Thermally conductive flame-retardant semi-aromatic polyamide compositions, process for their preparation and use

By combining modified spherical boron nitride with isocyanurate alkoxysilane, the problems of thermal conductivity and surface roughness of semi-aromatic polyamide materials are solved, achieving high thermal conductivity and a smooth surface, suitable for electronic products.

CN118813039BActive Publication Date: 2026-11-20KINGFA SCI & TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310422040.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2026-11-20
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Existing semi-aromatic polyamide materials suffer from poor interplanar thermal conductivity and high surface roughness, making it difficult to meet the high thermal conductivity and smooth surface requirements of electronic products.

Method used

Modified spherical boron nitride is used, and the surface of the spherical boron nitride is treated with isocyanurate alkoxysilane to improve its interfacial adhesion with semi-aromatic polyamide, improve thermal conductivity, and maintain the smooth surface of the material.

Benefits of technology

It achieves high interplane thermal conductivity, isotropic thermal conductivity, and low surface roughness, meeting the requirements of high thermal conductivity and smooth surface for electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004187223880000081
    Figure BDA0004187223880000081
  • Figure BDA0004187223880000091
    Figure BDA0004187223880000091
  • Figure BDA0004187223880000101
    Figure BDA0004187223880000101
Patent Text Reader

Abstract

The application relates to a heat-conducting flame-retardant semi-aromatic polyamide composition and a preparation method and application thereof. The heat-conducting flame-retardant semi-aromatic polyamide composition comprises the following components in parts by weight: semi-aromatic polyamide resin 30-65 parts, organic phosphinate flame retardant 5-22 parts, and modified spherical boron nitride 10-40 parts; the modified spherical boron nitride is spherical boron nitride with isocyanurate alkoxysilane on the surface. The heat-conducting flame-retardant semi-aromatic polyamide composition has good flame-retardant performance, surface roughness, high interplanar thermal conductivity and thermal conductivity isotropy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyamide thermally conductive materials, and more specifically, to a thermally conductive and flame-retardant semi-aromatic polyamide composition, its preparation method, and its application. Background Technology

[0002] In recent years, with the increasing density and miniaturization of electronic products, lead-free reflow surface mount technology (SMT) has become an important assembly method. Its application requires components to withstand high temperatures of 250-280°C. Traditional engineering plastics such as PA66 and PBT cannot meet this requirement, so high-temperature resistant engineering plastics have emerged. Semi-aromatic polyamide (PPA) has been widely used due to its many advantages such as high melting point, high heat distortion temperature, and high strength.

[0003] Furthermore, with the rapid development of microelectronics integration and assembly technologies, assembly density has increased dramatically, and the size of electronic components and logic circuits has shrunk by thousands of times. Electronic instruments are becoming increasingly thinner and smaller, while operating frequencies are increasing dramatically, and the semiconductor thermal environment is rapidly changing towards higher temperatures. At this point, the heat generated by electronic devices accumulates rapidly. To ensure that electronic components can still operate normally with high reliability and efficiency under ambient temperatures, timely heat dissipation becomes a crucial limiting factor affecting their lifespan.

[0004] In the flame retardant system of semi-aromatic polyamide materials, organic phosphonates are often used as halogen-free flame retardants, mainly because they have better temperature resistance and good flame retardant properties compared with other halogen-free flame retardants (such as red phosphorus, melamine polyphosphate, melamine cyanurate, etc.), and require a small amount to be added.

[0005] Thermal conductivity is a property of materials and can be measured using appropriate equipment and instruments, such as the protective plate method, heat flow meter method, and laser flash method. In the injection molding or extrusion molding process of thermoplastic thermally conductive composite materials, the thermally conductive filler is usually oriented along the flow direction, resulting in different thermal conductivity properties in the parallel and perpendicular flow directions.

[0006] Interplanar thermal conductivity refers to the thermal conductivity of a material in the direction perpendicular to the flow direction. Currently, the thermally conductive filler boron nitride used in thermal conductivity systems is mainly ordinary lamellar boron nitride. Because this lamellar structure orients along the melt flow direction during molding, the thermal conductivity of the part exhibits significant anisotropy, with higher thermal conductivity in the flow direction and lower thermal conductivity perpendicular to the flow direction. In actual product use, the heat generated internally must be dissipated to the external environment through the plastic shell, making the magnitude of the thermal conductivity in the vertical direction crucial.

