Thermoelectric power generation device based on transient liquid phase connection and preparation method thereof
Through the combination of the transient liquid phase connection process and the conductive metal layer auxiliary welding layer, the problem of adverse effects on materials and mismatch of thermal expansion coefficients caused by high-temperature welding of thermoelectric power generation devices in the traditional brazing process is solved, achieving low-temperature bonding and high-temperature service. , improving the conversion efficiency and stability of GeTe-based thermoelectric power generation devices.
Patent Information
- Application Number
- CN202410739581.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-18
AI Technical Summary
When preparing GeTe-based thermoelectric power generation devices using the traditional brazing process, it is difficult to ensure high conversion efficiency and long-term stability at the same time. High-temperature welding temperatures are detrimental to the material, while low-temperature welding cannot bring out the best performance of the material, and the thermal expansion coefficient of the metal electrode is ignored. Thermal stress concentration problem caused by.
The transient liquid phase connection process is used to connect thermoelectric materials and electrodes at low temperatures through conductive metal layers and auxiliary welding layers (such as Ni layers) to buffer the problem of mismatch in thermal expansion coefficients, form high-melting-point intermetallic compounds, and achieve low-temperature bonding , high temperature service.
It improves the service reliability of the joint, breaks the operating temperature bottleneck limited by traditional brazing, achieves high conversion efficiency and long-term stability of thermoelectric power generation devices, and is suitable for higher operating temperatures.
Smart Images

Figure CN118804663A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of thermoelectric technology, and in particular relates to a thermoelectric power generation device based on transient liquid phase connection and a preparation method thereof. Background Art
[0002] Based on the Seebeck effect, thermoelectric power generation devices can directly convert thermal energy into electrical energy through the directional movement of carriers inside the material. Due to their many advantages such as small size, light weight, noiseless operation, clean and environmentally friendly, they are widely used in portable power supplies, waste heat recovery, environmental monitoring, space exploration and other fields.
[0003] Radioisotope thermoelectric generator (RTG) is one of the typical examples. It is the only power supply system available for deep space exploration so far. It is equipped on many spacecraft, such as the Apollo lunar module, Pioneer, Viking, Voyager, Galileo and Ulysses spacecraft. Russian scientists have built more than 1,000 lighthouses near the Arctic Circle using devices similar to RTG, which have a maintenance-free life of 20 years. In terms of waste heat recovery, the BMW X6 Active Hybrid released by BMW uses high-temperature thermoelectric materials to cover the outer wall of the engine to directly recover the waste heat of the car from the engine body, and can recover up to more than ten kilowatts of energy; the U.S. Department of Energy announced a "Advanced Thermoelectric Materials for Industrial Waste Heat Temperature Difference Power Generation" project on November 12, 2003, using waste heat from industrial high-temperature furnaces such as metallurgical furnaces to generate electricity to reduce energy consumption; Japan has established a "7500W-class garbage fuel waste heat power generation demonstration system" and achieved good practical results. In other aspects, the Matrix PowerWatch smartwatch launched by Indiegogo and the thermoelectric pacemaker developed by Biophan can use body heat to charge the device. The birth of many thermoelectric power generation devices proves that thermoelectric power generation devices have broad application prospects.
[0004] In actual production, the preparation of high-performance medium- and high-temperature thermoelectric devices depends on appropriate connection technology. For temperature-sensitive thermoelectric materials, due to the two factors that "the connection temperature in the traditional brazing process needs to be higher than the melting point of the brazing material" and "the operating temperature needs to be lower than the melting point of the brazing material", excessively high brazing temperatures will degrade the performance of thermoelectric materials, while lower brazing temperatures will not be able to achieve the best performance of thermoelectric devices.
[0005] Germanium telluride alloy (GeTe), as a medium-temperature thermoelectric material, can show excellent thermoelectric performance at 500K-773K through heterovalent doping and band degeneracy, which also means that the corresponding power generation device has very excellent thermal-electric conversion efficiency. The latest research shows that the average thermoelectric figure of merit of this material can exceed 1.8, and the theoretical conversion efficiency exceeds 20%. Therefore, the development and optimization of GeTe-based power generation devices is expected to break through the bottleneck of "low conversion efficiency" of thermoelectric power generation devices, and has great potential to develop into a commercially viable environmentally friendly energy device.
