High flow nylon copolymer and method for making same

By copolymerizing copolymer initiators with nylon monomers, the problem of high melt viscosity of nylon was solved, enabling the preparation of high-flow-rate nylon materials with better flowability and mechanical properties, suitable for the automotive and electronics industries.

CN118812839BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310416227.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2026-11-20
Estimated Expiration
2043-04-18

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0004185227820000061
    Figure BDA0004185227820000061
Patent Text Reader

Abstract

The present application relates to the field of high flow nylon preparation, in particular to a kind of high flow nylon copolymer and its preparation method.The nylon copolymer includes the chain segment derived from nylon monomer and the chain segment derived from copolymer initiator;The copolymer initiator has the functional group capable of in-situ polymerization with nylon monomer;The copolymer initiator can be dissolved in water, and the number average molecular weight is above 500.The high flow nylon copolymer in the present application can have higher tensile strength under the same relative viscosity, the high flow nylon has lower relative viscosity under the same tensile strength, has higher elongation at break under the same relative viscosity and / or the same tensile strength, has better flowability, that is, the novel nylon in the present application still maintains certain mechanical properties when viscosity decreases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-flow nylon preparation, and more specifically to a high-flow nylon copolymer and its preparation method. Background Technology

[0002] Nylon is a linear polymer with amide groups on its main chain. It possesses excellent comprehensive properties, including mechanical properties, heat resistance, wear resistance, chemical resistance, and self-lubricating properties. It also has a low coefficient of friction, some flame retardancy, and self-extinguishing properties, exhibiting discontinuous combustion once ignited. Due to its superior properties, nylon has received widespread attention in industry, and its applications are expanding with technological advancements. However, nylon's high polarity and crystallinity lead to increased toughness. Furthermore, its high melt strength makes processing and modification difficult.

[0003] Nylon materials are widely used in the automotive, electronics, and other industries. With the increasing demand for lightweight vehicles, more and more metal materials are being replaced by nylon. At the same time, these industries are also placing higher demands on the performance of nylon products. Therefore, the development of high-strength, high-flow-rate nylon materials has become a hot topic in product development for the automotive and electronics markets.

[0004] High-flow nylon 6 resin refers to nylon 6 resin with advantages such as low melt flow index, easy molding with short molding time, low energy consumption and cost, and suitability for glass fiber reinforcement. High-flow nylon products have high fluidity, requiring lower injection molding pressure, thus reducing manufacturing costs and increasing production flexibility. Simultaneously, due to the low filling pressure, the internal stress of the product is low, reducing the product defect rate. Compared with other common PA6-30GF materials, it achieves product weight reduction. Compared with commonly used PP materials, it can be directly fixed with screws, has better heat resistance, and is suitable for use in high-temperature environments around heat sinks.

[0005] The key challenge in preparing high-flow nylon is reducing the viscosity of the nylon melt without negatively impacting material properties. To obtain high-flow nylon, small-molecule branching agents are typically added. However, the inventors of this invention have discovered that the poor dispersibility and reaction uniformity of these small-molecule branching agents in nylon polymerization significantly affect the performance of the high-flow nylon polymerized products, resulting in branched or star-shaped structures with poor mechanical properties.

[0006] Therefore, how to provide a new type of nylon that reduces the viscosity of nylon melt while maintaining the mechanical properties of nylon remains a key research focus and challenge in this field. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for in-situ preparation of high-flow nylon and a high-flow nylon copolymer. The high-flow nylon copolymer of this invention can have higher tensile strength at the same relative viscosity, and at the same tensile strength, the high-flow nylon has lower relative viscosity. At the same relative viscosity and / or the same tensile strength, it has higher elongation at break and better flowability. That is, the novel nylon of this invention maintains certain mechanical properties even when the viscosity decreases.

[0008] A first aspect of the present invention is to provide a nylon copolymer comprising segments derived from nylon monomers and segments derived from a copolymer initiator; said copolymer initiator having functional groups capable of in-situ polymerization with nylon monomers; said copolymer initiator being soluble in water and having a number average molecular weight of 500 or higher.

[0009] According to the present invention, the copolymer initiator is a random copolymer, an alternating copolymer, or a block copolymer, preferably a random copolymer.

[0010] In a preferred embodiment of the present invention, the copolymer initiator has a functional group capable of reacting with the amino or carboxyl groups in the nylon monomer, preferably having at least one functional group selected from amino, hydroxyl, epoxy, and carboxyl groups.

[0011] In a preferred embodiment of the present invention, the copolymer initiator comprises structural units derived from comonomer B and optionally structural units derived from comonomer A; preferably, the initiator of the present invention is obtained by copolymerizing monomers A and B.

[0012] To ensure that the polymerization process of nylon VK tubes can be met, the copolymer must be soluble in water.

