene oxide was prepared by oxidizing graphene flakes using the Hummers method after exfoliation with concentrated sulfuric acid (Aladdin reagent), resulting in a graphene oxide (water) dispersion.

[0067] MXene (water) dispersion was prepared by peeling Ti3AlC2 powder with hydrofluoric acid.

[0068] The following is a method for preparing graphene, boron nitride, and molybdenum disulfide using ball milling:

[0069] The specific preparation of graphene by ball milling is as follows: 5g of flake graphite (diameter range 1-40 μm, average diameter 20 μm, Aladdin reagent) was mixed with 25ml of 200mg / ml CTAB (Aladdin reagent) (water) solution. After complete dissolution and mixing, 110g of 1mm diameter zirconia beads were added, and the mixture was placed in a ball mill jar and ball-milled at 400rpm for 24 hours to obtain a viscous slurry. The graphene obtained after milling had a flake diameter of 100nm-2μm (diameter range). The resulting CTAB / graphene mixture can be directly used as a raw material to prepare LOF frames without separation, washing, drying, etc. The raw material (CTAB / graphene mixture) obtained here was diluted with water or CTAB aqueous solution to obtain a graphene dispersion, which was used in the following examples.

[0070] Boron nitride (sheet diameter: 5 μm, Aladdin reagent) and molybdenum disulfide (sheet diameter: 5 μm, Aladdin reagent) were both prepared into mixed slurries of corresponding two-dimensional nanosheets using the ball milling method described above. The obtained raw materials (CTAB / boron nitride and CTAB / molybdenum disulfide) were diluted with water or an aqueous solution of CTAB to obtain the corresponding dispersions, which were used in the examples below. This invention employs ball milling to exfoliate the above-mentioned two-dimensional materials. Furthermore, the two-dimensional material raw materials used in this invention are not limited to the methods described above; raw materials obtained by any method can be used to prepare long-range ordered framework (LOF) structures using the technical route of this invention.

[0071] Example 1

[0072] A hydrogel was formed within 5 minutes at room temperature (25°C) by mixing 100 ml of a 100 mg / ml cetyltrimethylammonium bromide (CTAB) solution with 100 ml of a 10 mg / ml graphene dispersion and adding 6 g of phenol. The hydrogel exhibited a long-range ordered structure with parallel graphene sheets arranged internally. After freeze-drying, the prepared hydrogel yielded a CTAB / graphene aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure.

[0073] A scanning electron microscope image of the internal long-range ordered structure of a sample of graphene LOF aerogel is shown. Figure 1 .

[0074] Scanning electron microscope image of the internal long-range ordered structure of another sample of graphene LOF aerogel is shown below. Figure 2 .

[0075] Scanning electron microscope images of the long-range ordered structure inside the graphene LOF hydrogel are shown below. Figure 3 .

[0076] The morphology of graphene LOF hydrogel (left center) and graphene LOF aerogel (right) is shown in the figure. Figure 4 .

[0077] Example 2

[0078] 50 ml of a 100 mg / ml CTAB solution was mixed with 50 ml of a 4 mg / ml graphene oxide dispersion. The mixture was then sonicated in a water bath to ensure uniform dispersion. Subsequently, 1 g of ascorbic acid was added as a reducing agent until completely dissolved. Then, 3 g of phenol was added. A hydrogel was formed within 5 minutes of stirring at room temperature (25°C). This hydrogel possessed a long-range ordered structure with parallel graphene sheets. The hydrogel was then reduced at 40°C for 24 hours. After freeze-drying, the reduced hydrogel yielded a CTAB / reduced graphene oxide aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure as in Example 1.

[0079] Example 3

[0080] Example 2 was repeated, except that 1.1 g of sodium borohydride was used instead of ascorbic acid as the reducing agent. CTAB / reduced graphene oxide aerogel was obtained, forming a three-dimensional framework structure with a similar parallel ordered structure inside.