[0007] The Chinese patent entitled "Glass Fiber Reinforced Flame Retardant Thermally Conductive Semi-Aromatic Copolymer Nylon Composite Material and Preparation Method Thereof" uses at least one of the following as fillers: micron- or nano-sized alumina, magnesium oxide, zinc oxide, aluminum nitride, halloysite, boron nitride, and silicon carbide. The composite material obtained by this technology still has the problem of low interplanar thermal conductivity.

[0008] In addition, the application scenarios of electronic products also require semi-aromatic polyamide materials to have low surface roughness. After the thermally conductive filler is directly added to semi-aromatic polyamide, the surface of the semi-aromatic polyamide material often becomes rough, which does not meet the requirements of the corresponding application scenarios.

[0009] Therefore, it is necessary to develop a semi-aromatic polyamide material with high interplanar thermal conductivity and low surface roughness. Summary of the Invention

[0010] The primary objective of this invention is to overcome the problems of poor interplanar thermal conductivity or high surface roughness in current semi-aromatic polyamide materials, or the addition of thermally conductive fillers, and to provide a thermally conductive and flame-retardant semi-aromatic polyamide composition. This composition exhibits excellent flame-retardant properties, low surface roughness, high interplanar thermal conductivity, and isotropic thermal conductivity.

[0011] A further object of the present invention is to provide a method for preparing the above-mentioned thermally conductive and flame-retardant semi-aromatic polyamide composition.

[0012] A further object of the present invention is to provide the application of the above-described thermally conductive and flame-retardant semi-aromatic polyamide composition in the preparation of electronic products.

[0013] The above-mentioned objective of this invention is achieved through the following technical solution:

[0014] A thermally conductive and flame-retardant semi-aromatic polyamide composition comprising the following components in parts by weight:

[0015] 30-65 parts of semi-aromatic polyamide resin,

[0016] 5-22 parts of organic phosphonate flame retardant

[0017] 10-40 parts of modified spherical boron nitride;

[0018] The modified spherical boron nitride is a spherical boron nitride with a surface modified isocyanurate alkoxysilane.

[0019] The inventors of this invention discovered through research that adding spherical boron nitride to semi-aromatic polyamide can improve the interplanar thermal conductivity of the material to a certain extent. However, the direct addition of spherical boron nitride inevitably causes interfacial adhesion problems between it and semi-aromatic polyamide. Due to the weak interfacial adhesion between the two phases, significant interfacial thermal resistance is generated, which limits the improvement of the interplanar thermal conductivity of the material.

[0020] Through further research, the inventors discovered that surface treatment of spherical boron nitride with isocyanurate alkoxysilane yields modified spherical boron nitride. Adding this modified spherical boron nitride to a semi-aromatic polyamide resin can produce a thermally conductive and flame-retardant semi-aromatic polyamide composition with high interplanar thermal conductivity and isotropic thermal conductivity. The reason is that isocyanurate alkoxysilane acts as a coupling agent, making the two-phase interface of spherical boron nitride and semi-aromatic polyamide tightly bonded. In addition, isocyanurate alkoxysilane also has high reactivity and high heat resistance. The high reactivity enables it to generate good chemical bonding force with the active functional groups of the matrix resin, while the high heat resistance allows isocyanurate alkoxysilane to maintain good thermal stability and chemical activity at high temperature (the melting point of semi-aromatic polyamide resin is high, and the melting temperature needs to reach about 330℃ during processing). This allows the modified spherical boron nitride and semi-aromatic polyamide to maintain a strong interfacial bonding effect and low interfacial thermal resistance, thereby enabling the thermally conductive and flame-retardant semi-aromatic polyamide composition to obtain a high interplanar thermal conductivity. Meanwhile, due to the good interfacial wetting effect and strong interfacial bonding between the modified spherical boron nitride and the semi-aromatic polyamide under high temperature environment, the problem of increased surface roughness of polyamide materials caused by individual thermally conductive fillers is effectively avoided, thus allowing the thermally conductive and flame-retardant semi-aromatic polyamide composition to maintain low surface roughness (high surface gloss).

