Multi-fluoride mixing method
By freezing polyfluorides into solid powder and performing multi-stage in-phase mixing, the problem of homogeneous mixing of polyfluorides with large differences in melting and boiling points is solved, and the precise ratio and uniformity of molybdenum hexafluoride and tungsten hexafluoride are achieved. The quality state meets the measurement needs of distillation gas-liquid phase equilibrium data and promotes the development of dry uranium purification technology.
Patent Information
- Application Number
- CN202410859080.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-22
Smart Images

Figure CN118807593A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of uranium distillation and purification, and in particular relates to a mixing method of polynary fluorides. Background Art
[0002] Uranium purification conversion is a process of processing uranium concentrate into nuclear-grade uranium hexafluoride, which is an indispensable part of the nuclear fuel cycle. At present, there are two technical routes for preparing nuclear-grade uranium hexafluoride in the world: wet process and dry process. The dry process has become a recognized advanced uranium purification technology due to its low cost and good environmental protection. The key technology of the dry process is distillation purification. However, the research on dry uranium purification in China is basically blank, and a large amount of basic data is missing, especially the key distillation technology in dry uranium purification is less studied.
[0003] In the study of obtaining data on the distillation and purification of uranium hexafluoride, it is necessary to homogenously mix the multi-component fluoride components and determine the gas-liquid phase equilibrium data of the components respectively. The miscellaneous fluoride components commonly used in data determination are generally molybdenum hexafluoride, tungsten hexafluoride, and vanadium pentafluoride, among which the melting point of vanadium pentafluoride is 19.0℃, the boiling point is 48.5℃, the melting point of tungsten hexafluoride is 2.0℃, the boiling point is 17.0℃, and the melting point of molybdenum hexafluoride is 17.5℃, and the boiling point is 35℃. For the mixing of vanadium pentafluoride and molybdenum hexafluoride, since the melting and boiling points are relatively similar, they can be mixed in the same phase state. The same phase state can generally achieve accurate metering and uniform mixing of materials, and it is easier to achieve the purpose of homogeneous mixing. However, for the mixture of molybdenum hexafluoride and tungsten hexafluoride, or the mixture of vanadium pentafluoride and tungsten hexafluoride, due to the large difference in their melting and boiling points and the different phases of the two at room temperature and pressure, it is difficult to achieve precise ratio control of the materials and the homogeneous state of the two after mixing, especially in the gas-solid, gas-liquid, and liquid-solid states. It is almost impossible to achieve homogeneous mixing.
[0004] For materials with large differences in melting and boiling points, there is currently a lack of suitable mixing methods, which restricts the determination of data. Therefore, it is urgent to develop a new mixing method to achieve accurate quantitative and homogeneous mixing of molybdenum hexafluoride (or vanadium pentafluoride) and tungsten hexafluoride mixed materials, so as to meet the needs of subsequent distillation gas-liquid phase equilibrium data determination and promote the development of dry uranium purification technology. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a mixing method of polyfluorides. The mixing method of the present invention can achieve accurate quantitative and homogeneous mixing in the preparation of molybdenum hexafluoride (or vanadium pentafluoride) and tungsten hexafluoride mixed materials, meeting the requirements of subsequent distillation gas-liquid phase equilibrium data determination.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for mixing multi-element fluorides, wherein the multi-element fluorides include a first fluoride and a second fluoride, wherein the first fluoride includes molybdenum hexafluoride and / or vanadium pentafluoride, and the second fluoride includes tungsten hexafluoride; the mixing method includes the following steps:
[0008] Freezing the first fluoride and the second fluoride to form solids respectively, crushing the solids to obtain first fluoride powder and second fluoride powder, blowing the first fluoride powder and the second fluoride powder into a pressure container by nitrogen or an inert gas for first mixing to obtain a fluoride powder mixture;
[0009] heating the fluoride powder mixture to gasify the fluoride for a second mixing to form a fluoride gaseous mixture;
[0010] Nitrogen or an inert gas is charged into the pressure container containing the fluoride gas mixture to pressurize the container, so as to liquefy the fluoride gas mixture and perform the third mixing to obtain a liquid homogeneously mixed multi-component fluoride.
[0011] Preferably, the moisture content and oxygen content of the original gas in the pressure container are both lower than 10 ppm.
