Preparation method for improving expression precision of orthodontic round wire torque table

By using theoretical modeling and mirror polishing, a stable orthodontic square wire with a stable edge radius was fabricated, which solved the problem of insufficient torque expression accuracy of orthodontic square wires in the existing technology, and realized a stable orthodontic biomechanics system and precise tooth movement control.

CN118847745BActive Publication Date: 2026-11-24SUZHOU RUIMAIDE MEDICAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410871863.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2026-11-24
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

Existing methods for preparing orthodontic square wires make it difficult to control the accuracy of torque expression within the orthodontic bracket slots, leading to instability in the orthodontic biomechanics system.

Method used

By determining the deformation amount of each drawing pass and the deformation amount of each drawing step through theoretical modeling, and combining it with mirror polishing process, a normalized square wire with a stable edge curvature radius is prepared. This ensures that the edge bevels of normalized square wires with different cross-sectional areas of the same material are consistent, thereby improving the accuracy of torque expression.

Benefits of technology

A stable orthodontic biomechanics system was established, enabling more precise control of tooth movement and improving the torque expression accuracy of the orthodontic wire within the orthodontic bracket groove.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847745B_ABST
    Figure CN118847745B_ABST
Patent Text Reader

Abstract

This invention relates to the field of orthodontic square wire technology, specifically a method for improving the torque expression accuracy of orthodontic square wires, comprising the following steps: Step S1: Determine the deformation amount of the orthodontic square wire in each drawing pass; Step S2: Determine the initial feed wire diameter of the orthodontic square wire before drawing based on the target cross-sectional area of ​​the orthodontic square wire; Step S3: Determine the deformation amount of the orthodontic square wire in each drawing pass; Step S4: Perform a drawing-rolling series processing on the orthodontic square wire based on the deformation amount in each drawing pass and the deformation amount in each drawing pass; Step S5: Perform mirror polishing on the orthodontic square wire; This removes the oxide scale on the surface of the orthodontic square wire during the heat setting process, while the polishing particles do not damage the edge radius of the orthodontic square wire, ensuring that the edge bevels of orthodontic square wires of the same material but different cross-sectional areas remain consistent, thereby improving the torque expression accuracy of the orthodontic square wire in the orthodontic bracket groove, establishing a stable and controllable orthodontic mechanical system, and more precisely controlling tooth movement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of orthodontic square wire technology, specifically a preparation method for improving the torque expression accuracy of orthodontic square wires. Background Technology

[0002] In orthodontic treatment, torque is an important means of controlling tooth movement in three dimensions. Clinically, torque is mainly expressed through orthodontic square wires. The cross-section of the orthodontic square wire is square. When it is tied into the groove of the orthodontic bracket, which is also square, the height dimension of the orthodontic square wire is between 0.40 and 0.54 mm, while the width of the commonly used orthodontic bracket groove is 0.56 to 0.58 mm. Since the height dimension of the orthodontic square wire is smaller than the width dimension of the orthodontic bracket groove, there is a gap between the two. Therefore, the orthodontic square wire uses the torsion of its square cross-section to generate a pair of force couples on the orthodontic bracket, thereby indirectly applying orthodontic force and torque to the teeth, achieving control of the tooth root and crown in three dimensions.

[0003] Furthermore, the height of the orthodontic wire is smaller than the size of the orthodontic bracket groove. When the orthodontic wire is ligated into the orthodontic bracket groove, a gap will be created between them; this is called the clearance angle. The torque of the orthodontic wire is expressed as the torque angle after eliminating the clearance angle with the orthodontic bracket. The size of the clearance angle directly affects the torque expression of the orthodontic wire.

[0004] Furthermore, the bevel of the orthodontic square wire refers to the fact that, due to the influence of material properties and manufacturing processes, the four edges of the orthodontic square wire are not right angles but have a certain curvature. This curvature is the bevel of the orthodontic square wire. Gu Min et al. measured and analyzed the clearance angle of several commonly used orthodontic square wires and found that the clearance angle of nickel-titanium square wire is significantly larger than that of stainless steel square wire. This difference is clearly correlated with the difference in the bevel of their edges: the bevel of nickel-titanium square wire > that of stainless steel square wire. Sebanc et al. also found that the bevel of TMA wire > that of stainless steel square wire > that of nickel-chromium alloy wire. Gu Min et al. used the intercept measurement method to measure and analyze that within a 0.022-inch bracket, a 0.025-inch wide stainless steel square wire loses approximately 4° of torque for every 0.001-inch decrease in width, while a 0.025-inch wide nickel-titanium square wire loses approximately 6° of torque for every 0.001-inch decrease in width.

[0005] Therefore, it is necessary to improve the existing orthodontic square wire preparation method, reduce the radius of curvature of the four edges of the orthodontic square wire, and keep the edge bevels of orthodontic square wires of the same material but different cross-sectional dimensions consistent. This will improve the torque expression accuracy of the orthodontic square wire in the orthodontic bracket groove, provide clinicians with a stable orthodontic mechanical system, help clinicians determine a reasonable torque angle, and thus improve the orthodontic treatment effect. Summary of the Invention

[0006] In order to solve the problem that existing orthodontic square wire preparation methods have difficulty in controlling the torque expression accuracy of the orthodontic square wire in the orthodontic bracket groove, this invention provides a preparation method that improves the torque expression accuracy of orthodontic square wires.

[0007] This invention is achieved using the following technical solution:

[0008] A method for improving the accuracy of orthodontic square wire torque expression, the method comprising the following steps:

[0009] Step S1: Determine the deformation amount of the orthodontic square wire after each drawing test;

[0010] Step S2: Determine the initial feed wire diameter of the orthodontic square wire before drawing based on the target cross-sectional area of ​​the orthodontic square wire;

[0011] Step S3: Determine the deformation amount per pull pass for the orthodontic square wire;

[0012] Step S4: Perform a series of drawing-rolling processes on the orthogonal square wire based on the deformation amount of the drawing passes and the deformation amount of the drawing passes.

[0013] Step S5: Polish the orthodontic square wire to a mirror finish.

[0014] Furthermore, the drawing deformation amount is set to B. That is, when the actual drawing deformation amount of the orthodontic square wire reaches the drawing deformation amount B, an intermediate annealing is required to eliminate the structural stress of the orthodontic square wire and reduce the hardness of the orthodontic square wire. Determining the drawing deformation amount B of the orthodontic square wire includes the following steps.