[0021] Furthermore, the thermally conductive and flame-retardant semi-aromatic polyamide composition of the present invention also maintains good flame-retardant properties, meeting the requirements for use.

[0022] The thermally conductive and flame-retardant semi-aromatic polyamide composition of the present invention has good flame-retardant properties, low surface roughness (high surface gloss), high interplanar thermal conductivity and thermal isotropic properties.

[0023] Preferably, the thermally conductive and flame-retardant semi-aromatic polyamide composition comprises the following components in parts by weight:

[0024] 35-55 parts of semi-aromatic polyamide resin,

[0025] 14-18 parts of organic phosphonate flame retardant,

[0026] 15-25 parts of modified spherical boron nitride.

[0027] Preferably, the average particle size of the spherical boron nitride is 15–130 μm.

[0028] More preferably, the average particle size of the spherical boron nitride is 15–75 μm.

[0029] Within the average particle size range, the obtained thermally conductive and flame-retardant semi-aromatic polyamide composition exhibits higher thermal conductivity in both the in-plane and through-plane directions.

[0030] Optionally, the isocyanurate alkoxysilane is at least one of isocyanurate trimekoxysilane or isocyanurate dialekoxysilane.

[0031] Preferably, the isocyanurate alkoxysilane is isocyanurate trialkoxysilane.

[0032] Compared to isocyanurate dialkoxysilanes (e.g., 1,3,5-tris(methyldimethoxysilylpropyl)isocyanurate), modifying with isocyanurate trimekoxysilanes (e.g., 1,3,5-tris(trimethoxysilylpropyl)isocyanurate, 1,3,5-tris(triethoxysilylpropyl)isocyanurate) results in a thermally conductive and flame-retardant semi-aromatic polyamide composition with higher thermal conductivity in both the inplane and throughplane directions.

[0033] More preferably, the isocyanurate trialkoxysilane isocyanurate trimethoxysilane.

[0034] Compared to isocyanurate triethoxysilane (e.g., 1,3,5-tris(triethoxysilylpropyl)isocyanurate), the thermally conductive and flame-retardant semi-aromatic polyamide composition obtained by modification with isocyanurate trimethoxysilane (e.g., 1,3,5-tris(trimethoxysilylpropyl)isocyanurate) has a higher thermal conductivity in both the in-plane and through-plane directions.

[0035] In this invention, the mass ratio of isocyanurate alkoxysilane to spherical boron nitride in the modified spherical boron nitride is (0.2-3.5):100; it can be prepared by the following steps: 0.2-3.5 parts by weight of isocyanurate alkoxysilane and 100 parts by weight of spherical boron nitride are mixed at 40-80°C and 800-1200 rpm for 15-30 min.

[0036] Preferably, the mass ratio of isocyanurate alkoxysilane to spherical boron nitride in the modified spherical boron nitride is (1-3.5):100.

[0037] By adjusting the mass ratio of the modified spherical boron nitride to the isocyanurate alkoxysilane, a higher surface gloss can be achieved while maintaining good thermal conductivity (in the plane and through the plane) in the thermally conductive and flame-retardant semi-aromatic polyamide composition.

[0038] Conventional semi-aromatic polyamide resins and organic phosphonate flame retardants in the art can be used in this invention.

[0039] Optionally, the semi-aromatic polyamide resin comprises a diamine unit and a diacid unit; the diamine unit is derived from at least one of an aliphatic diamine with 6 to 12 carbon atoms; the diacid unit is derived from 45 to 100 mol% aromatic dicarboxylic acid and 0 to 55 mol% aliphatic dicarboxylic acid.