[0006] In fact, the conversion efficiency of GeTe power generation devices not only depends on the high performance of thermoelectric materials, but also on the quality of the device's joints, especially the interface performance between the connecting layer and the electrode. On the one hand, for the "thermoelectric material-connecting layer material-metal electrode" layered structure, how to reasonably select the connecting layer material to transition the thermal expansion coefficient between the thermoelectric material and the metal electrode to buffer the problem of thermal stress concentration caused by temperature changes is very important for the service reliability of the joint; on the other hand, GeTe materials can maintain stable performance below 773K and show a thermoelectric figure of merit that is proportional to the temperature, but above 773K, it is easy to experience degradation phenomena such as component volatilization and material softening, which is not conducive to long-term stable service.
[0007] There are the following problems in using traditional brazing process to prepare GeTe-based power generation devices: 1: In order to bring out the best performance of GeTe materials, higher melting point solders are used in the welding process, resulting in higher welding temperatures (>773K) during the connection process, which have adverse effects on GeTe materials and joints; 2: In order to ensure the stability of GeTe materials, lower melting point solders (<773K) are used in the welding process, resulting in the device being unable to bring out the best performance of the material during service.
[0008] At present, in order to select suitable connection layer materials for GeTe-based power generation devices, most researchers only focus on the thermal expansion coefficient matching (20-25×10 -6 K -1 ) Such as: Al 66 Si 34 , SnTe, TiAl, etc., but the small thermal expansion coefficient of the metal electrode after assembly (Cu: ~18×10 -6 K -1 ; Ni: ~15×10 -6 K -1 ) caused by thermal stress concentration; in the assembly of GeTe-based power generation devices, Ag-Cu-Zn and other high-melting-point solders are used for brazing (~850K), which cannot guarantee the performance of the assembled devices. Summary of the invention
[0009] The purpose of the present invention is to overcome at least one of the deficiencies of the above-mentioned prior art, and to provide a thermoelectric power generation device based on transient liquid phase connection and a preparation method thereof, which is beneficial to simultaneously ensure the high conversion efficiency and long-term service stability of the thermoelectric power generation device, and has a good application effect.
[0010] The technical solution of the present invention is: a thermoelectric power generation device based on transient liquid phase connection, including an n-type thermoelectric single arm and a p-type thermoelectric single arm, wherein the n-type thermoelectric single arm and the p-type thermoelectric single arm are connected to a substrate component through a transient liquid phase connection process.
[0011] Optionally, the p-type thermoelectric single arm is a GeTe-based power generation device, a bismuth telluride power generation device, a Zintl power generation device or a half-Heusler power generation device.
[0012] Optionally, the n-type thermoelectric single arm is a Mg3Sb2 thermoelectric single arm;
[0013] The Mg3Sb2 thermoelectric single arm comprises a Mg3Sb2 thermoelectric substrate, a first connection layer and a first auxiliary welding layer, wherein the first connection layer covers and connects to both ends of the Mg3Sb2 thermoelectric substrate respectively, and the first auxiliary welding layer covers and connects to the first connection layer respectively;
[0014] The first connection layer is a conductive metal layer, and the first auxiliary welding layer is a Ni layer.
[0015] Optionally, the p-type thermoelectric single arm is a germanium telluride-based thermoelectric single arm, and the germanium telluride-based thermoelectric single arm includes a germanium telluride thermoelectric substrate, a second connecting layer and a second auxiliary welding layer, the second connecting layer respectively covers and is connected to both ends of the germanium telluride thermoelectric substrate, and the second auxiliary welding layer respectively covers and is connected to the second connecting layer.
[0016] Optionally, the second connecting layer is a Ti—Al layer.
[0017] Optionally, the second auxiliary welding layer is a Ni layer.
[0018] The present invention also provides a method for preparing a thermoelectric power generation device based on transient liquid phase connection, which is used to prepare the above-mentioned thermoelectric power generation device based on transient liquid phase connection, comprising the following steps:
[0019] preparing an n-type thermoelectric single arm and a p-type thermoelectric single arm, wherein the p-type thermoelectric single arm is a germanium telluride-based thermoelectric single arm;
[0020] The n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are connected to the substrate component through a transient liquid phase connection process.
