Profile control agent composition, profile control agent and use
By combining modified asphalt particles with additives, the problem of unsatisfactory suspension and dispersion of asphalt particles in water was solved, and a highly stable suspension system was prepared, which improved the injection performance and effectiveness of steam flooding in heavy oil reservoirs.
Patent Information
- Application Number
- CN202410768612.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The existing asphalt particles have poor suspension and dispersibility in water, resulting in poor profile control agent injection and making it difficult to meet the requirements of steam drive sealing in heavy oil reservoirs.
By combining modified asphalt particles with additives, including the use of water-soluble polymers and/or surfactants, modified asphalt particles with excellent hydrophilicity are prepared, forming a highly stable suspension system and improving the dispersibility and suspension of asphalt particles in water.
It enables asphalt particles to be dispersed and suspended in water for a long time, with a settling time of ≥20h and a water separation rate of ≤30% after 8h, thereby improving the effect of steam drive sealing in heavy oil reservoirs.
Smart Images

Figure CN118792029B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oilfield chemical profile control, and more particularly to a profile control agent composition, profile control agent, and its application. Background Technology
[0002] With the increasing demand for petroleum resources, the demand for unconventional oil and gas development has also risen in recent years. Heavy oil resources account for approximately 20% of my country's total petroleum resources, making it a crucial area for increasing oil reserves and production. Heavy oil reservoirs have high viscosity and are highly temperature-sensitive, typically requiring thermal recovery methods such as steam injection and steam drive for auxiliary extraction. During steam injection and steam drive, steam channeling often occurs, necessitating the injection of a channeling-sealing system to expand the steam chamber volume and improve thermal efficiency and recovery rate.
[0003] Asphalt particle industrial preparation technology is mature, with stable performance and low price. It possesses selective plugging properties and, due to its different softening points, can be used to seal channeling in formations at varying temperatures, making it an ideal sealing material for heavy oil thermal recovery. However, asphalt particles have poor hydrophilicity, dispersibility, and suspension properties in water, making it difficult to meet the requirements for dispersion in water-based solutions followed by injection into and migration within the formation. Therefore, to achieve deep formation sealing channeling of asphalt particles, hydrophilic modification is necessary to improve their dispersibility in water, enabling better injection into the formation.
[0004] Currently, methods to improve the injection performance of asphalt particles mainly include polymer carrying, emulsification dispersion, and polymer plus activator. However, these methods have the following drawbacks: Polymer carrying can only solve the suspension problem of asphalt particles in water-based solutions, but cannot solve the dispersion problem, leading to particle agglomeration and accumulation in the near-wellbore zone, causing blockage; Emulsification dispersion can effectively solve the dispersion problem, but requires a large amount of emulsifier during the emulsification process, and the large amount of emulsifier adsorbed in the formation after injection leads to increased losses, system instability, and reduced effectiveness, and emulsifiers are expensive; Polymer plus activator method also suffers from the problem of activator adsorption in the formation, system instability, and affects the sealing effect.
[0005] Therefore, for profile control agents that mainly use bitumen particles as sealing materials, it is urgent to improve their injectability in order to better meet the needs of steam drive sealing in heavy oil reservoirs. Summary of the Invention
[0006] This invention addresses the problem that existing profile control agents using asphalt particles as sealing materials have poor suspension and dispersibility of asphalt particles in water, resulting in poor injectability of the profile control agent. The invention provides a profile control agent composition, a profile control agent, and its application.
[0007] To achieve the above objectives, the first aspect of the present invention provides a profile control composition comprising: modified asphalt particles and an additive; wherein the weight ratio of the modified asphalt particles to the additive is 1:(0.25-1);
[0008] The additives are selected from water-soluble polymers and / or surfactants;
[0009] The method for preparing the modified asphalt particles includes:
[0010] (1) The asphalt particles are reacted with acid in the first contact reaction to obtain the first product system;
[0011] (2) The first product system is reacted with an oxidant in a second contact reaction to obtain a second product system, and the second product system is separated to obtain oxidized asphalt particles.
[0012] (3) The oxidized asphalt particles are melt-blended with a modifier to obtain modified asphalt particles;
[0013] The modifier is polyvinylpyrrolidone.
[0014] A second aspect of the present invention provides a profile control agent, which is obtained by mixing a raw material containing the composition described in the first aspect with water;
[0015] The modified asphalt particles in the composition have a weight ratio of 1:(98-99.5) to water.