[0040] Further optionally, the aromatic dicarboxylic acid is at least one selected from terephthalic acid, isophthalic acid, 2-methylterephthalic acid, 2,5-dichloroterephthalic acid, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and 2,2'-biphenyldicarboxylic acid, wherein the aliphatic dicarboxylic acid has 4-12 carbon atoms; the diamine unit is derived from 1,4-butanediamine, 1,6-hexanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,5- The aliphatic dicarboxylic acid is selected from at least one of pentanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2,4-dimethyl-1,6-hexanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2-methyl-1,8-octanediamine, and 5-methyl-1,9-nonanediamine; the aliphatic dicarboxylic acid is selected from at least one of 1,4-succinic acid, 1,6-adipic acid, 1,8-octanediic acid, 1,9-azelaic acid, 1,10-sebacic acid, 1,11-undecanoic acid, and 1,12-dodecanoic acid.

[0041] More preferably, the semi-aromatic polyamide resin comprises a diamine unit and a diacid unit, wherein the diamine unit is derived from 1,5-pentanediamine; and the diacid unit is derived from 45-100 mol% terephthalic acid and 0-55 mol% adipic acid.

[0042] By optimizing the diamine unit and the diacid unit, the resulting thermally conductive and flame-retardant semi-aromatic polyamide composition exhibits better interplanar thermal conductivity and thermal isotropy.

[0043] Preferably, the organic phosphonate flame retardant includes at least one of aluminum diethylphosphonate, zinc diethylphosphonate, aluminum methyl ethylphosphonate, aluminum ethyl butylphosphonate, or aluminum ethylhexylphosphonate.

[0044] Preferably, the thermally conductive and flame-retardant semi-aromatic polyamide composition further includes 10 to 50 parts of reinforcing filler.

[0045] More preferably, the thermally conductive and flame-retardant semi-aromatic polyamide composition further includes 15 to 30 parts of reinforcing filler.

[0046] More preferably, the reinforcing material is at least one of glass fiber, carbon fiber, asbestos fiber, wollastonite fiber, ceramic fiber, potassium titanate whiskers, basic magnesium sulfate whiskers, silicon carbide whiskers, aluminum borate whiskers, silicon dioxide, aluminum silicate, silicon oxide, calcium carbonate, titanium dioxide, talc, wollastonite, diatomaceous earth, clay, kaolin, spherical glass, mica, or gypsum.

[0047] Preferably, the thermally conductive and flame-retardant semi-aromatic polyamide composition further includes 0.01 to 2 parts of other additives.

[0048] More preferably, the other additives are at least one of antioxidants, lubricants, or nucleating agents.

[0049] Optionally, the antioxidant is a hindered phenolic antioxidant or a phosphite antioxidant.

[0050] Optionally, the lubricant is a fluoropolymer, LLDPE, silicone oil, metal stearate, alkyl stearate, metal montanic acid, montanic ester wax, or polyethylene wax.

[0051] Optionally, the nucleating agent is talc, alumina, zirconium oxide, tin oxide, tin indium oxide, antimony tin oxide, calcium silicate, calcium carbonate, magnesium carbonate, or zeolite.

[0052] The preparation method of the above-mentioned thermally conductive and flame-retardant semi-aromatic polyamide composition includes the following steps: adding other components except for the organic phosphonate flame retardant, reinforcing material (if any) and modified spherical boron nitride from the main feed port of the extruder, adding the organic phosphonate flame retardant, reinforcing material (if any) and modified spherical boron nitride from the side feed port of the extruder, melting and blending at 250-330°C, granulating, and thus obtaining the thermally conductive and flame-retardant semi-aromatic polyamide composition.

[0053] Application of the above-mentioned thermally conductive and flame-retardant semi-aromatic polyamide composition in the preparation of electronic products.

[0054] Preferably, the electronic product is an electronic product that requires an SMT (Surface Mount Technology) process.

[0055] Optionally, the electronic products that need to undergo SMT processing include connectors, connector series components, optical cable connectors, plugs, USB series components, circuit breakers, winding elements, electric motor components, and electrical components.

[0056] Compared with the prior art, the beneficial effects of the present invention are:

[0057] The thermally conductive and flame-retardant semi-aromatic polyamide composition of the present invention has good flame-retardant properties, low surface roughness (high surface gloss), high interplanar thermal conductivity and thermal isotropic properties. Detailed Implementation

[0058] To more clearly and completely describe the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. Various changes can be made within the scope of the claims of the present invention.