[0021] Optionally, the method for preparing the germanium telluride-based thermoelectric single arm comprises the following steps;
[0022] GeTe powder, Ti-Al powder and Ni powder are loaded into a graphite mold and sintered at 753K to 773K and 40MPa-50MPa for 8 to 12 minutes.
[0023] Optionally, the transient liquid phase connection process comprises the following steps:
[0024] After the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are placed on the substrate component, they are placed on the welding platform and heated to 150° C. to 170° C. under a pressure of 0.15 to 0.25 MPa;
[0025] The pressure is adjusted to 0.5 MPa to 0.7 MPa and the temperature is raised to 250°C to 270°C and kept at this temperature for 15 to 25 minutes. Finally, the pressure is maintained at 0.15 to 0.25 MPa and cooled to room temperature.
[0026] Optionally, the transient liquid phase connection process comprises the following steps:
[0027] Solder paste is placed on the end surfaces of the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm, and then placed on the substrate component and placed on the welding platform, and the temperature is raised to 160° C. under a pressure of 0.25 MPa;
[0028] The pressure was adjusted to 0.6 MPa, the temperature was raised to 260°C and kept at that temperature for 20 minutes, and then the pressure was maintained at 0.2 MPa and cooled to room temperature.
[0029] The present invention provides a thermoelectric power generation device based on transient liquid phase connection and a preparation method thereof, which adopts a "thermoelectric material-connection layer-auxiliary welding layer" structure to overcome the problem of thermal expansion coefficient mismatch between the contact layer and the auxiliary welding layer buffering thermoelectric material and the electrode, so that the entire joint has higher service reliability; a transient liquid phase connection process is used to achieve the connection between the thermoelectric device and the electrode at low temperature, and based on the high melting point of the full metal compound in the interface, it is ensured that the device can serve at a higher operating temperature with high efficiency, breaking the bottleneck of traditional brazing that limits the operating temperature of the thermoelectric power generation device, and realizing "low temperature bonding, high temperature service", which is beneficial to simultaneously ensure the high conversion efficiency and long-term service stability of the thermoelectric power generation device, and has a good application effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] FIG. 1( a ) is a schematic diagram of the structure of an n-type thermoelectric single arm and a p-type thermoelectric single arm in a thermoelectric power generation device based on transient liquid phase connection in this embodiment;
[0032] FIG1( b ) is a comparison diagram of the thermal expansion coefficients of the thermoelectric material, the contact layer material and the nickel auxiliary welding layer;
[0033] FIG1( c ) is the contact resistance of each interface of a single p-type thermoelectric arm in this embodiment;
[0034] FIG1( d ) shows the contact resistance of each interface of the n-type thermoelectric single arm in this embodiment;
[0035] Figure 2 (ad) are schematic diagrams of the intermetallic compound growth process at the interface of transient liquid phase bonding for 2, 5, 10 and 20 minutes in this embodiment, respectively;
[0036] Figure 2 (eh) is a schematic diagram of the structural evolution process of the full intermetallic compound interface in this embodiment after isothermal aging for 120, 240, 360 and 480 hours at 773K;
[0037] FIG3(a) is a measured diagram showing the change in contact resistance of the full intermetallic compound interface at different isothermal aging times at 773K;
[0038] Figure 3(b) is a measured graph showing the change in shear strength of the full intermetallic compound interface at different isothermal aging times at 773K.
[0039] FIG4( a ) is a graph showing the voltage-current correspondence of a GeTe-based thermoelectric power generation device prepared based on transient liquid phase connection at different temperature differences;
[0040] FIG4( b ) is a measured result of the output power-current of a thermoelectric power generation device based on transient liquid phase connection in this embodiment;
[0041] FIG4( c ) is a measured result of efficiency-current of a thermoelectric power generation device based on transient liquid phase connection in this embodiment;
[0042] FIG4(d) shows the change in maximum conversion efficiency of a thermoelectric power generation device based on transient liquid phase connection and a traditional germanium telluride-based thermoelectric power generation device after serving for 150 hours at a temperature difference of 443K in this embodiment.