[0016] The third aspect of the present invention provides the application of the composition described in the first aspect or the profile control agent described in the second aspect in steam flooding and sealing of heavy oil reservoirs.
[0017] The composition provided by this invention comprises modified asphalt particles prepared by a specific method and an additive. The modified asphalt particles exhibit excellent hydrophilicity and can be well dispersed in water. The additive further improves the dispersibility and suspension of the modified asphalt particles in water. Using this composition and water to prepare an asphalt particle suspension system, this suspension system achieves a settling time of ≥20h, with a maximum of 72h, and a water separation rate of ≤30% after 8h in a settling experiment conducted at 25℃. It exhibits excellent injectability and can be used as a profile control agent for heavy oil reservoir development, effectively improving the steam flooding and channeling control effect in heavy oil reservoirs. Attached Figure Description
[0018] Figure 1 The infrared spectra of the modified asphalt particles and the unmodified raw asphalt particles prepared in Preparation Example 1 of the present invention are shown.
[0019] Figure 2 The diagram shows the state of the profile control agents prepared in Example 1 and Comparative Example 1 of the present invention after standing and settling at 25°C for 8 hours. Detailed Implementation
[0020] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0021] The first aspect of the present invention provides a profile control composition comprising: modified asphalt particles and an additive; wherein the weight ratio of the modified asphalt particles to the additive is 1:(0.25-1);
[0022] The additives are selected from water-soluble polymers and / or surfactants;
[0023] The method for preparing the modified asphalt particles includes:
[0024] (1) The asphalt particles are reacted with acid in the first contact reaction to obtain the first product system;
[0025] (2) The first product system is reacted with an oxidant in a second contact reaction to obtain a second product system, and the second product system is separated to obtain oxidized asphalt particles.
[0026] (3) The oxidized asphalt particles are melt-blended with a modifier to obtain modified asphalt particles;
[0027] The modifier is polyvinylpyrrolidone.
[0028] According to the present invention, when the additive is a water-soluble polymer in the profile control composition, polyacrylic acid and / or sodium polyacrylate are preferably used. These substances have thickening and suspension properties, which can increase the viscosity of the system in water and slow down the settling speed of asphalt particles in the water-based suspension system.
[0029] In this invention, preferably, the water-soluble polymer is sodium polyacrylate.
[0030] According to the present invention, preferably, the molecular weight of the water-soluble polymer is 1000-5000 g / mol.
[0031] According to the present invention, when the additive is a surfactant in the profile control composition, at least one of sodium dodecylbenzenesulfonate, decaalkyltrimethylammonium chloride, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, and octadecyltrimethylammonium chloride is preferably used. These substances have emulsifying and dispersing effects and can disperse and suspend asphalt particles in an aqueous suspension system.
[0032] In this invention, preferably, the surfactant is sodium dodecylbenzenesulfonate.
[0033] According to a more preferred embodiment of the present invention, in the profile control composition, the auxiliary agent is sodium polyacrylate.
[0034] According to the present invention, in the profile control composition, the modified asphalt particles are prepared by a specific preparation method and have excellent hydrophilicity, which can be effectively dispersed in water. Specifically, they can be prepared by reacting asphalt particles with an acid and an oxidant in sequence.
[0035] In this invention, the definition of the asphalt particles is relatively broad, and asphalt-based raw materials commonly used in the preparation of asphalt sealing materials in this art can be used. Preferably, the particle size of the asphalt particles is 75-125 μm, which can well match the sealing porosity and seepage size of the target reservoir.
[0036] According to the present invention, the particle size of asphalt particles refers to the median particle size D50, which can be determined by a laser particle size analyzer.
[0037] According to the present invention, the softening point of the asphalt particles is 120-280℃, preferably 150-160℃, which is more suitable for steam drive of heavy oil reservoirs in the target oil reservoir.
[0038] According to the present invention, in the method for preparing the modified asphalt particles, in step (1), the acid may be selected from concentrated sulfuric acid and / or concentrated nitric acid, preferably concentrated sulfuric acid.
[0039] According to the present invention, preferably, the acid is concentrated sulfuric acid with a concentration of 98% by weight.
[0040] According to the present invention, in the preparation method of the modified asphalt particles, in step (1), the weight ratio of the asphalt particles to the acid can be 1:(10-40). By contacting the asphalt particles with the acid to carry out an oxidation reaction, the smooth morphology of the asphalt particle surface can be destroyed, the surface roughness of the asphalt particles can be increased, wrinkles can be increased, thereby increasing the reaction sites, and the asphalt particles are in a liquid phase environment, which is conducive to the reaction of subsequent steps.