[0059] The reagents used in the various embodiments and comparative examples of this invention are described below:

[0060] Semi-aromatic polyamide resin #1: Self-made, preparation method as follows: Add terephthalic acid and 1,10-decanediamine in a molar ratio of 1:1 to a pressure vessel; then add benzoic acid, sodium hypophosphite (catalyst) and deionized water; the amount of benzoic acid is 2.5% of the total amount of diamine and diacid, the weight of sodium hypophosphite is 0.1% of the weight of other materials except deionized water, and the weight of deionized water is 30% of the total weight of materials; evacuate and fill with high-purity nitrogen as a protective gas, and heat up for 2 hours under stirring. The reaction mixture was stirred at 220°C for 1 hour, and then the temperature of the reactants was raised to 230°C with stirring. The reaction was continued at a constant temperature of 230°C and a constant pressure of 2.2 MPa for 2 hours, and the pressure was kept constant by removing the water formed. After the reaction was completed, the material was discharged, and the prepolymer was vacuum dried at 80°C for 24 hours to obtain the prepolymer product. The prepolymer product was solid-phase thickened at 250°C and 50 Pa vacuum for 10 hours to obtain semi-aromatic polyamide resin 1#.

[0061] Semi-aromatic polyamide resin #2: Homemade, preparation method as follows: Add terephthalic acid, adipic acid, and 1,5-pentanediamine in a molar ratio of 6.5:3.5:10 to a pressure vessel; then add benzoic acid, sodium hypophosphite (catalyst), and deionized water; the amount of benzoic acid is 2.5% of the total amount of diamine and diacid, the weight of sodium hypophosphite is 0.1% of the weight of other added materials excluding deionized water, and the weight of deionized water is 30% of the total added material weight; evacuate and fill with high-purity nitrogen as a protective gas, and stir. The temperature was raised to 220°C within one hour, and the reaction mixture was stirred at 220°C for 1 hour. Then, the temperature of the reactants was raised to 230°C with stirring. The reaction was continued at a constant temperature of 230°C and a constant pressure of 2.2 MPa for 2 hours. The pressure was kept constant by removing the water formed. After the reaction was completed, the material was discharged, and the prepolymer was vacuum dried at 80°C for 24 hours to obtain the prepolymer product. The prepolymer product was solid-phase thickened at 250°C and 50 Pa vacuum for 10 hours to obtain semi-aromatic polyamide resin 2#.

[0062] Semi-aromatic polyamide resin #3: Homemade, preparation method as follows: Add terephthalic acid, adipic acid, and hexamethylenediamine in a molar ratio of 6:4:10 to a pressure vessel; then add benzoic acid, sodium hypophosphite (catalyst), and deionized water; the amount of benzoic acid is 2.5% of the total amount of diamine and diacid, the weight of sodium hypophosphite is 0.1% of the weight of other added materials excluding deionized water, and the weight of deionized water is 30% of the total added material weight; evacuate and fill with high-purity nitrogen as a protective gas, and heat for 2 hours under stirring. The temperature was raised to 220°C, and the reaction mixture was stirred at 220°C for 1 hour. Then, the temperature of the reactants was raised to 230°C with stirring. The reaction was continued at a constant temperature of 230°C and a constant pressure of 2.2 MPa for 2 hours. The pressure was kept constant by removing the water formed. After the reaction was completed, the material was discharged, and the prepolymer was vacuum dried at 80°C for 24 hours to obtain the prepolymer product. The prepolymer product was solid-phase thickened at 250°C and 50 Pa vacuum for 10 hours to obtain semi-aromatic polyamide resin 3#.