[0015] Step S1.1: Select a standard diameter orthodontic square wire, set N square molds with a deformation amount of 10% for each pass, and match the cross-sectional area S1 of the first square mold with the standard diameter orthodontic square wire.

[0016] Step S1.2: Pass the standard diameter orthodontic square wire through N square dies in sequence and perform cold deformation drawing until the orthodontic square wire breaks in the nth square die. Calculate the sum of the deformation amount per pass from the first square die to the (n-1)th square die as the limit deformation amount A. The limit deformation amount per pass for breaking the orthodontic square wire is A; the value of n is 0 < n ≤ N.

[0017] Step S1.3: Set the safety factor to 80%, that is, the deformation amount B of the orthodontic square wire after one drawing heat treatment is A×80%; when the actual drawing deformation amount of the orthodontic square wire reaches the deformation amount B after one drawing heat treatment, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the orthodontic square wire.

[0018] Furthermore, the target cross-sectional area of ​​the orthodontic square wire is set as S, and the initial feed wire diameter of the orthodontic square wire before drawing is obtained based on the deformation amount B after each drawing pass.

[0019] Further, setting the deformation amount of the drawing pass as C, determining the deformation amount C of the orthodontic square wire through the drawing pass includes the following steps:

[0020] Step S3.1: Take the orthodontic square wire in the supplied state and perform a tensile test to measure the tensile strength σ1 of the orthodontic square wire; take the orthodontic square wire in the solution-treated state and perform a tensile test to measure the tensile strength σ2 of the orthodontic square wire; obtain the tensile strength σ of the orthodontic square wire; that is...

[0021] Step S3.2: Take M square molds, design the deformation amount C of the M square molds to increase sequentially with a constant t, and design the cross-sectional area S of the M square molds to decrease sequentially with a constant z.

[0022] Step S3.3: Set the theoretical tensile force F when the orthodontic square wire enters the square mold for drawing. The theoretical tensile force F is the product of the cross-sectional area S of the square mold and the tensile strength σ of the orthodontic square wire during the drawing process, i.e., F = σ × S; Thread the orthodontic square wire with an initial feed diameter of φ into M square molds, and simultaneously measure the actual tensile force F when threading into the m-th square mold. m Meanwhile, the theoretical tensile force F when penetrating the m-th square mold is obtained based on the cross-sectional area S and tensile strength σ of the m-th square mold; the value of m is 0 < m ≤ M;

[0023] Step S3.4: Determine the actual tension value F x Is it greater than the theoretical tensile force F? If F x If F ≤ F, continue inserting and pulling the (m+1)th square mold; if F x When F > F, the deformation C of each drawing pass can be obtained as C0. m-1 .

[0024] Furthermore, the step of performing a drawing-rolling tandem process on the orthogonal square wire based on the deformation amount from each drawing pass and the deformation amount from each drawing pass includes the following steps:

[0025] Step S4.1: Take a starting round wire with a diameter of φ, and set the width and height dimensions of the square die according to the target cross-sectional area S of the orthogonal square wire. Then, obtain the number G of square dies based on the deformation amount B and the deformation amount C of each drawing pass. It is a rounding function;

[0026] Step S4.2: Drawing is performed in a square die with a deformation of C in the g-th drawing pass, where the value of g is 0 < g ≤ G;

[0027] Step S4.3: Determine whether the edge radius of curvature R of the nickel-titanium orthodontic square wire is greater than 110μm, whether the edge radius of curvature R of the TMA orthodontic square wire is greater than 90μm, and whether the edge radius of curvature R of the stainless steel orthodontic square wire is greater than 90μm. If they are true, proceed to step S4.4; if they are not true, proceed to step S4.6.

[0028] Step S4.4: Roll the orthogonal square wire using a flat wire rolling mill; the outer surfaces of two relatively moving rolls in the X direction contact the two sides of the orthogonal square wire in the width direction, and the outer surfaces of two relatively moving rolls in the Y direction contact the two sides of the orthogonal square wire in the height direction; by screwing in or unscrewing the roll pressing amount knob in the X and / or Y directions, control the pressing amount of the rolls in the X and / or Y directions, so that the dimensions of the orthogonal square wire in the width and height directions are further reduced, and the orthogonal square wire is squeezed towards the four edge arc directions, thereby reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;

[0029] Step S4.5: After rolling, determine whether the edge radius of the nickel-titanium orthogonal square wire is 90μm≤R≤110μm, whether the edge radius of the TMA orthogonal square wire is 70μm≤R≤90μm, and whether the edge radius of the stainless steel orthogonal square wire is 70μm≤R≤90μm. If they are true, proceed to step S4.7; if they are not true, proceed to step S4.4.

[0030] Step S4.6: Determine whether the edge radius R of the orthodontic square wire matches the target edge radius R. 目 If the conditions are met, the orthodontic square wire preparation is complete; if not, proceed to step S4.7.

[0031] Step S4.7: In the g+1th drawing pass, the deformation amount is C in a square die, where the value of g is 0 < g ≤ G; proceed to step S4.3.

[0032] Furthermore, the amount of downward pressure of the rolls in both the X and Y directions is no more than 0.05 mm each time.

[0033] Furthermore, the orthodontic square wire includes TMA orthodontic square wire, stainless steel orthodontic square wire, and nickel-titanium orthodontic square wire; the target edge radius R of the TMA orthodontic square wire... 目 The target edge radius R of the stainless steel orthodontic square wire is 60±10μm. 目 The target edge radius R of the nickel-titanium orthodontic square wire is 60±10μm. 目It is 80±10μm.

[0034] Furthermore, the mirror polishing of the orthodontic square wire includes the following steps:

[0035] Step S5.1: Place the orthodontic square wire into the placement groove that matches the outline of the orthodontic square wire, then apply water-soluble glue to both ends and the middle of the orthodontic square wire, and attach the orthodontic square wire to the bottom of the placement groove.

[0036] Step S5.2: Using compressed air as power, select elastic polishing particles and use a programmed nozzle to bombard the orthodontic square wire placed inside the placement groove with polishing particles. At the same time, use the depressurization valve to adjust the speed of the nozzle spraying polishing particles so that the nozzle can reciprocate along the contour of the placement groove; the polishing particles after colliding with the orthodontic square wire are discharged from the leakage hole at the bottom of the placement groove.

[0037] Step S5.3: After spraying, immerse the placement groove with the orthodontic square wire attached in water to dissolve the water-soluble glue, so that the orthodontic square wire is separated from the placement groove, and blow dry the moisture on the surface of the orthodontic square wire and the placement groove.