[0041] According to the present invention, the conditions for the first contact reaction include: a reaction temperature of -5 to 5°C and a reaction time of 45 to 60 min.
[0042] According to the present invention, preferably, the first contact reaction is carried out under stirring conditions.
[0043] According to the present invention, in the method for preparing the modified asphalt particles, in step (2), the oxidant may be selected from at least one of potassium permanganate, potassium dichromate and tert-butyl hydroperoxide, preferably potassium permanganate.
[0044] According to the present invention, in the preparation method of the modified asphalt particles, in step (2), the weight ratio of the asphalt particles to the oxidant can be 1:(1-3). By contacting the first product system with the oxidant for reaction, the oxygen-containing groups such as hydroxyl and epoxy groups can be combined with the carbon atoms in the asphalt particles, thereby grafting hydrophilic groups onto the asphalt particles, so that the asphalt particles have certain hydrophilic properties.
[0045] According to the present invention, preferably, the conditions for the second contact reaction include: first reacting at a temperature of -5 to 10°C for 2-2.5 hours, and then raising the temperature and reacting at a temperature of 40-45°C for 0.5-1 hours.
[0046] According to the present invention, preferably, the oxidant is fed in a slow and uniform manner, with a feeding time of not less than 10 minutes, and more preferably 15-20 minutes, which is conducive to the safe conduct of the reaction.
[0047] According to the present invention, preferably, the second contact reaction is carried out under stirring conditions.
[0048] According to the present invention, in the method for preparing the modified asphalt particles, in step (2), the separation process includes product dilution, reduction of residual oxidant, centrifugal washing and drying performed sequentially.
[0049] According to the present invention, the product dilution can be achieved by adding water to the second product system and stirring. Preferably, a first portion of water (the amount added is the same as the total weight of the raw material asphalt particles, acid, and oxidant) is slowly added to the second product system, then the system temperature is raised to 90-95°C, and then a second portion of water (preferably 1.5 times the weight of the first portion of water) is added and stirred until homogeneous.
[0050] According to the present invention, for reducing the residual oxidant, hydrogen peroxide solution can be added to the diluted product system to reduce the residual oxidant in the system.
[0051] According to the present invention, for the centrifugal washing, the system obtained after reducing the residual oxidant can be centrifuged first, and then the solid product obtained by centrifugation can be washed with water. After washing, the solid can be centrifuged again. The washing and centrifugation can be repeated multiple times until the pH value of the centrifuged liquid reaches 5-6, so that the residual acid is cleaned.
[0052] According to the present invention, in the method for preparing modified asphalt particles, in step (3), the oxidized asphalt particles are melt-blended with a modifier, which can further improve the hydrophilicity of the oxidized asphalt particles. Preferably, the modifier is polyvinylpyrrolidone.
[0053] According to the present invention, in the method for preparing modified asphalt particles, in step (3), the weight ratio of oxidized asphalt particles to modifier is 1:(0.1-0.3), preferably 1:(0.2-0.25, which is more conducive to further improving the dispersion effect of asphalt particles in water.
[0054] According to the present invention, the melt blending is preferably carried out in a twin-screw extruder, and preferably, the temperature of the melt blending is 150-180°C, more preferably 155-165°C.
[0055] The composition provided by the present invention includes modified asphalt particles and additives prepared by a specific method. When these are thoroughly mixed with water, a highly stable asphalt particle suspension system can be obtained under the synergistic effect of the modified asphalt particles and additives. In a sedimentation test conducted at 25°C, the suspension system can achieve a sedimentation time of asphalt particles ≥20h and a water separation rate of ≤30% after 8h, exhibiting excellent injectability.
[0056] According to a preferred embodiment of the present invention, the composition comprises modified asphalt particles and sodium polyacrylate; wherein the weight ratio of the modified asphalt particles to sodium polyacrylate is 1:(0.25-0.5); the method for preparing the modified asphalt particles comprises: (1) subjecting the asphalt particles to concentrated sulfuric acid in a first contact reaction (the weight ratio of the asphalt particles to concentrated sulfuric acid is 1:20-25; the reaction temperature of the first contact reaction is 0-5℃, and the reaction time is 50-60min) to obtain a first product system; (2) subjecting the first product system to potassium permanganate in a second contact reaction. The reaction (the weight ratio of asphalt particles to potassium permanganate is 1:2-3; the second contact reaction is first carried out at a temperature of 0-5℃ for 2-2.5h, and then the temperature is raised and the reaction is carried out at a temperature of 40-45℃ for 0.5-1h) to obtain a second product system, and the second product system is separated to obtain oxidized asphalt particles; (3) the oxidized asphalt particles are melt-blended with polyvinylpyrrolidone (the weight ratio of oxidized asphalt particles to polyvinylpyrrolidone is 1:0.2-0.25; the melt-blending temperature is 155-165℃) to obtain modified asphalt particles. Using the composition of this preferred embodiment, an asphalt particle suspension system with further improved injectability can be prepared. In the sedimentation test conducted at 25℃, the asphalt particle sedimentation time can be ≥60h and the water separation rate can be ≤5% after 8h.