[0063] Semi-aromatic polyamide resin #4: Self-made, preparation method as follows: Add terephthalic acid, 1,10-sebacic acid, and 1,10-decanediamine in a molar ratio of 8.5:1.5:10 to a pressure vessel; then add benzoic acid, sodium hypophosphite (catalyst), and deionized water; the amount of benzoic acid is 2.5% of the total amount of diamine and diacid, the weight of sodium hypophosphite is 0.1% of the weight of other added materials excluding deionized water, and the weight of deionized water is 30% of the total weight of added materials; evacuate and fill with high-purity nitrogen as a protective gas, while stirring... The temperature was raised to 220°C within 2 hours of stirring, and the reaction mixture was stirred at 220°C for 1 hour. Then, the temperature of the reactants was raised to 230°C with stirring. The reaction was continued for 2 hours at a constant temperature of 230°C and a constant pressure of 2.2 MPa. The pressure was kept constant by removing the water formed. After the reaction was completed, the material was discharged, and the prepolymer was vacuum dried at 80°C for 24 hours to obtain the prepolymer product. The prepolymer product was solid-phase thickened at 250°C and 50 Pa vacuum for 10 hours to obtain semi-aromatic polyamide resin 4#.

[0064] Semi-aromatic polyamide resin #5: Homemade, preparation method as follows: Add terephthalic acid, isophthalic acid, and 1,10-decanediamine in a molar ratio of 9:1:10 to a pressure vessel; then add benzoic acid, sodium hypophosphite (catalyst), and deionized water; the amount of benzoic acid is 2.5% of the total amount of diamine and diacid, the weight of sodium hypophosphite is 0.1% of the weight of other added materials excluding deionized water, and the weight of deionized water is 30% of the total added material weight; evacuate and fill with high-purity nitrogen as a protective gas, and stir for 2 hours. The temperature was raised to 220°C, and the reaction mixture was stirred at 220°C for 1 hour. Then, the temperature of the reactants was raised to 230°C with stirring. The reaction was continued at a constant temperature of 230°C and a constant pressure of 2.2 MPa for 2 hours. The pressure was kept constant by removing the water formed. After the reaction was completed, the material was discharged, and the prepolymer was vacuum dried at 80°C for 24 hours to obtain the prepolymer product. The prepolymer product was solid-phase thickened at 250°C and 50 Pa vacuum for 10 hours to obtain semi-aromatic polyamide resin 5#.

[0065] Organic phosphinate flame retardant: aluminum diethylphosphinate, commercially available;

[0066] Reinforcing material #1: Glass fiber, OCV995, Owens Corning Composites;

[0067] Reinforcing material #2: Wollastonite, HQ-1250, Dalian Huanqiu Minerals Co., Ltd.;

[0068] Other additives: lubricant, LLDPE, commercially available;

[0069] Spherical boron nitride 1#: CFA 50M, average particle size 15μm, Kunshan Libaodi Electronic Materials;

[0070] Spherical boron nitride 2#: SA75, average particle size 75μm, SAINT-GOBAIN, FRANCE;

[0071] Spherical boron nitride 3#: SA125, average particle size 130μm, SAINT-GOBAIN, FRANCE;

[0072] Spherical boron nitride 4#: SA300, average particle size 315μm, SAINT-GOBAIN, FRANCE;

[0073] Flaky boron nitride: SP16, average particle size 16 μm, SAINT-GOBAIN, FRANCE;

[0074] Isocyanurate alkoxysilane 1#: KH-597, 1,3,5-tris(trimethoxysilylpropyl)isocyanurate, Hangzhou Jessica Chemical;

[0075] Isocyanurate alkoxysilane 2#: SF-YQ42, 1,3,5-tris(triethoxysilylpropyl)isocyanurate, Tangshan Sanfu New Materials;

[0076] Isocyanurate alkoxysilane 3#: SF-YQ43, 1,3,5-tris(methyldimethoxysilylpropyl)isocyanurate, Tangshan Sanfu New Materials;

[0077] Conventional silane coupling agent: KH-901, 3-isocyanate-propyltrimethoxysilane, Hangzhou Jessica Chemical;

[0078] Modified spherical boron nitride: self-made, the preparation process is as follows: mix isocyanurate alkoxysilane or conventional silane coupling agent with spherical boron nitride according to the formulation in Table 1, mixing temperature: 60℃, mixing time: 15min, mixing speed: 1000rpm.