[0012] Preferably, the freezing temperature is -5 to 0°C.
[0013] Preferably, the first mixing is: rotating and flipping the pressure container, the rotation speed is not less than 20 revolutions per minute, the flipping speed is not less than 6 times per minute; the rotation and flipping time is not less than 10 minutes.
[0014] Preferably, when the first fluoride is molybdenum hexafluoride, the heating temperature is above 40°C.
[0015] Preferably, when the first fluoride is vanadium pentafluoride, the heating temperature is above 52.5°C.
[0016] Preferably, the second mixing is: rotating and flipping the pressure container, the rotation speed is not less than 20 revolutions per minute, the flipping speed is not less than 6 times per minute; the rotation and flipping time is not less than 20 minutes.
[0017] Preferably, the time for pressurizing by filling with nitrogen or inert gas is no more than 10 seconds, and the pressure after filling with nitrogen or inert gas is 1 to 3 MPa.
[0018] Preferably, the third mixing is: rotating and flipping the pressure container, the rotation speed is not less than 20 revolutions per minute, the flipping speed is not less than 6 times per minute; the rotation and flipping time is not less than 10 minutes.
[0019] Preferably, the method further comprises: the liquid homogeneously mixed polyfluoride is discharged at a constant temperature and pressure during use, and nitrogen or an inert gas at the same temperature is added while the discharge is in progress.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention provides a method for mixing multi-element fluorides, wherein the fluorides include a first fluoride and a second fluoride, wherein the first fluoride includes molybdenum hexafluoride and / or vanadium pentafluoride, and the second fluoride includes tungsten hexafluoride; the mixing method includes the following steps:
[0022] Freezing the first fluoride and the second fluoride to form solids respectively, crushing the solids to obtain first fluoride powder and second fluoride powder, blowing the first fluoride powder and the second fluoride powder into a pressure container by nitrogen or an inert gas for first mixing to obtain a fluoride powder mixture;
[0023] heating the fluoride powder mixture to gasify the fluoride for a second mixing to form a fluoride gaseous mixture;
[0024] Nitrogen or an inert gas is charged into the pressure container containing the fluoride gas mixture to pressurize the container, so as to liquefy the fluoride gas mixture and perform the third mixing to obtain a liquid homogeneously mixed multi-component fluoride.
[0025] The present invention aims at the large difference in melting and boiling points between molybdenum hexafluoride (and / or vanadium pentafluoride) and tungsten hexafluoride, and the difficulty of homogenizing and mixing materials in different phases. When proportioning, molybdenum hexafluoride (and / or vanadium pentafluoride) and tungsten hexafluoride are accurately measured in the form of solid materials, and are added to the same mixing container respectively to achieve accurate proportioning; molybdenum hexafluoride (and / or vanadium pentafluoride) and tungsten hexafluoride are successively and fully mixed in the same phase and in stages in the form of solid and gaseous states to ensure the homogeneity of the multi-element fluoride material; then the molybdenum hexafluoride (or vanadium pentafluoride) and tungsten hexafluoride mixture are mixed in the form of pressurized liquid to further ensure the homogeneity of the multi-element fluoride material; the mixture is stored in the form of pressurized liquid. When in use, the material is discharged at a constant pressure, the stable state of the liquid is maintained, and the material after homogenization is prevented from being separated, so that the homogenized mixed material can be obtained, and finally the qualified raw material is provided for the determination of gas-liquid phase equilibrium data, and the accuracy of the determination process is guaranteed.