[0013] To ensure the copolymer dissolves in water, monomer A is preferably a water-soluble monomer or a monomer with a certain solubility in water, and a monomer that maintains structural stability under the conditions of in-situ polymerization of nylon. Preferably, the comonomer A is a water-soluble monomer and / or a monomer with a solubility in water of not less than 300 mg / L at 25°C, and a monomer that maintains structural unit stability under the conditions of in-situ polymerization of nylon. Structural stability here can be manifested as the absence of hydrolysis or other reactions that affect the structure. This includes, but is not limited to, one or more monomers such as (meth)acrylates, sodium p-vinylbenzenesulfonic acid, acrylamide monomers, vinyl acetate monomers, and vinyl ether monomers, preferably one or more of vinylpyrrolidone, N-vinylcaprolactam, vinyl morpholine ester, vinyl methyl ether, and vinyl ethyl ether.

[0014] In a preferred embodiment of the present invention, comonomer A is one or more of acrylate monomers (including but not limited to acrylates, methacrylates, glycidyl methacrylate, hydroxyethyl acrylate), p-vinylbenzenesulfonic acid monomers (including but not limited to p-vinylbenzenesulfonic acid, sodium p-vinylbenzenesulfonate, styrene monomers, acrylamide monomers, vinyl acetate monomers, vinyl ether monomers, preferably one or more of butyl acrylate, butyl methacrylate, vinylpyrrolidone, N-vinylcaprolactam, vinyl morpholine ester, vinyl methyl ether, vinyl ethyl ether, glycidyl methacrylate).

[0015] The preferred active monomer B is a monomer that possesses the ability to react with the terminal amino or carboxyl groups of nylon, such as monomers containing amino, hydroxyl, epoxy, or carboxyl groups, and which, under in-situ polymerization conditions of nylon, maintains the structural stability of the unit cells derived from comonomer B. This structural stability can be characterized by the absence of reactions that affect the structure, such as hydrolysis. Preferably, the comonomer B is a monomer containing at least one of the following functional groups: epoxy group, acid anhydride group, carboxylic acid group, oxazoline group, amino, and hydroxyl groups, and the monomer maintains the structural stability of the unit cells derived from comonomer B under in-situ polymerization conditions of nylon.

[0016] In a more preferred embodiment of the present invention, the comonomer B is selected from one or more of p-vinylbenzoic acid, p-aminostyrene, hydroxyethyl vinyl ether, glycidyl methacrylate, and hydroxyethyl acrylate.

[0017] In a more preferred embodiment of the present invention, comonomer B is selected from acrylate monomers, and comonomer A is selected from acrylate monomers and vinyl ether monomers. More preferably, comonomer B is selected from at least one of glycidyl methacrylate and hydroxyethyl acrylate, and comonomer A is selected from at least one of butyl acrylate, butyl methacrylate, and vinylpyrrolidone; even more preferably, the comonomers are in the following combinations: comonomer B is glycidyl methacrylate, and comonomer A is butyl acrylate; comonomer B is glycidyl methacrylate, and comonomer A is butyl methacrylate; comonomer B is hydroxyethyl acrylate, and comonomer A is vinylpyrrolidone.

[0018] In a preferred embodiment of the present invention, the total amount of all structural units in the copolymer initiator is 100% in molar quantity. The content of structural units derived from comonomer A in the copolymer initiator is 0-99%, preferably 10%-80%, more preferably 30%-70%, such as 30%, 40%, 50%, 60%, 70%, and any two values ​​or any range of any two values; the content of structural units derived from comonomer B is 1%-100%, preferably 20%-90%, more preferably 30%-70%, such as 30%, 40%, 50%, 60%, 70%, and any two values ​​or any range of any two values.

[0019] In a preferred embodiment of the present invention, the number average molecular weight of the copolymer initiator is 500-50000, preferably 700-20000, more preferably 1000-5000, such as 1000, 2000, 3000, 4000, 5000, and any two values ​​or any range of any two values.

[0020] The copolymer initiator can be prepared by living polymerization, which includes anionic polymerization, cationic polymerization, and living radical polymerization, preferably living radical polymerization. Living polymerization offers advantages such as controllable structure and molecular weight.

[0021] In the preparation method of the copolymer initiator of the present invention, the free radical living polymerization reaction can specifically adopt ATRP (atom transfer radical polymerization) or RAFT (reversible addition-fragmentation chain transfer radical polymerization) polymerization methods. Besides selecting a free radical initiator, other reaction aids can be selected for the living free radical polymerization reaction depending on the specific implementation method.

[0022] In the preparation method of the copolymer initiator of the present invention, the living radical polymerization reaction is preferably carried out by the ATRP polymerization method. ATRP (Atom Transfer Radical Polymerization) uses simple organic halides as initiators, transition metal salts and ligands as halogen atom supports. Through redox reactions, a reversible dynamic equilibrium is established between active and dormant species, thereby achieving control over the polymerization reaction. It is considered one of the most reliable polymer synthesis methods.

[0023] This invention does not limit the ATRP initiator, metal salt, and ligand used, as long as they can regulate styrene-based polymers or acrylamide-based polymers.