[0079] Table 1. Formulation of modified spherical boron nitride (parts by weight)

[0080]

[0081] Modified flake boron nitride: self-made, the preparation process is as follows: mix 1 part by weight of conventional silane coupling agent and 100 parts by weight of flake boron nitride, mixing temperature: 60℃, mixing time: 15min, mixing speed: 1000rpm.

[0082] Unless otherwise specified, all components (e.g., organic phosphonate flame retardants, other additives) used in the parallel examples and comparative examples are the same commercially available products.

[0083] The thermally conductive and flame-retardant semi-aromatic polyamide compositions provided in the embodiments and comparative examples of this invention were subjected to performance testing according to the following test methods:

[0084] (1) Flame retardant performance test: Tested according to UL 94 standard, with a sample thickness of 0.8 mm;

[0085] (2) Thermal conductivity test: Tested according to ASTM E1461 standard, using LFA 467 HyperFlash thermal conductivity meter, test temperature: 23℃, sample size Φ10×1mm round disc, in plane and through plane directions.

[0086] (3) Surface gloss: Tested according to ISO 2813 standard, test angle 60°;

[0087] The thermally conductive and flame-retardant semi-aromatic polyamide compositions of the various embodiments and comparative examples of the present invention are prepared by the following method: According to the formulation, the components other than the organic phosphonate flame retardant, reinforcing material and modified spherical boron nitride are mixed evenly, and then added from the main feed port of a twin-screw extruder. The reinforcing material is added from the first side feed port. The organic phosphonate flame retardant and the modified spherical boron nitride / modified flake boron nitride / spherical boron nitride are added from the side feed port of the twin-screw extruder. The mixture is melt-blended at 250-330°C and granulated to obtain the thermally conductive and flame-retardant semi-aromatic polyamide composition.

[0088] Examples 1-18

[0089] Examples 1-18 provide a series of thermally conductive and flame-retardant semi-aromatic polyamide compositions, the formulations of which are shown in Tables 2 and 3.

[0090] Table 2. Formulations (parts by weight) for Examples 1-11

[0091]

[0092]

[0093] Table 3. Formulations (parts by weight) for Examples 12-18

[0094]

[0095] Comparative Example 1

[0096] This comparative example provides a thermally conductive and flame-retardant semi-aromatic polyamide composition, the formulation of which differs from that of Example 1 in that modified spherical boron nitride 1# is replaced with modified spherical boron nitride 9#.

[0097] Comparative Example 2

[0098] This comparative example provides a thermally conductive and flame-retardant semi-aromatic polyamide composition, the formulation of which differs from that of Example 1 in that modified spherical boron nitride 1# is replaced with spherical boron nitride 1#.

[0099] Comparative Example 3

[0100] This comparative example provides a thermally conductive and flame-retardant semi-aromatic polyamide composition, the formulation of which differs from that of Example 1 in that modified spherical boron nitride 1 is not added.

[0101] Comparative Example 4

[0102] This comparative example provides a thermally conductive and flame-retardant semi-aromatic polyamide composition, the formulation of which differs from that of Example 1 in that the modified spherical boron nitride 1# is replaced with modified sheet boron nitride.

[0103] The properties of the thermally conductive and flame-retardant semi-aromatic polyamide compositions of each embodiment and comparative example were determined according to the test methods mentioned above, and the test results are shown in Table 4.

[0104] Table 4 Performance test results of each embodiment and comparative example

[0105]

[0106]

[0107] As can be seen from Table 4:

[0108] The thermally conductive and flame-retardant semi-aromatic polyamide compositions of Examples 1-18 have a flame retardancy rating of V-0, a thermal conductivity of 1.63 W / m·K or higher in the in-plane direction, a thermal conductivity of 1.60 W / m·K or higher in the through-plane direction, and a surface gloss of 37° or higher. This indicates that the thermally conductive and flame-retardant semi-aromatic polyamide compositions of the present invention have good flame retardant properties, high surface gloss, high interplanar thermal conductivity, and thermal isotropic properties.