[0043] Figure 5 This is a measured comparison of the long-term service efficiency of GeTe-based thermoelectric power generation devices prepared by transient liquid phase connection and traditional brazing. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0045] It should be noted that the terms “setting” and “connection” should be understood in a broad sense. For example, it can be directly setting or connecting, or it can be indirectly setting or connecting through a central component or a central structure.
[0046] In addition, in the embodiments of the present invention, if there are terms indicating orientation or positional relationships such as "longitudinal", "transverse", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., they are based on the orientation or positional relationships or conventional placement states or usage states shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the structure, feature, device or element referred to must have a specific orientation or positional relationship, nor must it be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0047] The various specific technical features and embodiments described in the specific implementation methods can be combined in any suitable manner unless there is any contradiction. For example, different implementation methods can be formed by combining different specific technical features / embodiments. In order to avoid unnecessary repetition, the various possible combinations of the specific technical features / embodiments in the present invention will not be described separately.
[0048] As shown in FIG1( a ), a thermoelectric power generation device based on transient liquid phase connection provided in an embodiment of the present invention includes an n-type thermoelectric single arm and a p-type thermoelectric single arm, wherein the n-type thermoelectric single arm and the p-type thermoelectric single arm are connected to a substrate component through a transient liquid phase connection process, and adopts low-temperature bonding and high-temperature service technology, which is beneficial to simultaneously ensure high conversion efficiency and long-term service stability of the thermoelectric power generation device, and has a good application effect.
[0049] Specifically, the p-type thermoelectric single arm is a germanium telluride-based thermoelectric single arm, and the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are connected to the substrate component through a transient liquid phase connection process. The n-type thermoelectric single arm can be selected from a Mg3Sb2 thermoelectric single arm, and the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are connected to the electrode of the substrate component through a transient liquid phase connection process, and the low-temperature bonding and high-temperature service technology are used, which is conducive to ensuring the high conversion efficiency and long-term service stability of the GeTe-based power generation device at the same time, and the application effect is good.
[0050] Specifically, the Mg3Sb2 thermoelectric single arm includes a Mg3Sb2 thermoelectric substrate 110, a first connection layer 111 and a first auxiliary welding layer 112, wherein the first connection layer 111 covers and connects to both ends of the Mg3Sb2 thermoelectric substrate 110, and the first auxiliary welding layer 112 covers and connects to the first connection layer 111; the first connection layer 111 is a conductive metal layer, and the first auxiliary welding layer 112 is a Ni layer. The conductive metal layer can be a stainless steel layer (material: 304SS).
[0051] Specifically, the p-type thermoelectric single arm can be a GeTe-based power generation device (single arm), a bismuth telluride power generation device (low temperature domain), a Zintl power generation device (medium temperature domain) or a half-Heusler power generation device (high temperature domain). By using low-temperature solder (the second connection layer of the p-type thermoelectric single arm) and the corresponding electrodes to fully react to form a high melting point (650-1221K) intermetallic compound (Cu-Sn, Ag-Sn, Ni-Sn and Al-based intermetallic compound, etc.), the melting point of the intermetallic compound is higher than 650K, which meets the corresponding higher temperature service conditions. In this embodiment, the germanium telluride-based thermoelectric single arm includes a germanium telluride thermoelectric substrate 210, a second connecting layer 211 and a second auxiliary welding layer 212. The second connecting layer 211 respectively covers and is connected to both ends of the germanium telluride thermoelectric substrate 210. The second auxiliary welding layer 212 respectively covers and is connected to the second connecting layer 211. The second connecting layer 211 is a Ti-Al layer, and the second auxiliary welding layer 212 is a Ni layer. The germanium telluride thermoelectric substrate 210, the second connecting layer 211 and the second auxiliary welding layer 212 can be sintered to form a structure of Ni layer, Ti-Al layer, germanium telluride thermoelectric substrate 210, Ti-Al layer, and Ni layer from top to bottom.
[0052] In this embodiment, the n-type thermoelectric single arm (Mg3Sb2 thermoelectric single arm) has a structure of Ni layer, conductive metal layer (304SS stainless steel layer), Mg3Sb2 thermoelectric substrate, conductive metal layer (304SS stainless steel layer), and Ni layer from top to bottom.