[0024] Preferably, the ARRP initiator is selected from at least one of α-bromophenylacetate, bromoethylbenzene, dodecyl 2-bromoisobutyrate, 2-hydroxyethyl 2-bromoisobutyrate, bromoacetonitrile, bromophenylacetate, benzyl bromide, and pentaerythritol tetra(2-bromoisobutyrate). The metal can be a chloride, bromide, cyanide, or porphyrin complex of copper, iron, cobalt, etc. The ARRP ligand is selected from at least one of tris[2-(dimethylamino)ethyl]amine, bipyridine, NN N'N'N"-pentamethyldiethylenetriamine, 4,4′-dinonyl-2,2′-bipyridine, and tris(2-pyridylmethyl)amine.

[0025] The present invention does not impose any particular limitation on the amount of ATRP initiator used, as long as it enables the living radical polymerization reaction to proceed smoothly. Preferably, the molar ratio of the ARRP reagent to the total amount of monomer components can be 1:(2-2000), more preferably 1:(10-100).

[0026] This invention does not impose any particular limitations on the conditions of the living radical polymerization reaction, as long as the synthesis of this invention can be successfully achieved. Preferably, the reaction conditions include: a temperature of (-20)-150℃, more preferably 40-90℃; and a time of 0.5-18 hours, more preferably 3-12 hours.

[0027] The copolymer initiator used in this invention can be prepared by methods known in the prior art, including but not limited to the preparation methods described above, and more specifically, including but not limited to the preparation methods in Preparation Examples 1-3 of this invention.

[0028] According to the present invention, the nylon monomer is a conventional nylon monomer in the art. In a preferred embodiment of the present invention, the nylon monomer is at least one of a polyamide monomer having the following structure:

[0029] NH3-R7-NH3 Equation (2-1);

[0030] R'OOC-R8-COOR” Equation (2-2);

[0031] R”'OOC-R9-NH3 Equation (2-3);

[0032]

[0033] NH3-R7'-NH4 + --OOC-R8'-COOH formula (2-5);

[0034] In equations (2-1) to (2-5), R7, R8, R7', R8', R9, and R10 are each independently C1-C. 20One of aromatic hydrocarbons, straight-chain hydrocarbons, or branched-chain alkanes;

[0035] In formula (2-2), R' and R” are each independently selected from one of hydrogen atom, phenyl, and C1-C4 alkyl group; preferably one of H and butyl.

[0036] In formula (2-3), R”' is selected from one of hydrogen atom, phenyl, and C1-C4 alkyl; preferably one of H and butyl.

[0037] In a preferred embodiment of the present invention, R7 and / or R7' are each C3-C 12 Aromatic hydrocarbons, straight-chain hydrocarbons, or branched-chain alkanes, preferably C4-C64. 10 Aromatic hydrocarbons, straight-chain hydrocarbon groups, or branched-chain alkanes, more preferably -(CH2)4-, -(CH2)6-, or -(CH2) 10 -

[0038] In a preferred embodiment of the present invention, R8 and / or R8' are each C1-C 10 The aromatic hydrocarbon, straight-chain hydrocarbon group or branched hydrocarbon group, preferably a C2-C8 straight-chain hydrocarbon group, more preferably -(CH2)2-, -(CH2)4-, -(CH2)8-.

[0039] In a preferred embodiment of the present invention, R9 and / or R10 are each C3-C. 12 Straight-chain hydrocarbon groups, preferably C3-C 10 The straight-chain hydrocarbon group is more preferably -(CH2)3- or -(CH2)8-.

[0040] In a preferred embodiment of the present invention, when the nylon monomer contains monomers of formula (2-1) and formula (2-2), the molar ratio between the two monomers of formula (2-1) and formula (2-2) is 1:(0.9-1.1).

[0041] In a preferred embodiment of the present invention, the nylon monomer contains at least one of the monomers of formula (2-3), formula (2-4) and formula (2-5); preferably at least one of caprolactam, aminocaproic acid and hexamethylene diammonium adipic acid.

[0042] In a preferred embodiment of the present invention, the chain segment derived from the nylon monomer has at least one of the following three structural units:

[0043] Where x, y, and z represent the molar content of the three structural units, and R1-R4 are each C1-C 18 Straight-chain hydrocarbon groups, C1-C 18 Branched hydroxyl groups, C6-C 18It is one of the aromatic hydrocarbon groups, and R3 and R4 do not have the same structure at the same time; x+y+z=1, and x, y, and z are all greater than or equal to 0; preferably, R1 is -(CH2)4-, -(CH2)6-, or -(CH2). 10 -; and / or, R2 is -(CH2)2-, -(CH2)4-, or -(CH2)8-; and / or, R3 and R4 are each -(CH2)5- or -(CH2) 10 -

[0044] According to the above technical solution, preferably, the chain segment derived from the nylon monomer has the following structure:

[0045] That is, the chain segments derived from nylon monomers are composed of three structural units corresponding to x, y, and z. There are no special requirements on the connection order of the structural units corresponding to x, y, and z. The nylon copolymer in this invention is a random copolymer.

[0046] The copolymer initiator can be used as a polymerization aid, added together with the nylon monomer to prepare a high-flow nylon material, or it can be used as a processing aid to prepare a high-flow nylon material during processing; preferably, it is added together with the nylon monomer during polymerization to obtain the nylon copolymer through in-situ polymerization.