[0057] A second aspect of the present invention provides a profile control agent, which is obtained by mixing a raw material containing the composition described in the first aspect with water;
[0058] The modified asphalt particles in the composition have a weight ratio of 1:(98-99.5) to water.
[0059] According to the present invention, there are no particular limitations on the mixing process during the preparation of the profile control agent; any method that can achieve thorough mixing of the above-mentioned raw materials and water can be used. Preferably, the modified asphalt particles in the composition can be added to water and stirred to obtain a dispersion, and then the remaining components in the composition can be added and stirred to obtain a uniform suspension system, i.e., the profile control agent.
[0060] The profile control agent provided by this invention is a highly stable asphalt particle suspension system. In a sedimentation experiment conducted at 25°C, the asphalt particles in the profile control agent had a sedimentation time of ≥20h and a water separation rate of ≤30% after 8h. It has excellent injectability and can effectively improve the steam drive sealing effect of heavy oil reservoirs.
[0061] The third aspect of the present invention provides the application of the composition described in the first aspect or the profile control agent described in the second aspect in steam flooding and sealing of heavy oil reservoirs.
[0062] The present invention will be described in detail below through embodiments. In the following preparation examples and embodiments,
[0063] Asphalt particles: particle size (D50) 100μm, ash content ≤0.5%, sulfur content ≤0.4%, purchased from Hebei Junsheng New Material Technology Co., Ltd.
[0064] Unless otherwise specified, all other materials used are common commercially available products.
[0065] Preparation Example 1
[0066] This preparation example illustrates the preparation of modified asphalt particles.
[0067] (1) Add asphalt particles to concentrated sulfuric acid (concentration of 98% by weight) and carry out the first contact reaction under stirring conditions (reaction temperature of 0℃, reaction time of 60min) to obtain the first product system; wherein, the weight ratio of asphalt particles to concentrated sulfuric acid is 1:25;
[0068] (2) Under stirring conditions, potassium permanganate (the weight ratio of asphalt particles to potassium permanganate is 1:2) is slowly added to the first product system above. The feeding time is 20 min. Then, the second contact reaction is carried out (the reaction is carried out at 0℃ for 2 h, then the temperature is raised to 40℃ and the reaction is carried out at that temperature for 1 h) to obtain the second product system.
[0069] Slowly add the first portion of water to the second product system for dilution (the amount added is the same as the total weight of the raw material asphalt particles, concentrated sulfuric acid, and potassium permanganate), stir for 30 minutes, then raise the system temperature to 90°C, and add the second portion of water (the amount added is 1.5 times the weight of the first portion of water), and stir for 30 minutes; add hydrogen peroxide solution to the diluted system until no bubbles are generated, completely reducing the residual potassium permanganate in the system; then centrifuge the system (centrifuge speed is 10000 rpm, centrifugation time is 30 minutes), after centrifugation, pour off the supernatant, retain the solid product, wash the solid product with water, and centrifuge again to separate the solid. Repeat the above centrifugation and washing until the pH value of the centrifuged liquid reaches 6, so that the residual acid is cleaned off, and then dry to obtain oxidized asphalt particles;
[0070] (3) The above-mentioned oxidized asphalt particles and polyvinylpyrrolidone were melt-blended in a twin-screw extruder (the weight ratio of oxidized asphalt particles to polyvinylpyrrolidone was 1:0.25, and the melt-blending temperature was 160℃) to obtain modified asphalt particles (denoted as A1).