[0053] Specifically, the substrate component may include a ceramic substrate and a plurality of electrodes disposed on the surface of the ceramic substrate. Two ceramic substrates may be provided, and the two ceramic substrates are disposed parallel to each other up and down, and each electrode is disposed on the opposite surfaces of the two ceramic substrates, respectively, for connecting each n-type thermoelectric single arm and germanium telluride-based thermoelectric single arm. Each n-type thermoelectric single arm and germanium telluride-based thermoelectric single arm are disposed between the two ceramic substrates, and an n-type thermoelectric single arm and an adjacent germanium telluride-based thermoelectric single arm are disposed adjacent to each other to form a pair of thermoelectric components. The Ni layer of the same end (for example, the lower end) of the same pair of thermoelectric components can be welded to the same electrode on the surface of the ceramic substrate of the lower layer. In a pair of adjacent thermoelectric components, the upper end of an n-type thermoelectric single arm and the upper end Ni layer of a germanium telluride-based thermoelectric single arm can be welded to the same electrode on the surface of the ceramic substrate of the upper layer. In specific applications, the number and arrangement of n-type thermoelectric single arms and germanium telluride-based thermoelectric single arms can be selected and applied according to actual needs.
[0054] The embodiment of the present invention further provides a method for preparing a thermoelectric power generation device based on transient liquid phase connection, which is used to prepare the above-mentioned thermoelectric power generation device based on transient liquid phase connection, comprising the following steps:
[0055] Prepare an n-type thermoelectric single arm and a p-type thermoelectric single arm, wherein the n-type thermoelectric single arm may be a Mg3Sb2 thermoelectric device, and the p-type thermoelectric single arm is a germanium telluride-based thermoelectric single arm;
[0056] The n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are connected to the substrate component through a transient liquid phase connection process. The low-temperature bonding and high-temperature service technology is used to ensure the high conversion efficiency and long-term service stability of the GeTe-based power generation device at the same time, and the application effect is good.
[0057] Specifically, the method for preparing the germanium telluride-based thermoelectric single arm comprises the following steps:
[0058] GeTe powder (TAGS-Pb; 4.2 g; thickness after sintering is about 5 mm), Ti-Al powder (Ti-34Al; 0.1 g; thickness after sintering is about 100 μm), and Ni powder (0.2 g; thickness after sintering is about 200 μm) are placed in a graphite mold with a diameter of 12.7 mm, and sintered at 753K to 773K and 40MPa-50 MPa for 8 to 12 minutes. That is, in the germanium telluride-based thermoelectric single arm, the thickness of the germanium telluride thermoelectric matrix 210 is 4.5 to 5.5 mm (5 mm in this embodiment), the thickness of the second connection layer is 80 to 120 μm (100 μm in this embodiment), and the thickness of the second auxiliary welding layer is 160 to 240 μm (200 μm in this embodiment).
[0059] Specifically, the TAGS-Pb material is (Ge 0.85 Pb 0.15 Te)0.8 (Ag 0.98 Sb 1.02 Te2) 0.2 .
[0060] Specifically, the transient liquid phase connection process includes the following steps:
[0061] After the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are placed on the substrate component, they are placed on the welding platform and heated to 150° C. to 170° C. under a pressure of 0.15 to 0.25 MPa;
[0062] The pressure is adjusted to 0.5 MPa to 0.7 MPa and the temperature is raised to 250°C to 270°C and kept at this temperature for 15 to 25 minutes. Finally, the pressure is maintained at 0.15 to 0.25 MPa and cooled to room temperature.
[0063] In this embodiment, the transient liquid phase connection process includes the following steps:
[0064] Solder paste is placed on the end surfaces of the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm, and then placed on the substrate component and placed on the welding platform, and the temperature is raised to 160° C. under a pressure of 0.25 MPa;
[0065] The pressure was adjusted to 0.6 MPa, the temperature was raised to 260°C and kept at that temperature for 20 minutes, and then the pressure was maintained at 0.2 MPa and cooled to room temperature.