[0047] The amount of copolymer initiator added during in-situ polymerization should take into full account the molar ratio of the amount of active monomer B to the amount of nylon monomer. In a preferred embodiment of the present invention, in the nylon copolymer, the molar ratio of the functional groups in the chain segment derived from the copolymer initiator that can undergo in-situ polymerization with the nylon monomer to the structural units derived from the nylon monomer is (1-10):100, preferably (2-10):100, more preferably (2-8):100, and even more preferably (2.5-4):100.

[0048] In a preferred embodiment of the present invention, the relative viscosity of the nylon copolymer is 1.5-2.2, preferably 1.6-2, for example 1.6, 1.7, 1.8, 1.9, 2, and any two values ​​or any range of any two values.

[0049] A second aspect of the present invention is to provide a method for preparing a nylon copolymer according to the first aspect, comprising polymerizing raw materials, including the copolymer initiator and the nylon monomer, to obtain the nylon copolymer.

[0050] This invention prepares a nylon copolymer by copolymerizing a reactive copolymer (i.e., the copolymer initiator described above) with a nylon monomer. This nylon copolymer exhibits superior toughness, thus demonstrating better overall performance than conventional nylon 6, nylon 66, and other nylon copolymers.

[0051] In a preferred embodiment of the present invention, the molar ratio of the functional groups in the copolymer initiator capable of in-situ polymerization with the nylon monomer to the nylon monomer is (1-10):100, preferably (2-8):100.

[0052] In a preferred embodiment of the present invention, the number average molecular weight of the copolymer initiator is 500-50000, preferably 700-20000, and more preferably 1000-5000.

[0053] In a preferred embodiment of the present invention, based on a molar amount, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 0-99%, preferably 10%-80%, more preferably 30%-70%; and the content of structural units derived from comonomer B is 1%-100%, preferably 20%-90%, more preferably 30%-70%.

[0054] According to the present invention, the preferred amount of the copolymer initiator can be metered by the molar ratio of the functional groups in the copolymer initiator capable of in-situ polymerization with the nylon monomer to the nylon monomer, or by the proportion of the copolymer initiator in the raw materials of the polymerization reaction. In a preferred embodiment of the present invention, based on 100% of the total weight of the raw materials of the polymerization reaction, the amount of the copolymer initiator is 1.5%-15%, preferably 2%-12%, and most preferably 3-10%.

[0055] The raw materials for the polymerization reaction include a copolymer initiator, nylon monomer, and optionally added water.

[0056] Taking the preparation of nylon 6 as an example, the raw materials for the polymerization reaction include a copolymer initiator, nylon monomer, and water. Preferably, based on the total weight of the raw materials for the polymerization reaction as 100%, the amount of the copolymer initiator is 1.5%-15%, more preferably 2%-12%, and most preferably 3-10%; the amount of the nylon 6 monomer is 80%-92%, and the amount of water is 5%-10%.

[0057] The polymerization of the nylon copolymer described in this invention can be at least one of condensation polymerization, ring-opening polymerization, anionic polymerization, and cationic polymerization, and can be carried out using existing nylon copolymer preparation conditions.

[0058] In a preferred embodiment of the present invention, the conditions for the polymerization reaction include:

[0059] The polymerization reaction is carried out under a protective atmosphere, which includes, but is not limited to, an inert atmosphere (nitrogen and / or inert gas).

[0060] In a preferred embodiment of the present invention, the polymerization reaction temperature is 140-280°C, preferably 220-260°C.

[0061] In a preferred embodiment of the present invention, the reaction time is 0.5-24 hours.

[0062] In a preferred embodiment of the present invention, the reaction pressure is 0-20 atmospheres.

[0063] More specifically, the polymerization method of the present invention is illustrated using nylon 6 as an example:

[0064] The copolymer initiator, nylon 6 monomer caprolactam, and water were added to the reactor, and an inert gas was introduced into it for deoxygenation treatment.

[0065] Heat the mixture to 180-260℃ to carry out the polymerization reaction. Finally, control the reaction temperature between 240 and 260℃ and stir the reaction. The preferred stirring time is 0-3 hours.

[0066] During the reaction, the pressure can be maintained at 0-20 atmospheres. The high vacuum is maintained for 0-6 hours, and the pressure is slowly reduced to maintain the reaction temperature at 180-260℃. The low vacuum reaction time is preferably 0-2 hours. After that, the high vacuum is evacuated and the vacuum degree is further reduced to below 2000Pa. The reaction can then proceed for 0.5-2 hours.

[0067] Preferably, the inert gas is nitrogen, and the deoxygenation treatment time is 30 minutes.

[0068] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0069] This invention provides a method for preparing high-flow nylon. The invention involves copolymerizing a copolymer initiator (which has functional groups capable of in-situ polymerization with nylon monomers; the copolymer initiator is soluble in water and has a number average molecular weight of 500 or higher) with nylon monomers in a one-step reaction to obtain a high-flow nylon copolymer.