[0026] The data of the embodiment show that the mixing method of the present invention can achieve accurate proportioning and sufficient homogeneous mixing of molybdenum hexafluoride and tungsten hexafluoride, the material proportioning error is less than 0.5%, and the homogenization error is less than 0.3%, which meets the requirements of subsequent distillation gas-liquid phase equilibrium data determination and is conducive to promoting the development of dry uranium purification technology in my country. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 Schematic diagram of the homogeneous mixing process of molybdenum hexafluoride and tungsten hexafluoride in the embodiment. DETAILED DESCRIPTION
[0029] The present invention provides a multi-component mixing method of fluorides, wherein the fluorides include a first fluoride and a second fluoride, wherein the first fluoride includes molybdenum hexafluoride and / or vanadium pentafluoride, and the second fluoride includes tungsten hexafluoride; the mixing method includes the following steps:
[0030] Freezing the first fluoride and the second fluoride to form solids respectively, crushing the solids to obtain first fluoride powder and second fluoride powder, blowing the first fluoride powder and the second fluoride powder into a pressure container by nitrogen or an inert gas for first mixing to obtain a fluoride powder mixture;
[0031] heating the fluoride powder mixture to gasify the fluoride for a second mixing to form a fluoride gaseous mixture;
[0032] Nitrogen or an inert gas is charged into the pressure container containing the fluoride gas mixture to pressurize the container, so as to liquefy the fluoride gas mixture and perform the third mixing to obtain a liquid homogeneously mixed multi-component fluoride.
[0033] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.
[0034] The present invention freezes the first fluoride and the second fluoride to form solids, crushes the solids to obtain the first fluoride powder and the second fluoride powder, and uses nitrogen or an inert gas to blow the first fluoride powder and the second fluoride powder into a pressure container for first mixing to obtain a fluoride powder mixture.
[0035] In the present invention, the moisture content and oxygen content of the original gas in the pressure container are preferably lower than 10ppm. The pressure container is preferably a steel cylinder, and the material of the steel cylinder is preferably monel. The steel cylinder material of the present invention can prevent fluoride from corroding the steel cylinder, which causes the material to be impure. The steel cylinder is preferably provided with an air inlet, an air outlet, a feeding port and a discharge port. The steel cylinder is preferably pretreated before use, and the pretreatment method preferably includes: heating the steel cylinder and continuously introducing nitrogen; when the moisture content and oxygen content in the gas at the outlet of the steel cylinder drop below 10ppm, closing the air inlet and the air outlet for standby use. The heating temperature is preferably 100-150°C, more preferably 100-120°C; the time for continuously introducing nitrogen is preferably 1 hour.
[0036] In the present invention, the freezing temperature is preferably -5 to 0°C, more preferably -2°C.
[0037] In the present invention, the particle size after the pulverization is preferably less than 50 mesh, more preferably less than 100 mesh, and even more preferably less than 200 mesh. The pulverization also includes weighing, and the temperature during the weighing is preferably below 0°C. The present invention has no special requirements for the weighing method.
[0038] In the present invention, the pressure of nitrogen or inert gas used to blow the first fluoride powder and the second fluoride powder into the pressure container is preferably 0.2-0.5 MPa, and the time is preferably 1-2 seconds; the present invention has no special requirements on the order in which the first fluoride powder and the second fluoride powder are blown into the pressure container.
[0039] In the present invention, the first mixing is preferably: rotating and flipping the pressure container, the rotation speed is preferably not less than 20 rpm, more preferably 30-45 rpm, and more preferably 40 rpm; the flip speed is preferably not less than 6 times / minute, more preferably 8-10 times / minute; the rotation and flip time is preferably not less than 10 minutes, more preferably 15-30 minutes. The rotation and flipping are preferably performed simultaneously.
[0040] In the present invention, the first mixing preferably includes standing for more than 2 hours, more preferably 3 to 5 hours. After the solid material is completely settled, the pressurized gas is slowly released to normal pressure.
[0041] After obtaining the fluoride powder mixture, the present invention heats the fluoride powder mixture to gasify the fluoride and perform a second mixing to form a fluoride gaseous mixture.
[0042] In the present invention, when the first fluoride is molybdenum hexafluoride, the heating temperature is preferably above 40° C., more preferably 45-50° C.; when the first fluoride is vanadium pentafluoride, the heating temperature is preferably above 52.5° C., more preferably 53-60° C., and even more preferably 54° C. The present invention performs the heating to turn the fluoride into a gaseous state.
[0043] In the present invention, the second mixing is preferably carried out while maintaining the heating temperature to ensure that the adhered material on the pressure container is completely gasified and the gas is fully mixed. The second mixing is preferably: rotating and flipping the pressure container, the rotation speed is preferably not less than 20 rpm, more preferably 30-45 rpm, and more preferably 40 rpm; the flip speed is preferably not less than 6 times / minute, more preferably 8-10 times / minute; the rotation and flip time is preferably not less than 20 minutes, more preferably 30-40 minutes. The rotation and flipping are preferably carried out simultaneously.