[0066] In this embodiment, the GeTe-based thermoelectric power generation device is composed of 7 n-type Mg3Sb2 single arms and 7 p-type GeTe single arms. The preparation process of the p-type GeTe single arm can be as follows: GeTe powder, Ti-Al powder and Ni powder are loaded into a graphite mold and sintered at 773K, 45MPa for 10 minutes. Further, the 7 pairs of n-type and p-type single arms are connected to the electrode-covered ceramic plate (substrate component) through a transient liquid phase connection process. The specific steps are as follows: Use a 100-micron steel plate to evenly brush SAC305 solder paste on the electrode of the substrate component, place the Mg3Sb2 single arm and 7 p-type GeTe single arms one by one and place them on the welding platform. Heat to 160°C under a pressure of 0.2MPa, further adjust to 0.6MPa, heat to 260°C and keep warm for 20 minutes, and finally maintain a pressure of 0.2MPa and cool to room temperature.
[0067] In Figure 1, (a) is a schematic diagram of the structure of n-type and p-type thermoelectric single arms; (b) is a comparison of the thermal expansion coefficients of thermoelectric materials, contact layer materials and nickel auxiliary welding layers; (c) is the contact resistance of each interface of the p-type thermoelectric single arm; (d) is the contact resistance of each interface of the n-type thermoelectric single arm.
[0068] Figure 2In the figure, (ad) are the intermetallic compound growth processes at the interface of transient liquid phase bonding for 2, 5, 10 and 20 minutes; (eh) are the structural evolution processes of the full intermetallic compound interface after isothermal aging for 120, 240, 360 and 480 hours at 773K.
[0069] FIG3(a) is a measured graph showing the change in contact resistance of the full intermetallic compound interface at different isothermal aging times at 773K, and FIG3(b) is a measured graph showing the change in shear strength of the full intermetallic compound interface at different isothermal aging times at 773K.
[0070] In Figure 4, (a) is the voltage-current corresponding measured diagram of the GeTe-based thermoelectric power generation device prepared based on transient liquid phase connection under different temperature differences, (b) is the measured result of output power-current, (c) is the measured result of efficiency-current; (d) is the change of maximum conversion efficiency after 150 hours of service at a temperature difference of 443K.
[0071] Figure 5 This is a measured comparison of the long-term service efficiency of GeTe-based thermoelectric power generation devices prepared by transient liquid phase connection and traditional brazing. The efficiency of the GeTe-based thermoelectric power generation device with transient liquid phase connection in this embodiment is significantly higher.
[0072] In the embodiment of the present invention, based on the interface reliability and "low temperature bonding, high temperature service" as the starting point, the GeTe-based thermoelectric power generation device was prepared at 533K for the first time using the transient liquid phase connection process and successfully applied in the working environment of 773K at the hot end and 300K at the cold end. Among them, by introducing the Ti-Al layer and the nickel layer, the transition of the thermal expansion coefficient of the thermoelectric material, the contact layer material, the auxiliary connection layer and the electrode was successfully achieved, and the service reliability of the overall joint was improved.
[0073] The present invention proposes a GeTe-based power generation device based on transient liquid phase connection and its preparation method. Compared with the GeTe-based power generation devices that have been reported, the "thermoelectric material substrate-connection layer-auxiliary welding layer" structure proposed in the present invention and the device prepared by using the "transient liquid phase connection process" are more superior in improving the long-term service stability of thermoelectric power generation devices. Compared with the GeTe-based power generation devices that have been reported so far, the "thermoelectric material-connection layer-auxiliary welding layer" structure starts from the overall structure, overcomes the problem of mismatch in thermal expansion coefficients between the contact layer and the auxiliary welding layer buffering thermoelectric material and the electrode, and makes the entire joint have higher service reliability; the transient liquid phase connection process is used to realize the connection between the thermoelectric single arm and the electrode at low temperature, and the high melting point of the full metal compound in the interface ensures that the device can serve at a higher working temperature with high efficiency, breaking the bottleneck of traditional brazing that limits the working temperature of thermoelectric power generation devices, and realizing "low temperature bonding, high temperature service". In addition to GeTe-based power generation devices, low-temperature bismuth telluride power generation devices, medium-temperature Zint l power generation devices, and high-temperature half-Heusler power generation devices can all utilize transient liquid phase connection technology to fully react with low-temperature solder and corresponding electrodes to form high-melting-point intermetallic compounds (Cu-Sn, Ag-Sn, Ni-Sn, and Al-based intermetallic compounds, etc.), thereby meeting the corresponding higher temperature service conditions. The proposal of preparing thermoelectric power generation devices based on the thermoelectric transient liquid phase connection process simplifies and enriches the ideas and concepts of medium and high temperature thermoelectric power generation device assembly, and has important scientific significance and application value.