[0070] The novel nylon of this invention exhibits a relative viscosity reduction to below 2.2, even as low as 1.6, representing a significant decrease in viscosity. Despite this reduction, the tensile strength of the novel nylon remains above 49.5 MPa, and both its flexural strength and elongation at break are above 25%. Compared to conventional nylon copolymers in the prior art, the high-flow nylon of this invention exhibits higher tensile strength at the same relative viscosity, and at the same tensile strength, it has a lower relative viscosity. Furthermore, at the same relative viscosity and / or the same tensile strength, it has a higher elongation at break and better flowability. Therefore, the novel nylon of this invention maintains certain mechanical properties even with a decrease in viscosity, achieving unexpected technical benefits.

[0071] In summary, the nylon copolymer of the present invention has both high fluidity and excellent mechanical properties, and has superior overall performance compared with conventional nylon 6, nylon 66 and nylon copolymers, making it more adaptable to a wide range of market demands.

[0072] Moreover, the preparation method of this invention is simple and has extremely high value for widespread application. Detailed Implementation

[0073] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the invention. The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values; these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0074] Tensile strength was measured according to ASTM D638 method at a tensile speed of 50 mm / min; elongation at break is the ratio of displacement at break to original length, expressed as a percentage.

[0075] Monomer composition: The microstructure of the polymer was determined using an AVANCE DRX 400MHz nuclear magnetic resonance spectrometer from Bruker, Switzerland. The determination was performed at room temperature using 1H NMR spectroscopy, with deuterated chloroform as the solvent and a sample concentration of 10 mg / mL.

[0076] Relative viscosity test of nylon copolymer: The molecular weight of the polyamide copolymer of this invention is characterized by a relative viscosity test. Weigh 0.25g of polymer sample and place it in a 25ml volumetric flask. Add concentrated sulfuric acid (until the mark is reached). After the sample is completely dissolved, add concentrated sulfuric acid to the mark in the volumetric flask and then shake well for measurement. Measure 10ml of the prepared solution into an Ubbelohde viscometer (4-1.0-1.1). Install the viscometer vertically in a constant temperature water bath at 25±0.5℃ for 20min. The time it takes for the solution to flow through both marks on the viscometer is the flow time. Measure each sample three times (with an error not exceeding ±0.2s) and take the average value.

[0077] The number-average molecular weight and molecular weight distribution PDI were determined by gel permeation chromatography.

[0078] Preparation Example 1

[0079] In this embodiment, the polymerization reaction used is ATRP polymerization. 2-Bromoisobutyryl bromide, PMEDTA (pentamethyldiethylenetriamine), and CuCl were added to a polymerization flask, dissolved in 50 ml of dioxane. Glycidyl methacrylate and butyl acrylate monomers were then added, and the mixture was purged with nitrogen for 30 minutes. The reactant feed ratio was: bromoisobutyryl bromide / PMEDTA / CuCl / glycidyl methacrylate / butyl acrylate molar ratio was 1 / 0.02 / 0.01 / 30 / 50. The reaction was carried out in an oil bath at 80°C. The polymer product was precipitated in diethyl ether; the product was A1, with a number-average molecular weight of 4500, PDI = 1.3, and the content ratio of structural units derived from glycidyl methacrylate / butyl acrylate in the polymer was 3:5.

[0080] Preparation Example 2

[0081] The implementation method is the same as above, except that the molar ratio of 2-bromoisobutyryl bromide / PMEDTA / CuCl / glycidyl methacrylate / butyl methacrylate (i.e., butyl methacrylate is used instead of butyl acrylate in Preparation Example 1) is 1 / 0.02 / 0.01 / 20 / 80. The product is A2, with a determined number-average molecular weight of 28300, PDI = 1.1, and the content ratio of structural units derived from glycidyl methacrylate / methacrylic acid in the polymer is 2:8.

[0082] Preparation Example 3

[0083] The implementation method is the same as above, except that hydroxyethyl acrylate and vinylpyrrolidone are used instead of glycidyl methacrylate and butyl methacrylate in Example 1. The reactant feed ratio in the first step is: bromoxyisobutyryl bromide / PMEDTA / CuCl / hydroxyethyl acrylate / vinylpyrrolidone molar ratio is 1 / 0.02 / 0.02 / 70 / 30. The product is A3, with a determined number-average molecular weight of 6800, PDI = 1.3, and the content ratio of structural units derived from hydroxyethyl acrylate / vinylpyrrolidone in the polymer is 7:3.

[0084] Example 1

[0085] A nylon copolymer is formed by polycondensation of the following components in parts by weight:

[0086] Copolymer A1 (i.e., the copolymer obtained in Preparation Example 1) with a mass content of 3%;

[0087] The monomer caprolactam has a mass content of 92%.

[0088] Deionized water with a mass content of 5%;

[0089] The method for preparing the nylon copolymer is as follows:

[0090] 200g of copolymer A1, monomer caprolactam, and water (in parts by weight) were added to a polymerization reactor. The molar ratio of glycidyl methacrylate to caprolactam in copolymer A1 was 0.013:1. The reactor was heated to 240-260°C for polymerization, and the pressure was controlled to be less than 0.5MPa. After 2 hours of reaction, the pressure was gradually reduced to atmospheric pressure to remove the byproduct water. The pressure was further reduced to 2000Pa and maintained for 2 hours to further polycondense and increase the molecular weight. The reaction was then completed. Finally, the product was cooled and pelletized to obtain the nylon copolymer product B1.