[0081] Example 4

[0082] 100g of CTAB solid powder was mixed with 1000ml of 10mg / ml graphene dispersion, and 60g of phenol was added. After stirring at room temperature (30℃) for 5 minutes, a hydrogel was formed, exhibiting a long-range ordered structure with parallel graphene sheets inside. The prepared hydrogel was freeze-dried to obtain a CTAB / graphene aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure inside.

[0083] Example 5

[0084] 10g of CTAB solid powder was mixed with 100ml of a 20mg / ml boron nitride nanosheet dispersion (average sheet diameter 250nm), and 1.5g of phenol was added. After stirring at 80℃ and cooling to room temperature, a hydrogel was formed with a long-range ordered structure of parallel boron nitride sheets inside. The prepared hydrogel was freeze-dried to obtain a CTAB / boron nitride aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure inside.

[0085] Example 6

[0086] 10g of CTAB solid powder and 2g of boron nitride nanosheets were mixed in 100ml of water, and 1.5g of phenol was added. After stirring at 25℃ and cooling to room temperature, a hydrogel was formed with a long-range ordered structure of parallel boron nitride sheets inside. The prepared hydrogel was freeze-dried to obtain a CTAB / boron nitride aerogel, which formed a three-dimensional framework structure with a similar parallel ordered structure inside.

[0087] Example 7

[0088] 100 ml of a 100 mg / ml CTAB solution was mixed with 100 ml of a 10 mg / ml molybdenum disulfide nanosheet dispersion (average sheet diameter 210 nm), and 6 g of phenol was added. A hydrogel was formed within 5 minutes of stirring at room temperature (35 °C), exhibiting a long-range ordered structure with parallel molybdenum disulfide sheets. After freeze-drying, the prepared hydrogel yielded a CTAB / molybdenum disulfide aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure within it.

[0089] Example 8

[0090] 100 ml of 100 mg / ml CTAB solution and 100 ml of 10 mg / ml MXene dispersion were mixed, and 6 g of phenol was added. A hydrogel was formed within 5 minutes of stirring at room temperature (25°C), exhibiting a long-range ordered structure with parallel MXene sheets. The prepared hydrogel was freeze-dried to obtain a CTAB / MXene aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure.

[0091] Example 9

[0092] 10g of CTAB solid powder was mixed with 50ml of 5mg / ml boron nitride dispersion and 50ml of 5mg / ml molybdenum disulfide nanosheet dispersion. 1.5g of phenol was added, and the mixture was stirred at 25°C and then cooled to room temperature to form a hydrogel. The hydrogel exhibited a long-range ordered structure with parallel arrangement of boron nitride and molybdenum disulfide composite layers. After freeze-drying, the prepared hydrogel yielded a CTAB / boron nitride / molybdenum disulfide aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure within it.

[0093] Example 10

[0094] 10g of CTAB solid powder was mixed with 30ml of 5mg / ml graphene dispersion, 30ml of 5mg / ml molybdenum disulfide nanosheet dispersion, 30ml of 5mg / ml boron nitride dispersion, and 30ml of 5mg / ml MXene dispersion. 1.5g of phenol was added, and the mixture was stirred at 25°C and then cooled to room temperature to form a hydrogel. The hydrogel exhibited a long-range ordered structure with parallel arrangement of graphene, molybdenum disulfide, boron nitride, and MXene composite sheets. After freeze-drying, the prepared hydrogel yielded a CTAB / molybdenum disulfide / boron nitride / MXene aerogel, forming a three-dimensional framework structure with a similar parallel ordered structure within it.

[0095] Example 11

[0096] Repeat Example 1, except that supercritical drying is used instead of ordinary freeze drying to obtain CTAB / reduced graphene oxide aerogel, forming a three-dimensional framework structure, which also has a parallel ordered structure similar to that in Example 1.

[0097] Example 12

[0098] Repeat Example 1, except that the ice template method of freeze drying was used instead of ordinary freeze drying to obtain CTAB / reduced graphene oxide aerogel, which forms a three-dimensional framework structure and has a parallel ordered structure similar to that in Example 1.