[0044] After the fluoride gaseous mixture is formed, the present invention charges nitrogen or an inert gas into the pressure vessel containing the fluoride gaseous mixture to pressurize the vessel, so as to liquefy the fluoride gaseous mixture and perform a third mixing to obtain a liquid homogeneously mixed multi-component fluoride.
[0045] In the present invention, the time for charging with nitrogen or inert gas for pressurization is preferably no more than 10 seconds, more preferably 7 to 8 seconds; the pressure after charging with nitrogen or inert gas is preferably 1 to 3 MPa, more preferably 2 MPa; the time and pressure for charging with nitrogen or inert gas described in the present invention can make the fluoride liquefy quickly and synchronously, and will not cause the situation of slow liquefaction leading to asynchronous liquefaction of fluoride and inhomogeneous mixture.
[0046] In the present invention, the third mixing is preferably carried out at room temperature, and the third mixing is preferably: rotating and flipping the pressure container, the rotation speed is preferably not less than 20 rpm, more preferably 30-45 rpm, and more preferably 40 rpm; the flip speed is preferably not less than 6 times / minute, more preferably 8-10 times / minute; the rotation and flip time is preferably not less than 10 minutes, more preferably 20-30 minutes. The rotation and flipping are preferably carried out simultaneously.
[0047] In the present invention, the mixing method preferably further comprises: the liquid homogeneously mixed fluoride is preferably discharged at a constant temperature and pressure during use, and nitrogen or an inert gas at the same temperature is added while discharging the material to ensure that the fluoride is in a liquid state during discharging; the fluctuation range of the constant temperature and constant pressure is preferably controlled within 2%. The present invention maintains a constant temperature and constant pressure discharge, which can maintain a stable state of the liquid material to prevent the material from segregating after homogenization.
[0048] In the present invention, the constant pressure is preferably 1-3 MPa, more preferably 2 MPa; the constant temperature is preferably 20-30°C, more preferably 25°C. The discharge time is preferably 30-50 minutes, more preferably 40 minutes. At the end of the discharge, the liquid level is preferably 2 cm higher than the discharge port.
[0049] In order to further illustrate the present invention, the mixing method of the polyfluoride provided by the present invention is described in detail below with reference to the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0050] Example 1
[0051] (1) The monel cylinder was heated to 100°C and nitrogen was continuously introduced for 1 hour. The moisture content of the outlet gas was 8 ppm and the oxygen content was 3 ppm.
[0052] (2) Under 0°C, weigh 300g of molybdenum hexafluoride and tungsten hexafluoride powders smaller than 50 mesh, and quickly blow 0.2MPa nitrogen into the steel cylinder treated in step (1). The steel cylinder rotates at 20 rpm and turns at 6 times / min. The cylinder rotates and turns for 10 minutes and remains stationary for 2 hours. The pressurized nitrogen is slowly released to normal pressure.
[0053] (3) The steel cylinder treated in step (2) is heated to 45° C. and kept at 45° C. The steel cylinder is rotated at a speed of 20 revolutions per minute and turned over at a speed of 6 times per minute for 20 minutes.
[0054] (4) Immediately fill the steel cylinder treated in step (3) with nitrogen to 1 MPa for 8 seconds. The steel cylinder filled with nitrogen is rotated and flipped at a rotation speed of 20 rpm and a flipping speed of 6 times / min for 10 minutes.
[0055] (5) The steel cylinder treated in step (4) is discharged at 20° C. The discharge port is placed at the lower end. While slowly discharging, nitrogen gas at room temperature of 1 MPa is added. The temperature of the steel cylinder is maintained at 19.7-20.2° C., and the pressure is maintained at 0.98-1.01 MPa. The discharge is completed in about 30 minutes. When the discharge is completed, the liquid material is 3 cm higher than the discharge port.
[0056] Sampling was performed every 6 minutes to determine the proportions of molybdenum hexafluoride and tungsten hexafluoride in the material (still in the same phase). The results are shown in Table 1.