[0091] Comparative Example 1

[0092] Polyamide polymerization was carried out without adding copolymer A1. The above-mentioned monomer caprolactam with a mass content of 83% and aminocaproic acid with a mass content of 17% were used to prepare polyamide copolymer product C1 using the same equipment, under the same conditions and process as in Example 1.

[0093] Comparative Example 2

[0094] Polyamide polymerization was carried out without adding copolymer A1. 83% by mass of the above monomer caprolactam and 16% by mass of aminocaproic acid were taken, and 1% adipic acid was added. Polyamide copolymer product C2 was prepared using the same equipment, under the same conditions, and with the same process as in Example 1.

[0095] Comparative Example 3

[0096] Polyamide polymerization was carried out without adding copolymer A1. 83% by mass of the above monomer caprolactam and 15.5% by mass of aminocaproic acid were taken, and 1.5% adipic acid was added. Polyamide copolymer product C3 was prepared using the same equipment, under the same conditions, and with the same process as in Example 1.

[0097] Example 2

[0098] A nylon copolymer is formed by polycondensation of the following components in parts by weight:

[0099] Copolymer A1 with a mass content of 5%;

[0100] The monomer caprolactam has a mass content of 90%.

[0101] Water with a mass content of 5%;

[0102] In copolymer A1, the molar ratio of glycidyl methacrylate to caprolactam monomer was 0.022:1; the polymerization conditions were the same as in Example 1, and nylon copolymer B2 was obtained.

[0103] Example 3

[0104] A nylon copolymer is formed by polycondensation of the following components in parts by weight:

[0105] Copolymer A1 with a mass content of 10%;

[0106] The monomer caprolactam has a mass content of 80%.

[0107] Water with a mass content of 10%;

[0108] In copolymer A1, the molar ratio of glycidyl methacrylate to caprolactam monomer was 0.049:1; the polymerization conditions were the same as in Example 1, and nylon copolymer B3 was obtained.

[0109] Example 4

[0110] A nylon copolymer is formed by polycondensation of the following components in parts by weight:

[0111] Copolymer A1 with a mass content of 15%;

[0112] The monomer caprolactam has a mass content of 80%.

[0113] Water with a mass content of 5%;

[0114] The molar ratio of glycidyl methacrylate to caprolactam monomer in copolymer A1 is 0.075:100;

[0115] The polymerization conditions were the same as in Example 1, and the resulting nylon copolymer was B4.

[0116] Example 5

[0117] Similar to Example 3, copolymer A1 was replaced with copolymer A2 to obtain copolymer B5.

[0118] Example 6

[0119] Similar to Example 3, copolymer A1 was replaced with copolymer A3 to obtain copolymer B6.

[0120] Example 7

[0121] A nylon copolymer is formed by polycondensation of the following components in parts by weight:

[0122] Copolymer A1 with a mass content of 5%;

[0123] The monomer caprolactam has a mass content of 60%.

[0124] Lauryl lactam with a mass content of 30%;

[0125] Deionized water with a mass content of 5%;

[0126] The method for preparing the nylon copolymer is as follows:

[0127] 200g of copolymer A1, monomer caprolactam, laurolactam, and water (in parts by weight) were added to a polymerization reactor. The molar ratio of glycidyl methacrylate to caprolactam in copolymer A1 was 0.013:1. The reactor was heated to 240-260°C for polymerization, with the pressure controlled to be less than 0.5MPa. After 2 hours of reaction, the pressure was gradually reduced to atmospheric pressure to remove the byproduct water. The pressure was further reduced to 2000Pa and maintained for 2 hours to further increase the molecular weight through polycondensation. The reaction was then completed, and the product was cooled and pelletized to obtain the nylon copolymer product B7.

[0128] Example 8

[0129] A nylon copolymer is formed by polycondensation of the following components in parts by weight:

[0130] Copolymer A1 with a mass content of 10%;

[0131] The monomer caprolactam has a mass content of 60%.

[0132] Nylon 66 salt with a mass content of 23%;

[0133] Deionized water with a mass content of 7%;

[0134] The method for preparing the nylon copolymer is as follows:

[0135] 200g of copolymer A1, monomer caprolactam, nylon 66 salt, and water (in parts by weight) were added to a polymerization reactor. The molar ratio of glycidyl methacrylate to caprolactam in copolymer A1 was 0.013:1. The reactor was heated to 240-260°C for polymerization, with the pressure controlled below 0.5 MPa. After 2 hours of reaction, the pressure was gradually reduced to atmospheric pressure to remove the byproduct water. The pressure was further reduced to 2000 Pa and maintained for 2 hours to further increase the molecular weight through polycondensation. The reaction was then terminated, and the product was cooled and pelletized to obtain the nylon copolymer product B8.

[0136] Table 1

[0137]

[0138] Generally, linear nylon has a relative viscosity of over 2.2 and a tensile strength of over 60 MPa, indicating high viscosity. When the relative viscosity decreases to 2.0 or below, the tensile strength and elongation at break of nylon generally decrease significantly, with the tensile strength even dropping below 30 MPa and the elongation at break dropping below 20%, or even below 15%.