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A thermoelectric power generation device based on transient liquid phase connection, characterized in that: It comprises an n-type thermoelectric single arm and a p-type thermoelectric single arm, wherein the n-type thermoelectric single arm and the p-type thermoelectric single arm are connected to a substrate component through a transient liquid phase connection process.
2. A thermoelectric power generation device based on transient liquid phase connection according to claim 1, characterized in that: The p-type thermoelectric single arm is a GeTe-based power generation device, a bismuth telluride power generation device, a Zintl power generation device or a half-Heusler power generation device.
3. A thermoelectric power generation device based on transient liquid phase connection according to claim 1, characterized in that: The n-type thermoelectric single arm is a Mg3Sb2 thermoelectric single arm; The Mg3Sb2 thermoelectric single arm comprises a Mg3Sb2 thermoelectric substrate, a first connection layer and a first auxiliary welding layer, wherein the first connection layer covers and connects to both ends of the Mg3Sb2 thermoelectric substrate respectively, and the first auxiliary welding layer covers and connects to the first connection layer respectively; The first connection layer is a conductive metal layer, and the first auxiliary welding layer is a Ni layer.
4. A thermoelectric power generation device based on transient liquid phase connection according to any one of claims 1 to 3, characterized in that: The p-type thermoelectric single arm is a germanium telluride-based thermoelectric single arm, which includes a germanium telluride thermoelectric substrate, a second connecting layer and a second auxiliary welding layer, wherein the second connecting layer is respectively covered and connected to both ends of the germanium telluride thermoelectric substrate, and the second auxiliary welding layer is respectively covered and connected to the second connecting layer.
5. A thermoelectric power generation device based on transient liquid phase connection according to claim 4, characterized in that: The second connection layer is a Ti—Al layer.
6. A thermoelectric power generation device based on transient liquid phase connection according to claim 4, characterized in that: The second auxiliary welding layer is a Ni layer.
7. A method for preparing a thermoelectric power generation device based on transient liquid phase connection, characterized in that: The method for preparing a thermoelectric power generation device based on transient liquid phase connection according to any one of claims 1 to 6 comprises the following steps: preparing an n-type thermoelectric single arm and a p-type thermoelectric single arm, wherein the p-type thermoelectric single arm is a germanium telluride-based thermoelectric single arm; The n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are connected to the substrate component through a transient liquid phase connection process.
8. The preparation method according to claim 7, characterized in that: The method for preparing the germanium telluride-based thermoelectric single arm comprises the following steps: GeTe powder, Ti-Al powder and Ni powder are loaded into a graphite mold and sintered at 753K to 773K and 40MPa-50MPa for 8 to 12 minutes.
9. The preparation method according to claim 7 or 8, characterized in that: The transient liquid phase connection process comprises the following steps: After the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm are placed on the substrate component, they are placed on the welding platform and heated to 150° C. to 170° C. under a pressure of 0.15 to 0.25 MPa; The pressure is adjusted to 0.5 MPa to 0.7 MPa and the temperature is raised to 250°C to 270°C and kept at this temperature for 15 to 25 minutes. Finally, the pressure is maintained at 0.15 to 0.25 MPa and cooled to room temperature.
10. The preparation method according to claim 7 or 8, characterized in that: The transient liquid phase connection process comprises the following steps: Solder paste is placed on the end surfaces of the n-type thermoelectric single arm and the germanium telluride-based thermoelectric single arm, and then placed on the substrate component and placed on the welding platform, and the temperature is raised to 160° C. under a pressure of 0.25 MPa; The pressure was adjusted to 0.6 MPa, the temperature was raised to 260°C and kept at that temperature for 20 minutes, and then the pressure was maintained at 0.2 MPa and cooled to room temperature.