[0071] Infrared spectroscopy tests were performed on the modified asphalt particles A1 and the unmodified raw asphalt particles used in step (1), and the results are as follows: Figure 1 , Figure 1 As can be seen, the modified asphalt particle A1 sample and the raw asphalt particle sample are similar at 3440 cm⁻¹. -1 and 1619cm -1 A distinct characteristic peak appears at 3440 cm⁻¹. -1 The absorption peaks corresponding to the stretching vibrations of the -OH group and the C=O group are shown. Among them, the modified asphalt particle A1 sample shows an absorption peak at 3440 cm⁻¹. -1 and 1619cm -1 The peak height at the point increased significantly, and the peak area also increased accordingly, indicating that the number of the two hydrophilic groups -OH and C=O in the modified asphalt particles A1 increased greatly, thereby significantly enhancing the dispersion performance of the modified asphalt particles A1 in water.
[0072] Preparation Example 2
[0073] This preparation example illustrates the preparation of modified asphalt particles.
[0074] (1) Add asphalt particles to concentrated sulfuric acid (concentration of 98% by weight) and carry out the first contact reaction under stirring conditions (reaction temperature of 5°C and reaction time of 45 min) to obtain the first product system; wherein, the weight ratio of asphalt particles to concentrated sulfuric acid is 1:10.
[0075] (2) Under stirring conditions, potassium permanganate (the weight ratio of asphalt particles to potassium permanganate is 1:1) is slowly added to the first product system above. The feeding time is 20 min. Then, the second contact reaction is carried out (the reaction is first carried out at 10℃ for 2 h, and then the temperature is raised to 40℃ and the reaction is carried out at that temperature for 0.7 h) to obtain the second product system.
[0076] Slowly add the first portion of water to the second product system for dilution (the amount added is the same as the total weight of the raw material asphalt particles, concentrated sulfuric acid, and potassium permanganate), stir for 30 minutes, then raise the system temperature to 90°C, and add the second portion of water (the amount added is 1.5 times the weight of the first portion of water), and stir for 30 minutes; add hydrogen peroxide solution to the diluted system until no bubbles are generated, completely reducing the residual potassium permanganate in the system; then centrifuge the system (centrifuge speed is 10000 rpm, centrifugation time is 30 minutes), after centrifugation, pour off the supernatant, retain the solid product, wash the solid product with water, and centrifuge again to separate the solid. Repeat the above centrifugation and washing until the pH value of the centrifuged liquid reaches 6, so that the residual acid is cleaned off, and then dry to obtain oxidized asphalt particles;
[0077] (3) The above-mentioned oxidized asphalt particles and polyvinylpyrrolidone were melt-blended in a twin-screw extruder (the weight ratio of oxidized asphalt particles to polyvinylpyrrolidone was 1:0.25, and the melt-blending temperature was 160℃) to obtain modified asphalt particles (denoted as A2).
[0078] Preparation Example 3
[0079] This preparation example illustrates the preparation of modified asphalt particles.
[0080] (1) Add asphalt particles to concentrated sulfuric acid (concentration of 98% by weight) and carry out the first contact reaction under stirring conditions (reaction temperature of -5℃, reaction time of 60min) to obtain the first product system; wherein, the weight ratio of asphalt particles to concentrated sulfuric acid is 1:40.
[0081] (2) Under stirring conditions, potassium permanganate (the weight ratio of asphalt particles to potassium permanganate is 1:3) is slowly added to the first product system above. The feeding time is 20 min. Then, the second contact reaction is carried out (the reaction is carried out at 0℃ for 2 h, then the temperature is raised to 40℃ and the reaction is carried out at that temperature for 1 h) to obtain the second product system.
[0082] Slowly add the first portion of water to the second product system for dilution (the amount added is the same as the total weight of the raw material asphalt particles, concentrated sulfuric acid, and potassium permanganate), stir for 30 min, then raise the system temperature to 90℃, and add the second portion of water (the amount added is 1.5 times the weight of the first portion of water), and stir for 1 h; add hydrogen peroxide solution to the diluted system until no bubbles are generated, completely reducing the residual potassium permanganate in the system; then centrifuge the system (centrifuge speed is 10000 rpm, centrifugation time is 30 min), after centrifugation, pour off the supernatant, retain the solid product, wash the solid product with water, and centrifuge again to separate the solid. Repeat the above centrifugation and washing until the pH value of the centrifuged liquid reaches 6, so that the residual acid is cleaned off, and then dry to obtain oxidized asphalt particles;
[0083] (3) The above-mentioned oxidized asphalt particles and polyvinylpyrrolidone were melt-blended in a twin-screw extruder (the weight ratio of oxidized asphalt particles to polyvinylpyrrolidone was 1:0.25, and the melt-blending temperature was 160℃) to obtain modified asphalt particles (denoted as A3).