[0139] The data in the comparison table show that, compared with conventional nylon copolymers, the relative viscosity of the novel nylon in this invention is reduced to below 2.2, and even to 1.6, showing a significant decrease in viscosity. Under these conditions, the tensile strength of the novel nylon in this invention is still above 49.5 MPa, and the flexural strength and elongation at break are both above 25%. At the same relative viscosity, the high-flow nylon in this invention has a higher tensile strength. At the same tensile strength, the high-flow nylon has a lower relative viscosity and better flowability. It can be seen that the mechanical properties of the novel nylon in this invention are still maintained to a certain extent when the viscosity decreases, achieving unexpected technical effects.

[0140] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

[0141] All publications, patent applications, patents, and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings commonly understood by those skilled in the art. In case of conflict, the definitions in this specification shall prevail.

[0142] When this specification uses the prefixes “known to those skilled in the art,” “prior art,” or similar terms to derive materials, substances, methods, steps, apparatus, or components, the objects derived from such prefixes cover those commonly used in the art at the time of this application, but also include those that are not currently commonly used but will become generally recognized in the art as suitable for similar purposes.

[0143] The endpoints and any values ​​of the ranges disclosed in this application are not limited to the precise ranges or values; such ranges or values ​​should be understood to include values ​​close to them. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. In principle, various technical solutions can be combined with each other to obtain new technical solutions, which should also be considered as specifically disclosed herein.

[0144] In the context of this specification, except where expressly stated otherwise, any matters or issues not mentioned shall apply directly to those known in the art without any modification.

[0145] Furthermore, any implementation described herein can be freely combined with one or more other implementations described herein, and the resulting technical solutions or technical ideas shall be regarded as part of the original disclosure or original record of the present invention, and should not be regarded as new content not disclosed or anticipated herein, unless those skilled in the art consider the combination to be obviously unreasonable.

Claims

1. A nylon copolymer comprising segments derived from a nylon monomer and segments derived from a copolymer initiator; said nylon copolymer is obtained by polymerization of a copolymer initiator, a nylon monomer, and optionally water; The copolymer initiator has functional groups that enable in-situ polymerization with nylon monomers; the copolymer initiator is soluble in water and has a number average molecular weight of over 500; The copolymer initiator was prepared by a living polymerization method; The copolymer initiator comprises structural units derived from comonomer B and structural units derived from comonomer A; comonomer A is a water-soluble monomer and / or a monomer with a solubility in water of not less than 300 mg / L at 25°C and which maintains structural unit stability under the conditions of in-situ polymerization of nylon; and comonomer A is one or more of acrylate monomers and vinylpyrrolidone. The comonomer B is a monomer containing at least one of the following functional groups: The monomer contains at least one group selected from epoxy group, acid anhydride group, carboxylic acid group, oxazoline group, amino group, and hydroxyl group, and the monomer can maintain the structural stability of the structural unit derived from comonomer B under the in-situ polymerization conditions of nylon; the comonomer B is selected from one or more of p-vinylbenzoic acid, p-aminostyrene, hydroxyethyl vinyl ether, glycidyl methacrylate, and hydroxyethyl acrylate. In the nylon copolymer, the molar ratio of the functional groups in the chain segment derived from the copolymer initiator that can undergo in-situ polymerization with the nylon monomer to the structural units derived from the nylon monomer is (1-10):

100.

2. The nylon copolymer according to claim 1, characterized in that: The copolymer initiator is a random copolymer, alternating copolymer, or block copolymer; and / or, The copolymer initiator has functional groups that can react with amino or carboxyl groups in the nylon monomer.

3. The nylon copolymer according to claim 1, characterized in that: In molar terms, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 0-99%, and not 0; the content of structural units derived from comonomer B is 1%-100%.

4. The nylon copolymer according to claim 1, characterized in that: In molar amounts, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 10%-80%; and the content of structural units derived from comonomer B is 20%-90%.

5. The nylon copolymer according to claim 1, characterized in that: In molar amounts, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 30%-70%; and the content of structural units derived from comonomer B is 30%-70%.

6. The nylon copolymer according to claim 1, characterized in that: Comonomer A is one or more of butyl acrylate, butyl methacrylate, vinylpyrrolidone, and glycidyl methacrylate.

7. The nylon copolymer according to claim 1, characterized in that: The number average molecular weight of the copolymer initiator is between 500 and 50,000.

8. The nylon copolymer according to claim 1, characterized in that: The number average molecular weight of the copolymer initiator is 700-20000.

9. The nylon copolymer according to claim 1, characterized in that: The number average molecular weight of the copolymer initiator is 1000-5000.