[0038] Step S5.4: Flip the orthodontic square wire and repeat steps S5.1, S5.2, and S5.3 to obtain the orthodontic square wire with the surface oxide scale and scratches removed.

[0039] Furthermore, the surface roughness R of the orthodontic square wire after mirror polishing... a No larger than 0.8μm.

[0040] Furthermore, the hardness value of the polishing particles is between 0.2 and 0.5 times the hardness value of the orthogonal square wire.

[0041] This invention features a reasonable and reliable structural design. Through theoretical modeling, the parameters of the orthodontic square wire during manufacturing can be determined. The deformation per drawing pass is the critical cold deformation of the orthodontic square wire during the drawing process, and the deformation per drawing pass is the critical drawing force that the orthodontic square wire can withstand in each drawing pass. Obtaining the deformation per drawing pass (B) and the deformation per drawing pass (C) allows for the optimal determination of the number of drawing dies and the drawing force based on the target dimensions of the orthodontic square wire. The core front-end process involves a series of orthodontic square wire drawing and rolling processes, producing orthodontic square wires with stable edge curvature radii. The core back-end process is mirror polishing, which removes the oxide scale from the surface of the orthodontic square wire during heat setting. More importantly, the polishing particles do not damage the edge curvature radius of the orthodontic square wire, ensuring that the edge bevels of orthodontic square wires of the same material but different cross-sectional areas remain consistent. This improves the torque expression accuracy of the orthodontic square wire within the orthodontic bracket groove, establishing a stable and controllable orthodontic mechanical system for more precise control of tooth movement. Attached Figure Description

[0042] Figure 1 This is a schematic diagram of the process flow of the present invention.

[0043] Figure 2 This is a stress-strain curve diagram of a 0.014×0.025 inch nickel-titanium orthogonal square wire in the supplied state and solution-treated state in this invention;

[0044] Figure 3 This is a stress-strain curve diagram of a 0.017×0.025 inch TMA orthodontic square wire in the supplied state and solution-treated state in this invention;

[0045] Figure 4 This is a stress-strain curve diagram of a 0.019×0.025 inch stainless steel orthogonal square wire in the supplied state and solution-treated state in this invention;

[0046] Figure 5 This is a schematic diagram of the edge radius of the 0.014×0.025 inch nickel-titanium orthodontic square wire in Embodiment 1 of the present invention;

[0047] Figure 6 This is a schematic diagram of the edge radius of the 0.017×0.025 inch TMA orthodontic square wire in Embodiment 2 of the present invention;

[0048] Figure 7 This is a schematic diagram of the edge radius of the 0.019×0.025 inch stainless steel orthodontic square wire in Embodiment 3 of the present invention;

[0049] Figure 8 This is a schematic diagram of the structure of the placement groove and nozzle in this invention.

[0050] In the diagram: 1-placement groove, 2-nozzle, 3-exhaust hole. Detailed Implementation

[0051] The core processes in the fabrication of orthodontic square wires are the total deformation and the deformation per pass. The drawing parameters of orthodontic square wires made of different materials are different, and the drawing parameters of orthodontic square wires made of the same material but with different proportions are also different. This invention proposes a fabrication method to improve the accuracy of torque expression of orthodontic square wires. Unlike the existing technology that relies on the experience of workers to judge the drawing parameters, this invention proposes a replicable, safe and efficient fabrication method by theoretical modeling and combining the processing performance characteristics of orthodontic square wires made of different materials during the specific drawing process.

[0052] Example 1

[0053] Taking the fabrication of a nickel-titanium orthodontic square wire with a target size of 0.014 × 0.025 inches as an example, a method for improving the torque expression accuracy of the orthodontic square wire is described in the attached figure. Figure 1 Appendix Figure 2Appendix Figure 5 As shown, the method includes the following steps:

[0054] Step S1: Determine the deformation amount of the orthodontic square wire after drawing heat treatment; set the deformation amount of the drawing heat treatment as B, that is, when the actual drawing deformation amount of the orthodontic square wire reaches the deformation amount of the drawing heat treatment B, an intermediate annealing is required to eliminate the structural stress of the orthodontic square wire and reduce the hardness of the orthodontic square wire; determining the deformation amount B of the orthodontic square wire after drawing heat treatment includes the following steps:

[0055] Step S1.1: Select a 1.0mm diameter nickel-titanium orthodontic square wire, and set N square molds with a deformation amount of 10% for each pass, wherein the cross-sectional area of ​​the square molds matches that of the 1.0mm diameter nickel-titanium orthodontic square wire; that is, the cross-sectional areas of the N square molds are as follows: S1 = 0.9mm. 2 S2 = 0.81 mm 2 S3 = 0.73 mm 2 S4 = 0.66 mm 2 S5 = 0.59 mm 2 ...;

[0056] Step S1.2: Pass the 1.0mm nickel-titanium orthodontic square wire through N square dies in sequence and perform cold deformation drawing until the nickel-titanium orthodontic square wire breaks in the 6th square die. Calculate the sum of the deformation amount from the first square die to the fifth square die as the limit deformation amount, which is 50%. The limit deformation amount A of the nickel-titanium orthodontic square wire is 50%.

[0057] Step S1.3: Set the safety factor to 80%, that is, the deformation amount B of the drawing heat treatment of the nickel-titanium orthogonal square wire is A×80%=40%; when the actual drawing deformation amount of the nickel-titanium orthogonal square wire reaches the deformation amount B of the drawing heat treatment, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the nickel-titanium orthogonal square wire.

[0058] Step S2: Set the target cross-sectional area S of the nickel-titanium orthodontic square wire to 0.23 mm. 2 The target size of the nickel-titanium orthodontic square wire is 0.014 × 0.025 inches. Taking the deformation amount B from the drawing pass as 40%, the initial feed wire diameter of the nickel-titanium orthodontic square wire before drawing is obtained based on the deformation amount B = 40%.