[0057] Table 1 Example 1 Measurement results
[0058]
[0059] Note: The proportion is the mass ratio of molybdenum hexafluoride or hexafluoride in the output material, with the total theoretical value being 1, and is determined by gas chromatography; Proportion error = (∣molybdenum hexafluoride proportion / tungsten hexafluoride proportion-1∣ / 1)*100%; Molybdenum hexafluoride homogeneity error = (∣Molybdenum hexafluoride proportion-0.5∣ / 0.5)*100%; Tungsten hexafluoride homogeneity error = (∣Tungsten hexafluoride proportion-0.5∣ / 0.5)*100%.
[0060] Example 2
[0061] (1) The monel cylinder was heated to 120°C and nitrogen was continuously introduced for 1 hour. The moisture content of the outlet gas was 10 ppm and the oxygen content was 6 ppm.
[0062] (2) Under -2°C, weigh 500g of molybdenum hexafluoride and tungsten hexafluoride powders with mesh size less than 200 and quickly blow 0.3MPa nitrogen into the steel cylinder treated in step (1). The steel cylinder rotates at a speed of 30 rpm and flips at a speed of 8 times / min. The cylinder rotates and flips for 15 minutes and remains stationary for 3 hours. The pressurized nitrogen is slowly released to normal pressure.
[0063] (3) The steel cylinder treated in step (2) is heated to 50° C. and kept at 50° C. The steel cylinder is rotated at a speed of 30 revolutions per minute and turned over at a speed of 8 times per minute for 30 minutes.
[0064] (4) Immediately fill the steel cylinder treated in step (3) with nitrogen to 2 MPa for 7 seconds. The steel cylinder filled with nitrogen is rotated and flipped at a rotation speed of 30 rpm and a flipping speed of 8 times / min for 20 minutes.
[0065] (5) The steel cylinder treated in step (4) is discharged at 25° C. The discharge port is placed at the lower end. While slowly discharging, nitrogen at 25° C. and 2 MPa is added. The temperature of the steel cylinder is maintained at 24.6-25.3° C., and the pressure is maintained at 1.97-2.02 MPa. The discharge takes about 40 minutes. When the discharge is completed, the liquid material is 2.5 cm higher than the discharge port.
[0066] Sampling was performed every 8 minutes to determine the proportions of molybdenum hexafluoride and tungsten hexafluoride in the material. The results are shown in Table 2.
[0067] Table 2 Example 2 Measurement results
[0068]
[0069] Example 3
[0070] (1) The monel cylinder was heated to 150°C and nitrogen was continuously introduced for 1 hour. The moisture content of the outlet gas was 8 ppm and the oxygen content was 10 ppm.
[0071] (2) Under -5°C, weigh 800g of molybdenum hexafluoride and tungsten hexafluoride powders with a mesh size less than 100, and quickly blow 0.5MPa nitrogen into the steel cylinder treated in step (1). The steel cylinder rotates at 40 rpm and turns at 10 times / min. The cylinder rotates and turns for 30 minutes and remains stationary for 5 hours. The pressurized nitrogen is slowly released to normal pressure.
[0072] (3) The steel cylinder treated in step (2) is heated to 45° C., kept at 45° C., rotated at 30 rpm, turned 10 times / min, and rotated and turned for 40 minutes.
[0073] (4) Immediately fill the steel cylinder treated in step (3) with nitrogen to 3 MPa for 10 seconds. The steel cylinder filled with nitrogen is rotated and flipped at a rotation speed of 30 revolutions per minute and a flipping speed of 8 times per minute for 30 minutes.
[0074] (5) The steel cylinder treated in step (4) is discharged at 30° C. The discharge port is placed at the lower end. While slowly discharging, nitrogen at 30° C. and 3 MPa is added. The temperature of the steel cylinder is maintained at 29.6-30.4° C., and the pressure is maintained at 2.96-3.04 MPa. The discharge is completed in about 50 minutes. When the discharge is completed, the liquid material is 4 cm higher than the discharge port.
[0075] Sampling was performed every 10 minutes to determine the proportions of molybdenum hexafluoride and tungsten hexafluoride in the material. The results are shown in Table 3.
[0076] Table 3 Example 3 Measurement results
[0077]
[0078] Example 4
[0079] (1) The monel cylinder was heated to 140°C and nitrogen was continuously introduced for 1 hour. The moisture content of the outlet gas was 7 ppm and the oxygen content was 6 ppm.