10. The nylon copolymer according to claim 1, characterized in that: The nylon monomer contains monomers of formulas (2-1) and (2-2), and / or, The nylon monomer contains at least one monomer of formula (2-3) and formula (2-4): NH2-R7-NH2 formula (2-1); R'OOC-R8-COOR'' formula (2-2); R'''OOC-R9-NH2 formula (2-3); Equation (2-4); In equations (2-1) to (2-4), R7, R8, R9, and R10 are each independently C1-C. 20 One of the straight-chain hydrocarbon group or the branched-chain alkane group; In formula (2-2), R' and R'' are each independently selected from one of hydrogen atoms, phenyl groups, and C1-C4 alkyl groups; In formula (2-3), R''' is selected from one of hydrogen atoms, phenyl, and C1-C4 alkyl groups.

11. The nylon copolymer according to claim 10, characterized in that: In equation (2-2), R' and R'' are each independently one of H and butyl; In equation (2-3), R''' is either H or butyl.

12. The nylon copolymer according to claim 10, characterized in that: R7 is C3-C 12 Straight-chain hydrocarbon groups or branched alkane groups; and / or, R8 is C1-C 10 Straight-chain hydrocarbon groups or branched hydrocarbon groups; and / or, R9 and R10 are each C3-C 12 Straight-chain hydrocarbon groups.

13. The nylon copolymer according to claim 10, characterized in that: R7 is C4-C 10 Straight-chain hydrocarbon groups or branched alkane groups.

14. The nylon copolymer according to claim 10, characterized in that: The R8 is a C2-C8 straight-chain hydrocarbon group.

15. The nylon copolymer according to claim 10, characterized in that: R9 and R10 are each C3-C 10 Straight-chain hydrocarbon groups.

16. The nylon copolymer according to claim 10, characterized in that: The R7 is -(CH2)4-, -(CH2)6-, -(CH2) 10 -; and / or, The R8 is -(CH2)2-, -(CH2)4-, -(CH2)8-; and / or, R9 and R10 are -(CH2)3- and -(CH2)8-, respectively.

17. The nylon copolymer according to claim 10, characterized in that: When the nylon monomer contains monomers of formula (2-1) and formula (2-2), the molar ratio between the two monomers of formula (2-1) and formula (2-2) is 1:(0.9-1.1).

18. The nylon copolymer according to claim 10, characterized in that: The nylon monomer is at least one of caprolactam and aminocaproic acid.

19. The nylon copolymer according to claim 1, characterized in that: The chain segments derived from nylon monomers have at least one of the following three structural units: Where x, y, and z represent the molar content of the three structural units, and R1-R4 are each C1-C 18 Straight-chain hydrocarbon groups, C1-C 18 Branched hydroxyl groups, C6-C 18 One of the aromatic hydrocarbon groups, and R3 and R4 do not have the same structure at the same time; x+y+z=1, x, y, and z are all greater than or equal to 0.

20. The nylon copolymer according to claim 19, characterized in that: R1 is -(CH2)4-, -(CH2)6-, or -(CH2). 10 -; and / or, R2 is -(CH2)2-, -(CH2)4-, or -(CH2)8-; and / or, R3 and R4 are each -(CH2)5- or -(CH2). 10 - 21. The nylon copolymer according to any one of claims 1-20, characterized in that: In the nylon copolymer, the molar ratio of functional groups in the segments derived from the copolymer initiator capable of in-situ polymerization with nylon monomers to structural units derived from nylon monomers is (2-8):100; and / or, The relative viscosity of the nylon copolymer is 1.5-2.

2.

22. The nylon copolymer according to any one of claims 1-20, characterized in that: The relative viscosity of the nylon copolymer is 1.6-2.

23. A method for preparing a nylon copolymer according to any one of claims 1-22, comprising polymerizing raw materials, including the copolymer initiator and the nylon monomer, to obtain the nylon copolymer.

24. The preparation method according to claim 23, characterized in that: The molar ratio of the functional groups in the copolymer initiator capable of in-situ polymerization with nylon monomers to the nylon monomers is (2-8):

100.

25. The preparation method according to claim 23, characterized in that: The number average molecular weight of the copolymer initiator is between 500 and 50,000; and / or, In molar amounts, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 0-99%; and the content of structural units derived from comonomer B is 1%-100%.

26. The preparation method according to claim 23, characterized in that: The number-average molecular weight of the copolymer initiator is 700-20000; and / or, In molar amounts, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 10%-80%; and the content of structural units derived from comonomer B is 20%-90%.

27. The preparation method according to claim 23, characterized in that: The number average molecular weight of the copolymer initiator is 1000-5000; and / or, In molar amounts, with the total amount of all structural units in the copolymer initiator being 100%, the content of structural units derived from comonomer A in the copolymer initiator is 30%-70%; and the content of structural units derived from comonomer B is 30%-70%.

28. The preparation method according to any one of claims 23-27, characterized in that: The polymerization reaction is carried out under a protective atmosphere, and / or the temperature of the polymerization reaction is 140-280°C; and / or the reaction time is 0.5-24 hours; and / or the reaction pressure is 0-20 atmospheres.

29. The preparation method according to any one of claims 23-27, characterized in that: The polymerization reaction is carried out at a temperature of 220-260℃.

Citation Information

Patent Citations

  • Multichain polyamide resins

    US2524045A

  • Graft copolymer of polyamide onto a vinyl aromatic-unsaturated carboxylic acid copolymeric backbone

    US3325561A