[0099] Comparative Example 1

[0100] Example 1 was repeated, except that an equal volume (i.e., 100 ml of sodium dodecylbenzenesulfonate (SDBS) solution was used instead of hexadecyltrimethylammonium bromide (CTAB) solution to obtain SDBS / graphene aerogel. However, it does not have the long-range ordered structure of parallel graphene sheets, but only the local, short-range ordered arrangement of graphene.

[0101] Comparative Example 2

[0102] This is carried out according to Example 3 of CN113184832A.

[0103] A 10 mg / mL solution of graphene oxide liquid crystal (graphene oxide nanosheets with lateral dimensions ranging from 0.4 to 4 μm and an average thickness of 1.23 nm) was taken. 10 mL of a surfactant aqueous solution (sodium dodecylbenzenesulfonate as the surfactant, ultrapure water as the solvent, and a surfactant aqueous solution concentration of 1.0 mol / L) was added to the 10 mL solution. The solution was mechanically stirred at 3000 rpm for 30 min to form a homogeneous solution, resulting in a 5 mg / mL reconstructed graphene oxide solution. This reconstructed graphene oxide solution was then added to a high-pressure reactor with a polytetrafluoroethylene (PTFE) liner. The temperature was increased to 180 °C at a rate of 10 °C / min, and hydrothermal self-assembly was performed for 12 h to obtain a graphene oxide hydrogel. The graphene oxide hydrogel was then placed in a vacuum freeze dryer and dried at -50 °C for 48 h to obtain a flexible three-dimensional graphene aerogel (1.96 cm in height).

[0104] The aerogel obtained in Comparative Example 2 did not exhibit a parallel-arranged sheet structure.

[0105] Therefore, the results of the above embodiments demonstrate that the present invention, by employing quaternary ammonium salt RR as a self-assembly aid, achieves its intended effect. 1 R 2 R 3 NX compounds (I) and phenolic compounds (II) can be used to obtain two-dimensional material aerogels with parallel-arranged sheet structures.

Claims

1. A method for preparing a self-assembled framework structure of a two-dimensional material, the method comprising the following steps: 1) Using quaternary ammonium salt RR as a self-assembly aid 1 R 2 R 3 NX compound (I) is mixed with a two-dimensional material dispersion, and phenolic compound (II) is added. The mixture is stirred to form a hydrogel (A), which has a long-range ordered structure within the hydrogel; wherein: RR 1 R 2 R 3 NX compound (I) is selected from one or more of the following compounds: hexadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, hexadecyldimethylethylammonium bromide, tetradecyldimethylethylammonium bromide, octadecyldimethylethylammonium bromide, hexadecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, hexadecyldimethylethylammonium chloride, tetradecyldimethylethylammonium chloride, and octadecyldimethylethylammonium chloride; the two-dimensional material is selected from one or more of graphene, reduced graphene oxide, boron nitride, boron carbide, silicon carbide, silicon nitride, molybdenum disulfide, MXene, inorganic mineral nanosheets, metal nanosheets, and other ceramics; the phenolic compound (II) is: phenols, phenols substituted with one or two C1-C4 hydrocarbon groups, or fused-ring phenols; quaternary ammonium salts RR 1 R 2 R 3 The weight ratio of NX compound (I) to the two-dimensional material is 20-1:1; the percentage of phenolic compound (II) is 10-65 wt%, based on quaternary ammonium salt RR. 1 R 2 R 3 The weight of NX compound (I); the other ceramics are conductive ceramics; the long-range ordered structure of the hydrogel refers to: a parallel-arranged sheet structure; 2) The obtained hydrogel (A) is dried to obtain a self-assembled framework structure of two-dimensional material, namely aerogel (B), which has a long-range ordered structure; the long-range ordered structure of aerogel refers to the parallel-arranged sheet structure.