[0059] Step S3: Set the deformation amount of the drawing pass as C. Determining the deformation amount C of the drawing pass for the nickel-titanium orthodontic square wire includes the following steps:

[0060] Step S3.1: Three sets of 0.014×0.025 inch nickel-titanium orthodontic square wires in the supplied condition were subjected to tensile tests. The tensile strengths of the three sets of nickel-titanium orthodontic square wires were measured to be 1849.1 MPa, 1855.5 MPa, and 1846.7 MPa, respectively. The average value was taken as the tensile strength σ1 = 1849.4 MPa of the nickel-titanium orthodontic square wire in the supplied condition. Three sets of nickel-titanium orthodontic square wires in the solution-treated condition were also subjected to tensile tests. The tensile strengths of the three sets of nickel-titanium orthodontic square wires were measured to be 534.0 MPa, 544.5 MPa, and 528.8 MPa, respectively. The average value was taken as the tensile strength σ2 = 535.8 MPa of the nickel-titanium orthodontic square wire in the solution-treated condition. The tensile strength σ of the nickel-titanium orthodontic square wire was thus obtained. The tensile test for measuring the tensile strength of orthodontic square wires is an existing technique and will not be elaborated further here.

[0061] Step S3.2: Take 8 square molds and design the deformation C per pass for the 8 square molds to increase sequentially by a constant 2%, i.e., C1 is 2%, C2 is 4%, C3 is 6%, C4 is 8%, C5 is 10%, C6 is 12%, C7 is 14%, and C8 is 16%. Also, design the cross-sectional area S of the 8 square molds to be a constant 0.02 mm. 2 The values ​​decrease sequentially, meaning S1 is 0.98 mm. 2 S2 is 0.96mm 2 S3 is 0.94mm. 2 S4 is 0.92mm. 2 S5 is 0.90mm 2 S6 is 0.88mm 2 The S7 is 0.86mm. 2 The S8 is 0.84mm. 2 ;

[0062] Step S3.3: Set the theoretical tensile force value F when the nickel-titanium orthodontic square wire enters the square die for drawing. The theoretical tensile force value F is the product of the cross-sectional area S of the square die and the tensile strength σ of the nickel-titanium orthodontic square wire during the drawing process, that is, F=σ×S;

[0063] A nickel-titanium orthodontic square wire with an initial infeed diameter of φ = 1.0 mm is first inserted into the first square mold. At the same time, the actual tensile force F1 = 557 N is measured when it is inserted into the first square mold. Based on the cross-sectional area S and tensile strength σ of the first square mold, the theoretical tensile force F = 0.98 × 1192.6 = 1168.8 N is obtained when it is inserted into the first square mold; that is, F1 < F.

[0064] Repeat the above steps to measure the actual tensile force F2 = 636 N when penetrating the second square mold, and obtain the theoretical tensile force F = 0.96 × 1192.6 = 1144.9 N when penetrating the second square mold; that is, F2 < F;

[0065] The actual tensile force when the die was inserted into the third square mold was measured to be F3 = 759 N, and the theoretical tensile force when the die was inserted into the third square mold was obtained to be F = 0.94 × 1192.6 = 1121.0 N; that is, F3 < F;

[0066] The actual tensile force when the mold was inserted into the fourth square mold was measured to be F4 = 861 N, and the theoretical tensile force when the mold was inserted into the fourth square mold was obtained to be F = 0.92 × 1192.6 = 1097.2 N; that is, F4 < F;

[0067] The actual tensile force when the 5th square mold was inserted was measured to be F5 = 972 N, and the theoretical tensile force when the 5th square mold was inserted was obtained to be F = 0.90 × 1192.6 = 1073.3 N; that is, F5 < F;

[0068] The actual tensile force when the 6th square mold was inserted was measured to be F6 = 1067 N, and the theoretical tensile force when inserting the 6th square mold was obtained to be F = 0.88 × 1192.6 = 1049.5 N; at this time, F6 > F.

[0069] It can be seen that when a nickel-titanium orthodontic square wire with a diameter of 1.0 mm passes through a square die with a deformation of 12% in the 6th pass, its actual tensile force F6 is greater than the theoretical tensile force F. Therefore, the deformation of the drawing pass for preparing a nickel-titanium orthodontic square wire with a size of 0.014×0.025 inch is C=C5=10%.

[0070] Step S4: Based on the drawing deformation amount B of 40% and the drawing deformation amount C of 10% obtained from steps S1 to S3 above, the nickel-titanium orthogonal square wire is subjected to a drawing-rolling series processing, including the following steps:

[0071] Step S4.1: Take a nickel-titanium round wire with an initial infeed diameter of φ = 0.70 mm, and set the target cross-sectional area S of the nickel-titanium orthodontic square wire to 0.23 mm. 2 The target size of the square die is 0.014 × 0.025 inches. Then, based on the drawing pass deformation amount B being 40% and the drawing pass deformation amount C being 10%, the number of square dies G is determined. It is a rounding function;

[0072] Step S4.2: Drawing is performed in a square die with a deformation of C in the g-th drawing pass, where the value of g is 0 < g ≤ G;

[0073] Step S4.3: Determine whether the edge radius of curvature R of the nickel-titanium orthodontic square wire is greater than 110μm. If it is true, proceed to step S4.4; if it is not true, proceed to step S4.6.

[0074] Step S4.4: Roll the nickel-titanium orthogonal square wire using a flat wire rolling mill; the outer surfaces of two relatively moving rolls in the X direction contact the two sides of the nickel-titanium orthogonal square wire in the width direction, and the outer surfaces of two relatively moving rolls in the Y direction contact the two sides of the nickel-titanium orthogonal square wire in the height direction; by screwing in or unscrewing the roll pressing amount knob in the X and / or Y directions, control the pressing amount of the rolls in the X and / or Y directions, so that the size of the nickel-titanium orthogonal square wire in the width and height directions is further reduced, and the nickel-titanium orthogonal square wire is squeezed towards the four edge arc directions, thereby recovering and reducing the gradually increasing four edge arc radius generated by the square die drawing process;

[0075] Step S4.5: After rolling, determine whether the edge radius of the nickel-titanium orthogonal square wire is 90μm≤R≤110μm. If it is true, proceed to step S4.7; if it is not true, proceed to step S4.4.

[0076] Step S4.6: Determine whether the edge radius R of the nickel-titanium orthodontic square wire meets the target edge radius R. 目 The target edge radius R of the nickel-titanium orthogonal square wire 目 The value is 80±10μm; if this is met, the target size is 0.014×0.025inch and the target cross-sectional area S is 0.23mm. 2 The preparation of the nickel-titanium orthodontic square wire is completed; if it does not meet the requirements, proceed to step S4.7.

[0077] Step S4.7: In the g+1th drawing pass, the deformation C is 10% in a square die, where the value of g is 0 < g ≤ G; proceed to step S4.3.