[0109] Comparative Example 1 used modified spherical boron nitride 9#, obtained by modifying spherical boron nitride with a conventional coupling agent. The resulting thermally conductive and flame-retardant semi-aromatic polyamide composition exhibited low thermal conductivity in both the in-plane and through-plane directions, as well as low surface gloss. Comparative Example 2 used unmodified spherical boron nitride 1#. The resulting thermally conductive and flame-retardant semi-aromatic polyamide composition also showed low thermal conductivity in both the in-plane and through-plane directions, along with low surface gloss. Comparative Example 3 did not use modified spherical boron nitride 1#. The resulting thermally conductive and flame-retardant semi-aromatic polyamide composition had very low thermal conductivity in both the in-plane and through-plane directions. Comparative Example 4 used modified flake boron nitride. The resulting thermally conductive and flame-retardant semi-aromatic polyamide composition exhibited relatively low thermal conductivity in the in-plane direction to some extent, and significantly low thermal conductivity in the through-plane direction.

[0110] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A thermally conductive and flame-retardant semi-aromatic polyamide composition, characterized in that, The components include the following parts by weight: 30-65 parts of semi-aromatic polyamide resin, 5-18 parts of organic phosphonate flame retardant 15-40 parts of modified spherical boron nitride; The modified spherical boron nitride is a spherical boron nitride with a surface modified isocyanurate alkoxysilane; The isocyanurate alkoxysilane is isocyanurate trialkoxysilane; The semi-aromatic polyamide resin comprises a diamine unit and a diacid unit; the diamine unit is derived from at least one of an aliphatic diamine with 6 to 12 carbon atoms; the diacid unit is derived from 45 to 100 mol% aromatic dicarboxylic acid and 0 to 55 mol% aliphatic dicarboxylic acid.

2. The thermally conductive and flame-retardant semi-aromatic polyamide composition according to claim 1, characterized in that, The average particle size of the spherical boron nitride is 15~130 μm.

3. The thermally conductive and flame-retardant semi-aromatic polyamide composition according to claim 1, characterized in that, The isocyanurate trialkoxysilane is isocyanurate trimethoxysilane.

4. The thermally conductive and flame-retardant semi-aromatic polyamide composition according to claim 1, characterized in that, The organic phosphonate flame retardant includes at least one of aluminum diethylphosphonate, zinc diethylphosphonate, aluminum methyl ethylphosphonate, aluminum ethyl butylphosphonate, or aluminum ethylhexylphosphonate.

5. The thermally conductive and flame-retardant semi-aromatic polyamide composition according to claim 1, characterized in that, The thermally conductive and flame-retardant semi-aromatic polyamide composition further includes 10-50 parts of reinforcing filler; the reinforcing material is at least one of glass fiber, carbon fiber, asbestos fiber, wollastonite fiber, ceramic fiber, potassium titanate whiskers, basic magnesium sulfate whiskers, silicon carbide whiskers, aluminum borate whiskers, silicon dioxide, aluminum silicate, silicon oxide, calcium carbonate, titanium dioxide, talc, wollastonite, diatomaceous earth, clay, kaolin, spherical glass, mica, or gypsum.

6. The thermally conductive and flame-retardant semi-aromatic polyamide composition according to claim 1, characterized in that, The thermally conductive and flame-retardant semi-aromatic polyamide composition comprises the following components in parts by weight: 35-55 parts of semi-aromatic polyamide resin, 14-18 parts of organic phosphonate flame retardant, 15-25 parts of modified spherical boron nitride.

7. A method for preparing the thermally conductive and flame-retardant semi-aromatic polyamide composition according to any one of claims 1 to 6, characterized in that, The process includes the following steps: adding all components except the organic phosphonate flame retardant and modified spherical boron nitride from the main feed port of the extruder, adding the organic phosphonate flame retardant and modified spherical boron nitride from the side feed port of the extruder, melting and blending at 250~350℃, and granulating to obtain the thermally conductive and flame-retardant semi-aromatic polyamide composition.

8. The use of the thermally conductive and flame-retardant semi-aromatic polyamide composition according to any one of claims 1 to 6 or the thermally conductive and flame-retardant semi-aromatic polyamide composition prepared by the preparation method according to claim 7 in the preparation of electronic products.

Citation Information

Patent Citations

  • Thermally conductive composition and method for preparing the same