2. The preparation method according to claim 1, wherein, Phenolic compounds (II) are: phenol, hydroquinone, resorcinol, catechol, bisphenol A, bisphenol F, bisphenol S, naphthol, 2,3-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, anthraquinone, or 1,8-dihydroxyanthracene; and / or Inorganic mineral nanosheets are montmorillonite nanosheets, calcined mica nanosheets, or sheet-like silicate nanosheets; and / or The metal nanosheets are titanium alloy nanosheets, aluminum nanosheets, or copper nanosheets; and / or The long-range ordered structure within the hydrogel exhibits the structure of worm micelles; and / or Quaternary ammonium salts RR as self-assembly aids 1 R 2 R 3 NX compound (I) is in the form of an aqueous solution; and / or The resulting hydrogel (A) was dried by freeze-drying, ice-template freeze-drying, or supercritical drying.

3. The preparation method according to claim 1 or 2, wherein, Quaternary ammonium salt RR 1 R 2 R 3 NX compound (I) is in the form of an aqueous solution, and the concentration of the solution is 40-600 mg / ml.

4. The preparation method according to claim 3, wherein, Quaternary ammonium salt RR 1 R 2 R 3 NX compound (I) is in the form of an aqueous solution, and the concentration of the solution is 43-500 mg / ml.

5. The preparation method according to claim 4, wherein, Quaternary ammonium salt RR 1 R 2 R 3 NX compound (I) is in the form of an aqueous solution, and the concentration of the solution is 45-300 mg / ml.

6. The preparation method according to claim 5, wherein, Quaternary ammonium salt RR 1 R 2 R 3 NX compound (I) is in the form of an aqueous solution, and the concentration of the solution is 50-250 mg / ml.

7. The preparation method according to claim 1 or 2, wherein, The concentration of the two-dimensional material in the dispersion is 0.01-250 mg / ml.

8. The preparation method according to claim 7, wherein, The concentration of the two-dimensional material in the dispersion is 0.1-220 mg / ml.

9. The preparation method according to claim 8, wherein, The concentration of the two-dimensional material in the dispersion is 1-200 mg / ml.

10. The preparation method according to claim 9, wherein, The concentration of the two-dimensional material in the dispersion is 2-150 mg / ml.

11. The preparation method according to claim 1 or 2, wherein, Quaternary ammonium salt RR 1 R 2 R 3 The weight ratio of NX compound (I) to the two-dimensional material is 20-9:

1.

12. The preparation method according to claim 11, wherein, Quaternary ammonium salt RR 1 R 2 R 3 The weight ratio of NX compound (I) to two-dimensional material is 15-8.5 :

1.

13. The preparation method according to claim 1 or 2, wherein, The percentage of phenolic compound (II) used is 12-60 wt%.

14. The preparation method according to claim 1 or 2, wherein, The average particle size of the two-dimensional material is 100 nanometers to 600 micrometers; and / or When graphene oxide is used as the starting two-dimensional material, step 1) of the above method includes: 1) using quaternary ammonium salt RR as a self-assembly aid. 1 R 2 R 3 NX compound (I) was mixed with a two-dimensional material graphene oxide dispersion, a reducing agent was added, and then a phenolic compound (II) was added. The mixture was stirred to form a hydrogel (A).

15. The preparation method according to claim 14, wherein, The reducing agent is ascorbic acid, sodium borohydride, potassium borohydride, glucose, hydroxylamine hydrochloride, L-cysteine, or formaldehyde.

16. A self-assembled framework structure of two-dimensional material, prepared by the method described in any one of claims 1-15.

Citation Information

Patent Citations

  • Graphene-based porous macroscopic carbon material and preparation method thereof

    CN101993056A

  • Method for preparing multilevel pore duct graphene / carbon composite materials

    CN103560016A

  • Preparation method and application of tin oxide-aza graphene aerosol composite material

    CN103904313A

  • Method for preparing high orientation graphene aerogel

    CN106044752A

  • Graphene aerogel, preparation method and applications thereof

    CN107311152A