[0078] The amount of downward pressure of the rolls in both the X and Y directions shall not exceed 0.05 mm each time.

[0079] By taking steps S1, S2, and S3, the parameters of the nickel-titanium orthogonal square wire during the manufacturing process can be obtained. Among them, the deformation amount B obtained in the drawing process is the critical cold deformation amount of the nickel-titanium orthogonal square wire during the drawing process, and the deformation amount C in each drawing pass is the critical drawing force that the nickel-titanium orthogonal square wire can withstand in each drawing process. Obtaining the deformation amount B in the drawing process and the deformation amount C in each drawing pass can, to the greatest extent possible, determine the optimal number of drawing dies and the drawing force based on the target size of the nickel-titanium orthogonal square wire.

[0080] Step S4 involves preparing a nickel-titanium orthodontic square wire based on the parameters measured in steps S1, S2, and S3, to obtain a nickel-titanium orthodontic square wire that conforms to torque expression. Compared with the torque expression of existing nickel-titanium orthodontic square wires prepared based on the experience of workers, this invention greatly improves the accuracy of torque expression of nickel-titanium orthodontic square wires.

[0081] The smaller the radius of curvature of the orthodontic wire, the better. A smaller radius results in a sharper edge, which can easily scratch the patient's oral mucosa and the dentist's hand. Conversely, an increased radius increases the probability of the wire spinning within the bracket slot, leading to increased torque loss. The torque applied to the teeth by the dentist is wasted due to the larger radius, ultimately resulting in ineffective treatment.

[0082] As attached Figure 5 As shown, the edge curvature radii of the 0.014×0.025 inch nickel-titanium orthodontic square wires are 85μm, 77μm, 82μm, and 77μm, respectively.

[0083] Step S5: Mirror polishing of the nickel-titanium orthodontic square wire; After the nickel-titanium orthodontic square wire of the target size is prepared through steps S1 to S4, since its microstructure is in a cold-drawn or cold-rolled state, it needs to be heat-set to an arch shape that matches the ideal dental arch shape through subsequent heat treatment processes; After the nickel-titanium orthodontic square wire is heat-set, the surface of the wire will oxidize, so mirror polishing is required to remove the oxide scale from the surface of the wire.

[0084] Traditional methods for removing oxide scale from orthodontic wire surfaces include mechanical polishing, electrochemical polishing, and chemical etching. These processes involve complex equipment, environmental pollution, and high costs. More importantly, while removing the oxide scale, the polishing process rounds the edge radius of the orthodontic wire, increasing it and reducing the torque expression accuracy. Therefore, this invention proposes a mirror polishing method that removes the oxide scale while avoiding increasing the edge radius of the orthodontic wire. (See attached diagram.) Figure 8 As shown; the specific steps are as follows:

[0085] Step S5.1: Place the orthodontic square wire into the placement groove 1 that matches the outline of the orthodontic square wire, then apply water-soluble glue to both ends and the middle of the orthodontic square wire, and attach the orthodontic square wire to the bottom of the placement groove 1.

[0086] Step S5.2: Using compressed air as power, select elastic polishing particles, and use a programmed nozzle 2 to bombard the orthodontic square wire placed inside the placement groove 1 with polishing particles. At the same time, use the depressurization valve to adjust the speed of the polishing particles sprayed by the nozzle 2, so that the nozzle 2 can reciprocate along the contour of the placement groove 1; the polishing particles after colliding with the orthodontic square wire are discharged from the leakage hole 3 at the bottom of the placement groove 1.

[0087] During bombardment, the polishing particles sprayed onto the side wall of placement tank 1 are reflected to the side of the orthodontic square wire by their elastic characteristics. In this way, each bombardment can spray onto three sides of the orthodontic square wire, and the characteristics of its hardness being between 0.2 and 0.5 times the hardness of the orthodontic square wire will not damage the edge radius of the prepared orthodontic square wire. The polishing particles and the oxide scale of the orthodontic square wire are fully mechanically rubbed, removing the oxide scale and scratches on the surface of the orthodontic square wire.

[0088] Step S5.3: After spraying, immerse the placement groove 1 with the orthodontic square wire attached in water to dissolve the water-soluble glue, so that the orthodontic square wire is separated from the placement groove 1, and blow dry the moisture on the surface of the orthodontic square wire and the placement groove 1.

[0089] Step S5.4: Flip the orthodontic square wire and repeat steps S5.1, S5.2, and S5.3 to obtain the orthodontic square wire with the surface oxide scale and scratches removed.

[0090] Surface roughness R of orthodontic square wire after mirror polishing a The surface thickness is no greater than 0.8μm, with a glossy finish, clean and free of oil stains, obvious scratches, folds, and burrs.

[0091] The hardness of the polishing particles is between 0.2 and 0.5 times that of the orthodontic square wire.

[0092] The computer-controlled nozzle 2 moves along a trajectory that reciprocates within a placement groove 1 that matches the outline of the orthodontic square wire, ensuring the uniformity and consistency of the mirror polishing process.

[0093] Example 2

[0094] Taking the fabrication of a TMA orthodontic square wire with a target size of 0.017 × 0.025 inches as an example, a method for improving the torque expression accuracy of the orthodontic square wire is described in the attached figure. Figure 1 Appendix Figure 3 Appendix Figure 6 As shown, the method includes the following steps:

[0095] Step S1: Determine the deformation amount of the orthodontic square wire after drawing; set the deformation amount of the drawing to B, that is, when the actual drawing deformation amount of the orthodontic square wire reaches the deformation amount of the drawing to B, an intermediate annealing is required to eliminate the structural stress of the orthodontic square wire and reduce the hardness of the orthodontic square wire; determining the deformation amount B of the orthodontic square wire after drawing includes the following steps.

[0096] Step S1.1: Select a 1.0mm diameter TMA orthodontic square wire, and set N square molds with a deformation amount of 10% for each pass, ensuring that the cross-sectional area of ​​the square molds matches the 1.0mm diameter TMA orthodontic square wire; that is, the cross-sectional areas of the N square molds are as follows: S1 = 0.9mm. 2 S2 = 0.81 mm 2 S3 = 0.73 mm 2 S4 = 0.66 mm 2 S5 = 0.59 mm 2 ...;

[0097] Step S1.2: Pass the 1.0mm TMA orthodontic square wire through N square dies in sequence and perform cold deformation square wire drawing until the TMA orthodontic square wire breaks in the 4th square die. Calculate the sum of the deformation amount per pass from the first square die to the third square die as the limit deformation amount per pass, which is 30%. The limit deformation amount A of the TMA orthodontic square wire is 30%.