[0080] (2) Under -4°C, weigh 600g of vanadium pentafluoride and tungsten hexafluoride powders with a size less than 100 mesh, and quickly blow 0.5MPa nitrogen into the steel cylinder treated in step (1). The steel cylinder rotates at 45 rpm and turns at 10 times / min. The cylinder rotates and turns for 30 minutes and remains stationary for 5 hours. The pressurized nitrogen is slowly released to normal pressure.
[0081] (3) The steel cylinder treated in step (2) is heated to 54° C. and kept at 54° C. The steel cylinder is rotated at 45 rpm and turned 10 times / min for 40 minutes.
[0082] (4) Immediately fill the steel cylinder treated in step (3) with nitrogen to 2 MPa for 8 seconds. The steel cylinder filled with nitrogen is rotated and flipped at a rotation speed of 45 rpm and a flipping speed of 8 times / min for 30 minutes.
[0083] (5) The steel cylinder treated in step (4) is discharged at 25° C. The discharge port is placed at the lower end. While slowly discharging, nitrogen at 25° C. and 3 MPa is added. The temperature of the steel cylinder is maintained at 25.1-25.5° C., and the pressure is maintained at 1.95-2.04 MPa. The discharge is completed in about 50 minutes. When the discharge is completed, the liquid material is 3 cm higher than the discharge port.
[0084] Sampling was performed every 10 minutes to determine the proportions of vanadium pentafluoride and tungsten hexafluoride in the material. The results are shown in Table 3.
[0085] Table 4 Example 4 Measurement results
[0086]
[0087] Comparative Example 1
[0088] (1) The monel cylinder was heated to 120°C and nitrogen was continuously introduced for 1 hour. The moisture content of the outlet gas was 10 ppm and the oxygen content was 6 ppm.
[0089] (2) Under -2°C, weigh 500g of molybdenum hexafluoride and tungsten hexafluoride powders with mesh size less than 200 and quickly blow 0.3MPa nitrogen into the steel cylinder treated in step (1). The steel cylinder rotates at a speed of 30 rpm and flips at a speed of 8 times / min. The cylinder rotates and flips for 15 minutes and remains stationary for 3 hours. The pressurized nitrogen is slowly released to normal pressure.
[0090] (3) Immediately fill the steel cylinder treated in step (2) with nitrogen to 2 MPa for 7 seconds. The steel cylinder filled with nitrogen is rotated and flipped at a rotation speed of 30 rpm and a flipping speed of 8 times / min for 20 minutes.
[0091] (4) The steel cylinder treated in step (3) is discharged at 25° C. The discharge port is placed at the lower end. While slowly discharging, nitrogen at 25° C. and 2 MPa is added. The temperature of the steel cylinder is maintained at 24.4-25.2° C., and the pressure is maintained at 1.95-2.03 MPa. The discharge takes about 40 minutes. When the discharge is completed, the liquid material is 2.5 cm higher than the discharge port.
[0092] Sampling was performed every 8 minutes to determine the proportions of molybdenum hexafluoride and tungsten hexafluoride in the material. The results are shown in Table 5.
[0093] Table 5 Comparative Example 1 Measurement Results
[0094]
[0095] Comparative Example 2
[0096] (1) The monel cylinder was heated to 140°C and nitrogen was continuously introduced for 1 hour. The moisture content of the outlet gas was 7 ppm and the oxygen content was 6 ppm.
[0097] (2) Under -4°C, weigh 600g of vanadium pentafluoride and tungsten hexafluoride powders with a size less than 100 mesh, and quickly blow 0.5MPa nitrogen into the steel cylinder treated in step (1). The steel cylinder rotates at 45 rpm and turns at 10 times / min. The cylinder rotates and turns for 30 minutes and remains stationary for 5 hours. The pressurized nitrogen is slowly released to normal pressure.
[0098] (3) The temperature of the steel cylinder treated in step (2) was raised to 54° C., and then kept at 54° C. The steel cylinder was rotated at a speed of 45 rpm, flipped at a speed of 10 times / min, and rotated and flipped for 40 minutes.