[0084] Preparation Example 4
[0085] This preparation example illustrates the preparation of modified asphalt particles.
[0086] The method of Preparation Example 1 is the same, except that in step (3), the weight ratio of oxidized asphalt particles to polyvinylpyrrolidone is 1:0.3, and the other steps and conditions are the same as in Preparation Example 1, to obtain modified asphalt particles (denoted as A4).
[0087] Preparation Example 5
[0088] This preparation example illustrates the preparation of modified asphalt particles.
[0089] The method of Preparation Example 1 is the same, except that in step (3), the weight ratio of oxidized asphalt particles to polyvinylpyrrolidone is 1:0.1. Other steps and conditions are the same as in Preparation Example 1, and modified asphalt particles (denoted as A5) are obtained.
[0090] Comparative Preparation Example 1
[0091] Asphalt particles were placed in a three-necked flask, and then concentrated sulfuric acid (98% by weight) and potassium permanganate were added simultaneously (the weight ratio of asphalt particles: concentrated sulfuric acid: potassium permanganate was 1:25:2). A violent reaction occurred, and a large amount of gas was generated during the reaction. The reaction was stopped after 5 minutes, and modified asphalt particles (denoted as DA1) were obtained.
[0092] Comparative Preparation Example 2
[0093] The method is the same as in Preparation Example 1, except that step (3) is omitted, and the oxidized asphalt particles obtained in step (2) are used as modified asphalt particles (denoted as DA2).
[0094] Comparative preparation example 3
[0095] The method of Preparation Example 1 is the same, except that in step (3), polyvinylpyrrolidone is replaced with an equal weight of 2-acrylamide-2-methylpropanesulfonic acid, and the other steps and conditions are the same as in Preparation Example 1, to obtain modified asphalt particles (denoted as DA3).
[0096] Example 1
[0097] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0098] Profile control composition: the above-mentioned modified asphalt particles A1 and sodium polyacrylate (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles A1 to sodium polyacrylate is 1:0.5;
[0099] Profile modifier: Add the modified asphalt particles A1 in the above composition to water (the weight ratio of modified asphalt particles A1 to water is 1:98.75) and mix for 5 minutes under mechanical stirring at 300 rpm to obtain a dispersion. Then add sodium polyacrylate in the above composition and continue stirring for 45 minutes to obtain the profile modifier (denoted as P1).
[0100] Example 2
[0101] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0102] Profile control composition: the above-mentioned modified asphalt particles A1 and polyacrylic acid (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles A1 to polyacrylic acid is 1:0.5;
[0103] Profile modifier: Add the modified asphalt particles A1 in the above composition to water (the weight ratio of modified asphalt particles A1 to water is 1:98.75) and mix for 5 minutes under mechanical stirring at 300 rpm to obtain a dispersion. Then add the polyacrylic acid in the above composition and continue stirring and mixing for 45 minutes to obtain the profile modifier (denoted as P2).
[0104] Example 3
[0105] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0106] Profile control composition: the above-mentioned modified asphalt particles A2 and polyacrylic acid (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles A2 to polyacrylic acid is 1:0.5;
[0107] Profile modifier: Add the modified asphalt particles A2 in the above composition to water (the weight ratio of modified asphalt particles A2 to water is 1:98.75) and mix for 5 minutes under mechanical stirring at 300 rpm to obtain a dispersion. Then add the polyacrylic acid in the above composition and continue stirring for 45 minutes to obtain the profile modifier (denoted as P3).
[0108] Example 4
[0109] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0110] Profile control composition: the above-mentioned modified asphalt particles A3 and polyacrylic acid (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles A3 to polyacrylic acid is 1:0.5;
[0111] Profile modifier: Add the modified asphalt particles A3 in the above composition to water (the weight ratio of modified asphalt particles A3 to water is 1:98.75) and mix for 5 minutes under mechanical stirring at 300 rpm to obtain a dispersion. Then add the polyacrylic acid in the above composition and continue stirring for 45 minutes to obtain the profile modifier (denoted as P4).
[0112] Example 5
[0113] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0114] Profile control composition: the above-mentioned modified asphalt particles A4 and polyacrylic acid (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles A4 to polyacrylic acid is 1:0.5;
[0115] Profile modifier: Add the modified asphalt particles A4 from the above composition to water (the weight ratio of modified asphalt particles A4 to water is 1:98.75) and mix for 5 minutes under mechanical stirring at 300 rpm to obtain a dispersion. Then add the polyacrylic acid from the above composition and continue stirring for 45 minutes to obtain the profile modifier (denoted as P5).