[0098] Step S1.3: Set the safety factor to 80%, that is, the deformation amount B of the TMA orthodontic square wire after one drawing heat treatment is A×80%=24%; when the actual drawing deformation amount of the TMA orthodontic square wire reaches the deformation amount B after one drawing heat treatment, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the TMA orthodontic square wire.

[0099] Step S2: Set the target cross-sectional area S of the TMA orthodontic square wire to 0.27 mm. 2 The target size of the TMA orthodontic square wire is 0.017 × 0.025 inches. Taking the deformation amount B from the drawing pass as 24%, the initial feed wire diameter of the TMA orthodontic square wire before drawing is obtained based on the deformation amount B = 24%.

[0100]

[0101] Step S3: Set the deformation amount of the drawing pass as C, and determine the deformation amount C of the drawing pass of the TMA orthodontic square wire, which includes the following steps:

[0102] Step S3.1: Three sets of 0.017×0.025inch TMA orthodontic square wires in the supplied condition were subjected to tensile tests. The tensile strengths of the three sets of TMA orthodontic square wires were measured to be 1312.9MPa, 1285.6MPa, and 1302.8MPa, respectively. The average value was taken as the tensile strength σ1 of the TMA orthodontic square wire in the supplied condition, which is 1300.4MPa. Three sets of TMA orthodontic square wires in the solution-treated condition were also subjected to tensile tests. The tensile strengths of the three sets of TMA orthodontic square wires were measured to be 946.0MPa, 955.5MPa, and 944.5MPa, respectively. The average value was taken as the tensile strength σ2 of the TMA orthodontic square wire in the solution-treated condition, which is 948.7MPa. The tensile strength σ of the TMA orthodontic square wire was thus obtained. The tensile test for measuring the tensile strength of orthodontic square wires is an existing technique and will not be elaborated further here.

[0103] Step S3.2: Take 8 square molds and design the deformation C per pass for the 8 square molds to increase sequentially by a constant 2%, i.e., C1 is 2%, C2 is 4%, C3 is 6%, C4 is 8%, C5 is 10%, C6 is 12%, C7 is 14%, and C8 is 16%. Also, design the cross-sectional area S of the 8 square molds to be a constant 0.02 mm. 2 The values ​​decrease sequentially, meaning S1 is 0.98 mm. 2 S2 is 0.96mm 2 S3 is 0.94mm. 2 S4 is 0.92mm 2 S5 is 0.90mm 2 S6 is 0.88mm 2 The S7 is 0.86mm. 2 The S8 is 0.84mm. 2 ;

[0104] Step S3.3: Set the theoretical tensile force value F when the TMA orthodontic square wire enters the square die for drawing. The theoretical tensile force value F is the product of the cross-sectional area S of the square die and the tensile strength σ of the TMA orthodontic square wire during the drawing process, that is, F=σ×S;

[0105] The TMA orthodontic square wire with an initial infeed diameter of φ = 1.0 mm is first inserted into the first square mold. At the same time, the actual tensile force F1 = 950 N is measured when it is inserted into the first square mold. Based on the cross-sectional area S and tensile strength σ of the first square mold, the theoretical tensile force F = 0.98 × 1124.6 = 1102.1 N is obtained when it is inserted into the first square mold; that is, F1 < F.

[0106] Repeat the above steps to measure the actual tensile force F2 = 1002 N when penetrating the second square mold, and obtain the theoretical tensile force F = 0.96 × 1124.6 = 1079.6 N when penetrating the second square mold; that is, F2 < F;

[0107] The actual tensile force when the material penetrates the third square mold is measured to be F3 = 1051 N, and the theoretical tensile force when penetrating the third square mold is obtained as F = 0.94 × 1124.6 = 1057.1 N; that is, F3 < F.

[0108] The actual tensile force when the die was inserted into the fourth square mold was measured to be F4 = 1136 N, and the theoretical tensile force when the die was inserted into the fourth square mold was obtained to be F = 0.92 × 1124.6 = 1034.6 N; at this time, F4 > F.

[0109] It can be seen that when a TMA orthodontic square wire with a diameter of 1.0 mm passes through a square die with a deformation of 8% in the 4th pass, its actual tensile force F4 is greater than the theoretical tensile force F. Therefore, the deformation of the TMA orthodontic square wire with a size of 0.017×0.025 inch in the drawing pass is C=C3=6%.

[0110] Step S4: Based on the drawing deformation amount B of 24% and the drawing deformation amount C of 6% obtained from steps S1 to S3 above, the TMA orthogonal square wire is subjected to a drawing-rolling series process, including the following steps:

[0111] Step S4.1: Take a TMA round wire with an initial infeed diameter of φ = 0.67 mm, and set the target cross-sectional area S of the TMA orthodontic square wire to 0.27 mm. 2 The target size of the square die is 0.017 × 0.025 inches. Then, based on the drawing pass deformation amount B being 24% and the drawing pass deformation amount C being 6%, the number of square dies G is determined. It is a rounding function;

[0112] Step S4.2: Drawing is performed in a square die with a deformation of C in the g-th drawing pass, where the value of g is 0 < g ≤ G;

[0113] Step S4.3: Determine whether the edge radius of curvature R of the TMA orthodontic square wire is greater than 90μm. If it is true, proceed to step S4.4; if it is not true, proceed to step S4.6.

[0114] Step S4.4: Roll the TMA orthogonal square wire using a flat wire rolling mill; the outer surfaces of two relatively moving rolls in the X direction contact the two sides of the TMA orthogonal square wire in the width direction, and the outer surfaces of two relatively moving rolls in the Y direction contact the two sides of the TMA orthogonal square wire in the height direction; by screwing in or unscrewing the roll pressing amount knob in the X and / or Y directions, control the pressing amount of the rolls in the X and / or Y directions, so that the dimensions of the TMA orthogonal square wire in the width and height directions are further reduced, and the TMA orthogonal square wire is squeezed towards the four edge arc directions, thereby reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;

[0115] Step S4.5: After rolling, determine whether the edge radius of the TMA orthogonal square wire is 70μm≤R≤90μm. If it is true, proceed to step S4.7; if it is not true, proceed to step S4.4.