[0099] (4) Immediately fill the steel cylinder treated in step (3) with nitrogen to 2 MPa for 8 seconds. The sample is liquefied and then discharged at 25° C. The discharge port is placed at the lower end. While slowly discharging, nitrogen at 25° C. and 3 MPa is added. The temperature of the steel cylinder is maintained at 25.0-25.5° C. and the pressure is maintained at 1.96-2.03 MPa. The discharge takes about 45 minutes. When the discharge is completed, the liquid material is 3 cm higher than the discharge port.
[0100] Sampling was performed every 10 minutes to determine the proportions of vanadium pentafluoride and tungsten hexafluoride in the material. The results are shown in Table 6.
[0101] Table 6 Comparative Example 2 Measurement Results
[0102]
[0103] Figure 1 The figure is a schematic diagram of the homogeneous mixing process of molybdenum hexafluoride and tungsten hexafluoride in the embodiment. In view of the large difference in melting and boiling points between molybdenum hexafluoride and tungsten hexafluoride, the embodiment of the present invention makes it difficult to homogeneously mix materials of different phases. When proportioning, the materials are accurately measured in the form of solid materials to achieve accurate proportioning; when mixing, they are successively mixed in the same phase and in stages in the form of solid, gaseous and liquid to ensure the homogeneity of the multi-element fluoride materials; when storing and using, the materials are discharged at a constant pressure and temperature in the form of liquid to prevent the segregation of the homogenized materials. The final material proportion error is less than 0.5%, and the homogenization error is less than 0.3%, which provides qualified raw materials for the determination of gas-liquid phase equilibrium data and ensures the accuracy of the determination process.
[0104] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for mixing polyfluorides, wherein the polyfluorides include a first fluoride and a second fluoride, wherein the first fluoride includes molybdenum hexafluoride and / or vanadium pentafluoride, and the second fluoride includes tungsten hexafluoride; the mixing method The following steps are involved: Freezing the first fluoride and the second fluoride to form solids respectively, crushing the solids to obtain first fluoride powder and second fluoride powder, blowing the first fluoride powder and the second fluoride powder into a pressure container by nitrogen or an inert gas for first mixing to obtain a fluoride powder mixture; heating the fluoride powder mixture to gasify the fluoride for a second mixing to form a fluoride gaseous mixture; Nitrogen or an inert gas is charged into the pressure container containing the fluoride gas mixture to pressurize the container, so as to liquefy the fluoride gas mixture and perform the third mixing to obtain a liquid homogeneously mixed multi-component fluoride.
2. The mixing method according to claim 1, It is characterized in that The moisture content and oxygen content of the original gas in the pressure container are both lower than 10 ppm.
3. The mixing method according to claim 1, It is characterized in that The freezing temperature is -5 to 0°C.
4. The mixing method according to claim 1, It is characterized in that The first mixing is: rotating and flipping the pressure container, the rotation speed is not less than 20 revolutions per minute, the flipping speed is not less than 6 times per minute; the rotation and flipping time is not less than 10 minutes.
5. The mixing method according to claim 1, It is characterized in that When the first fluoride is molybdenum hexafluoride, the heating temperature is above 40°C.
6. The mixing method according to claim 1, It is characterized in that When the first fluoride is vanadium pentafluoride, the heating temperature is above 52.5°C.
7. The mixing method according to claim 1 or 5 or 6, It is characterized in that The second mixing is: rotating and flipping the pressure container, the rotation speed is not less than 20 revolutions per minute, the flipping speed is not less than 6 times per minute; the rotation and flipping time is not less than 20 minutes.
8. The mixing method according to claim 1, It is characterized in that The time for filling with nitrogen or inert gas to pressurize is no more than 10 seconds, and the pressure after filling with nitrogen or inert gas is 1 to 3 MPa.
9. The mixing method according to claim 1 or 8, It is characterized in that The third mixing comprises: rotating and flipping the pressure container, wherein the rotation speed is not less than 20 revolutions per minute, and the flipping speed is not less than 6 times per minute; and the rotation and flipping time is not less than 10 minutes.
10. The mixing method according to claim 1, It is characterized in that Also includes: The liquid homogeneously mixed polyfluoride is discharged at a constant temperature and pressure during use, and nitrogen or inert gas at the same temperature is added while the discharge is in progress.
Citation Information
Cited By
Gas configuration system and method