[0116] Example 6
[0117] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0118] Profile control composition: the above-mentioned modified asphalt particles A5 and polyacrylic acid (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles A5 to polyacrylic acid is 1:0.5;
[0119] Profile modifier: Add the modified asphalt particles A5 from the above composition to water (the weight ratio of modified asphalt particles A5 to water is 1:98.75) and mix for 5 minutes under mechanical stirring at 300 rpm to obtain a dispersion. Then add the polyacrylic acid from the above composition and continue stirring and mixing for 45 minutes to obtain the profile modifier (denoted as P6).
[0120] Example 7
[0121] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0122] Profile control composition: the above-mentioned modified asphalt particles A5 and hexadecyltrimethylammonium chloride, wherein the weight ratio of modified asphalt particles A5 to hexadecyltrimethylammonium chloride is 1:0.5;
[0123] Profile control agent: The profile control agent (denoted as P7) was prepared using the above composition according to the same steps and parameters as in Example 6.
[0124] Example 8
[0125] This embodiment is used to illustrate the profile control agent composition and profile control agent.
[0126] Profile control composition: the above-mentioned modified asphalt particles A5 and sodium dodecylbenzene sulfonate, wherein the weight ratio of modified asphalt particles A5 to sodium dodecylbenzene sulfonate is 1:0.5;
[0127] Profile control agent: The profile control agent (denoted as P8) was prepared using the above composition according to the same steps and parameters as in Example 6.
[0128] Comparative Example 1
[0129] Profile control composition: the above-mentioned modified asphalt particles DA1 and sodium polyacrylate (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles DA1 to sodium polyacrylate is 1:0.5;
[0130] Profile control agent: The profile control agent (denoted as DP1) was prepared using the above composition according to the same steps and parameters as in Example 1.
[0131] Comparative Example 2
[0132] Profile control composition: the above-mentioned modified asphalt particles DA2 and sodium polyacrylate (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles DA2 to sodium polyacrylate is 1:0.5;
[0133] Profile control agent: The profile control agent (denoted as DP2) was prepared using the above composition according to the same steps and parameters as in Example 1.
[0134] Comparative Example 3
[0135] Profile control composition: the above-mentioned modified asphalt particles DA3 and sodium polyacrylate (molecular weight of 3500 g / mol), wherein the weight ratio of modified asphalt particles DA3 to sodium polyacrylate is 1:0.5;
[0136] Profile control agent: The profile control agent (denoted as DP3) was prepared using the above composition according to the same steps and parameters as in Example 1.
[0137] Comparative Example 4
[0138] Profile modifier: Add the above modified asphalt particles A1 to water (the weight ratio of modified asphalt particles A1 to water is 1:98.75) and mix for 45 minutes under mechanical stirring at 300 rpm to obtain the profile modifier (denoted as DP4).
[0139] Test case
[0140] 1. Settlement test
[0141] The profile control agents P1-P8 and DP1-DP4 prepared in Examples 1-8 and Comparative Examples 1-4 were subjected to sedimentation tests at 25°C, and the results are shown in Table 1.
[0142] The states of profile control agents P1 and DP1 after 8 hours of static settling are as follows: Figure 2 As shown, by Figure 2 It is evident that the P1 system is stable, with almost no stratification, and the asphalt particles in DP1 have almost completely settled.
[0143] Settlement test procedure: At 25℃, the above-mentioned profile control agents P1-P8 and DP1-DP4 were placed into stoppered graduated cylinders and allowed to stand. The settling time of the asphalt particles (the time required for the asphalt particles to settle completely) and the water separation of the profile control agent were observed (the water separation is the clear liquid that precipitates from the upper layer of the profile control agent after standing). The water separation rate of the profile control agent was calculated according to the following formula.
[0144] Where Q represents the water separation rate (%), V1 represents the total volume of the profile control agent (mL), and V2 represents the system of water separated by the profile control agent (mL).
[0145] Table 1
[0146] Profile control agent Are the asphalt particles evenly dispersed? Settling time / h 8h water separation rate / % P1 yes 72 0 P2 yes 24 25 P3 yes 32 20 P4 yes 28 30 P5 yes 24 25 P6 yes 26 30 P7 yes 28 25 P8 yes 32 15 DP1 no 0 100 DP2 no 0 100 DP3 yes 10 60 DP4 no 0 100
[0147] Note: In Table 1, a water separation rate of 0% indicates that almost no water separation occurs; a water separation rate of 100% indicates that almost all asphalt particles in the system have settled; a settling time of 0h indicates that the asphalt particles in the system settle immediately after standing, and settle almost completely in a very short time.