[0116] Step S4.6: Determine whether the edge radius R of the TMA orthodontic square wire matches the target edge radius R. 目 The target edge radius R of the TMA orthodontic square wire 目 The value is 60±10μm. If this is met, the target size is 0.017×0.025inch, and the target cross-sectional area S is 0.27mm. 2 The TMA orthodontic square wire preparation is complete; if it does not meet the requirements, proceed to step S4.7.

[0117] Step S4.7: In the g+1th drawing pass, the deformation C is 6% in a square die, where the value of g is 0 < g ≤ G; proceed to step S4.3.

[0118] The amount of downward pressure of the rolls in both the X and Y directions shall not exceed 0.05 mm each time.

[0119] By taking steps S1, S2, and S3, the parameters of the TMA orthodontic square wire during the manufacturing process can be obtained. Among them, the deformation amount B obtained in the drawing process is the critical cold deformation amount of the TMA orthodontic square wire during the drawing process, and the deformation amount C in each drawing pass is the critical drawing force that the TMA orthodontic square wire can withstand in each drawing process. Obtaining the deformation amount B and the deformation amount C in each drawing pass can determine the optimal number of drawing dies and the drawing force based on the target size of the TMA orthodontic square wire to the greatest extent.

[0120] Step S4 involves preparing the TMA orthodontic square wire based on the parameters measured in steps S1, S2, and S3, to obtain a TMA orthodontic square wire that conforms to torque expression. Compared with the torque expression of existing TMA orthodontic square wires prepared based on the experience of workers, this invention greatly improves the accuracy of torque expression of TMA orthodontic square wires.

[0121] As attached Figure 6 As shown, the edge curvature radii of the 0.017×0.025 inch TMA orthodontic square wires are 43μm, 45μm, 53μm, and 49μm, respectively.

[0122] After heat treatment and shaping, the surface of TMA orthodontic square wires will also oxidize, requiring mirror polishing to remove the oxide scale. The mirror polishing process for TMA orthodontic square wires is the same as step S5 in Example 1, and will not be repeated here.

[0123] Example 3

[0124] Taking the fabrication of a stainless steel orthodontic square wire with a target size of 0.019 × 0.025 inch as an example, a method for improving the torque expression accuracy of the orthodontic square wire is described in the attached figure. Figure 1 Appendix Figure 4 Appendix Figure 7 As shown, the method includes the following steps:

[0125] Step S1: Determine the deformation amount of the orthodontic square wire after drawing; set the deformation amount of the drawing to B, that is, when the actual drawing deformation amount of the orthodontic square wire reaches the deformation amount of the drawing to B, an intermediate annealing is required to eliminate the structural stress of the orthodontic square wire and reduce the hardness of the orthodontic square wire; determining the deformation amount B of the orthodontic square wire after drawing includes the following steps.

[0126] Step S1.1: Select a stainless steel orthodontic square wire with a diameter of 1.0 mm, and set N square molds with a deformation amount of 10% for each pass, and the cross-sectional area of ​​the square molds matches that of the 1.0 mm stainless steel orthodontic square wire; that is, the cross-sectional areas of the N square molds are as follows: S1 = 0.9 mm. 2 S2 = 0.81 mm 2 S3 = 0.73 mm 2 S4 = 0.66 mm 2 S5 = 0.59 mm 2 ...;

[0127] Step S1.2: Pass the 1.0mm stainless steel orthodontic square wire through N square dies in sequence and perform cold deformation square wire drawing until the stainless steel orthodontic square wire breaks in the 6th square die. Calculate the sum of the deformation amount from the first square die to the fifth square die as the limit deformation amount, which is 50%. The limit deformation amount A of the stainless steel orthodontic square wire is 50%.

[0128] Step S1.3: Set the safety factor to 80%, that is, the deformation amount B of the stainless steel orthogonal square wire after drawing is A×80%=40%; when the actual drawing deformation amount of the stainless steel orthogonal square wire reaches the deformation amount B after drawing, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation process of the stainless steel orthogonal square wire.

[0129] Step S2: Set the target cross-sectional area S of the stainless steel orthodontic square wire to 0.31 mm. 2 The target size of the stainless steel orthogonal square wire is 0.019 × 0.025 inches. Taking the deformation amount B from the drawing pass as 40%, the initial feed wire diameter of the stainless steel orthogonal square wire before drawing is obtained based on the deformation amount B = 40%.

[0130] Step S3: Set the deformation amount of the drawing pass as C. Determining the deformation amount C of the drawing pass for stainless steel orthogonal square wire includes the following steps:

[0131] Step S3.1: Take three sets of 0.019×0.025 inch stainless steel orthogonal square wires in the supplied condition and conduct tensile tests. The tensile strengths of the three sets of stainless steel orthogonal square wires are measured to be 1976.8 MPa, 1946.6 MPa, and 1963.4 MPa, respectively. Take the average value as the tensile strength σ1 of the stainless steel orthogonal square wire in the supplied condition, which is 1962.9 MPa. Take three sets of stainless steel orthogonal square wires in the solution-treated condition and conduct tensile tests. The tensile strengths of the three sets of stainless steel orthogonal square wires are measured to be 867.9 MPa, 869.1 MPa, and 865.8 MPa, respectively. Take the average value as the tensile strength σ2 of the stainless steel orthogonal square wire in the solution-treated condition, which is 867.6 MPa. The tensile strength σ of the stainless steel orthogonal square wire is thus obtained. The tensile test for measuring the tensile strength of orthodontic square wires is an existing technique and will not be elaborated further here.

[0132] Step S3.2: Take 8 square molds and design the deformation C per pass for the 8 square molds to increase sequentially by a constant 2%, i.e., C1 is 2%, C2 is 4%, C3 is 6%, C4 is 8%, C5 is 10%, C6 is 12%, C7 is 14%, and C8 is 16%. Also, design the cross-sectional area S of the 8 square molds to be a constant 0.02 mm. 2 The values ​​decrease sequentially, meaning S1 is 0.98 mm. 2 S2 is 0.96mm 2 S3 is 0.94mm. 2 S4 is 0.92mm 2 S5 is 0.90mm 2 S6 is 0.88mm 2 The S7 is 0.86mm. 2The S8 is 0.84mm. 2 ;

[0133] Step S3.3: Set the theoretical tensile force value F when the stainless steel orthogonal square wire enters the square die for drawing. The theoretical tensile force value F is the product of the cross-sectional area S of the square die and the tensile strength σ of the stainless steel orthogonal square wire during the drawing process, that is, F=σ×S;

[0134] A stainless steel orthodontic square wire with an initial infeed diameter of φ = 1.0 mm is first inserted into the first square mold. At the same time, the actual tensile force F1 = 876 N is measured when it is inserted into the first square mold. Based on the cross-sectional area S and tensile strength σ of the first square mold, the theoretical tensile force F = 0.98 × 1415.3 = 1387.0 N is obtained when it is inserted into the first square mold; that is, F1 < F.