[0148] As shown in Table 1, the profile control agents P1-P8 prepared using the profile control agent composition provided by this invention exhibit excellent stability. In the aforementioned settling tests, they can achieve a settling time of asphalt particles ≥20h and a water separation rate ≤30% after 8h, thus demonstrating excellent injectability. Among them, profile control agent P1 has a particularly outstanding advantage, achieving a settling time of asphalt particles up to 72h and almost no water separation after 8h. In contrast, profile control agents DP1-DP4 have shorter settling times and poorer injectability.
[0149] 2. Sealing test
[0150] The profile control agents P1 and DP1-DP4 prepared in Example 1 and Comparative Examples 1-4, respectively, were used for plugging tests, and the process is as follows:
[0151] (1) To the sand-filled pipe (permeability 3.9μm) 2 Inject steam (steam temperature 350℃) and continue injecting steam until the pressure is constant, and record the pressure P1;
[0152] (2) Stop injecting steam and wait for the temperature of the sand-filled pipe to stabilize before injecting 1PV profile control agent using a plunger pump.
[0153] (3) Simulate well simmering by wrapping the sand-filled pipe with insulation cotton and then wrapping the insulation cotton with tin foil for 8 hours;
[0154] (4) Continue to introduce steam (steam temperature is 350℃) and use steam to continuously displace until the pressure is constant. Record the pressure P2 at this time.
[0155] (5) According to the formula The vapor phase plugging rate (%) was calculated, and the results are shown in Table 2.
[0156] Table 2
[0157]
[0158]
[0159] As shown in Table 2, profile control agent P1 has a very good sealing effect, with a sealing rate of 98%. However, profile control agents DP1, DP2, and DP4 cannot effectively seal due to their very poor injectability. Although DP3 has relatively better injectability than DP1, DP2, and DP4, and can inject a certain amount of modified asphalt particles, its injectability is not as good as P1, and its sealing effect cannot reach that of P1.
[0160] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A profile control composition comprising: Modified asphalt particles and additives; wherein the weight ratio of the modified asphalt particles to the additives is 1:(0.25-1); The additive is selected from sodium polyacrylate; The method for preparing the modified asphalt particles includes: (1) The asphalt particles are reacted with acid in a first contact reaction to obtain a first product system; the weight ratio of the asphalt particles to the acid is 1:(10-40); the conditions for the first contact reaction include: the reaction temperature is -5 to 5℃ and the reaction time is 45-60 min. (2) The first product system is subjected to a second contact reaction with an oxidant to obtain a second product system, and the second product system is separated to obtain oxidized asphalt particles; the weight ratio of the asphalt particles to the oxidant is 1:(1-3); the conditions for the second contact reaction include: first reacting at a temperature of -5 to 10°C for 2-2.5h, and then heating up and reacting at a temperature of 40-45°C for 0.5-1h; (3) The oxidized asphalt particles and the modifier are melt-blended to obtain modified asphalt particles; the weight ratio of the oxidized asphalt particles to the modifier is 1:(0.1-0.3); the melt-blending temperature is 150-180℃; The modifier is polyvinylpyrrolidone.
2. The composition according to claim 1, wherein, The particle size of the asphalt particles is 75-125 μm; And / or, the softening point of the asphalt particles is 120-280℃; And / or, the acid is selected from concentrated sulfuric acid and / or concentrated nitric acid.
3. The composition according to claim 2, wherein, The softening point of the asphalt particles is 150-160℃; And / or, the acid is concentrated sulfuric acid.
4. The composition according to claim 1, wherein, The oxidant is selected from at least one of potassium permanganate, potassium dichromate, and tert-butyl hydroperoxide.
5. The composition according to claim 4, wherein, The oxidant is potassium permanganate.
6. A profile control agent, characterized in that, The profile control agent is obtained by mixing raw materials containing the composition of any one of claims 1-5 with water; The modified asphalt particles in the composition have a weight ratio of 1:(98-99.5) to water.
7. The application of the composition according to any one of claims 1-5 or the profile control agent according to claim 6 in steam drive sealing of heavy oil reservoirs.
Citation Information
Patent Citations
Asphalt composition particle and preparation method thereof
CN103102705A
Granular asphalt profile control and water plugging agent and preparation method thereof