[0135] Repeat the above steps to measure the actual tensile force F2 = 992 N when penetrating the second square mold. The theoretical tensile force F when penetrating the second square mold is obtained as F = 0.96 × 1415.3 = 1358.7 N; that is, F2 < F.

[0136] The actual tensile force when the material penetrates the third square mold is measured to be F3 = 1048 N, and the theoretical tensile force when penetrating the third square mold is obtained as F = 0.94 × 1415.3 = 1330.4 N; that is, F3 < F.

[0137] The actual tensile force when the mold was inserted into the fourth square mold was measured to be F4 = 1144 N, and the theoretical tensile force when the mold was inserted into the fourth square mold was obtained to be F = 0.92 × 1415.3 = 1302.1 N; at this time, F4 < F;

[0138] The actual tensile force when the 5th square mold was inserted was measured to be F5 = 1257 N, and the theoretical tensile force when the 5th square mold was inserted was obtained to be F = 0.90 × 1415.3 = 1273.8 N; at this time, F5 < F;

[0139] The actual tensile force when penetrating the 6th square mold was measured to be F6 = 1341 N, and the theoretical tensile force when penetrating the 6th square mold was obtained to be F = 0.88 × 1415.3 = 1245.46 N; at this time, F6 > F.

[0140] It can be seen that when a stainless steel orthodontic square wire with a diameter of 1.0 mm passes through a square die with a deformation of 12% in the 6th pass, its actual tensile force F6 is greater than the theoretical tensile force F. Therefore, the deformation of the drawing pass C = C5 = 10% is required to prepare a stainless steel orthodontic square wire with a size of 0.019 × 0.025 inch.

[0141] Step S4: Based on the drawing deformation amount B of 40% and the drawing deformation amount C of 10% obtained from steps S1 to S3 above, the stainless steel orthogonal square wire is subjected to a drawing-rolling series processing, including the following steps:

[0142] Step S4.1: Select a stainless steel round wire with an initial infeed diameter of φ = 0.81 mm, and set the target cross-sectional area S of the stainless steel orthogonal square wire to 0.31 mm. 2 The target size of the square die is 0.019 × 0.025 inches. Then, based on the drawing pass deformation amount B being 40% and the drawing pass deformation amount C being 10%, the number of square dies G is determined. It is a rounding function;

[0143] Step S4.2: Drawing is performed in a square die with a deformation of C in the g-th drawing pass, where the value of g is 0 < g ≤ G;

[0144] Step S4.3: Determine whether the edge radius of curvature R of the stainless steel orthogonal square wire is greater than 90μm. If it is true, proceed to step S4.4; if it is not true, proceed to step S4.6.

[0145] Step S4.4: Roll the stainless steel orthogonal square wire using a flat wire rolling mill; the outer surfaces of two relatively moving rolls in the X direction contact the two sides of the stainless steel orthogonal square wire in the width direction, and the outer surfaces of two relatively moving rolls in the Y direction contact the two sides of the stainless steel orthogonal square wire in the height direction; by screwing in or unscrewing the roll pressing amount knob in the X and / or Y directions, control the pressing amount of the rolls in the X and / or Y directions, so that the size of the orthogonal square wire in the width and height directions is further reduced, and the orthogonal square wire is squeezed towards the four edge arc directions, thereby reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process;

[0146] Step S4.5: After rolling, determine whether the edge radius of the stainless steel orthogonal square wire is 70μm≤R≤90μm. If it is true, proceed to step S4.7; if it is not true, proceed to step S4.4.

[0147] Step S4.6: Determine whether the edge radius R of the stainless steel orthodontic square wire conforms to the target edge radius R. 目 The target edge radius R of the stainless steel orthogonal square wire 目 The value is 60±10μm. If this is met, the target size is 0.019×0.025inch, and the target cross-sectional area S is 0.31mm. 2 The stainless steel orthodontic square wire is prepared; if it does not meet the requirements, proceed to step S4.7.

[0148] Step S4.7: In the g+1th drawing pass, the deformation C is 6% in a square die, where the value of g is 0 < g ≤ G; proceed to step S4.3.

[0149] The amount of downward pressure of the rolls in both the X and Y directions shall not exceed 0.05 mm each time.

[0150] By taking steps S1, S2, and S3, the parameters of the stainless steel orthogonal square wire during the manufacturing process can be obtained. Among them, the deformation amount B obtained in the drawing process is the critical cold deformation amount of the stainless steel orthogonal square wire during the drawing process, and the deformation amount C in each drawing pass is the critical drawing force that the stainless steel orthogonal square wire can withstand in each drawing process. Obtaining the deformation amount B in the drawing process and the deformation amount C in each drawing pass can, to the greatest extent possible, determine the optimal number of drawing dies and the drawing force based on the target size of the stainless steel orthogonal square wire.

[0151] Step S4 involves preparing a stainless steel orthodontic square wire based on the parameters measured in steps S1, S2, and S3, to obtain a stainless steel orthodontic square wire that conforms to torque expression. Compared with the torque expression of existing stainless steel orthodontic square wires prepared based on the experience of workers, this invention greatly improves the accuracy of torque expression of stainless steel orthodontic square wires.

[0152] As attached Figure 7 As shown, the edge curvature radii of the 0.019×0.025 inch stainless steel orthodontic square wires are 55μm, 51μm, 52μm, and 58μm, respectively.

[0153] After heat treatment and shaping, the surface of the stainless steel orthodontic square wire will also oxidize, requiring mirror polishing to remove the oxide scale. The mirror polishing process for the stainless steel orthodontic square wire is the same as step S5 in Example 1, and will not be repeated here.

[0154] In the description of this invention, it should be understood that the indicated orientation or positional relationship is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing this invention and simplifying the description, and is not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.

[0155] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A preparation method for improving the expression accuracy of orthodontic wire torque, characterized by: The method includes the following steps: Step S1: Determine the deformation amount of the orthodontic square wire after one drawing pass, and set the deformation amount of the drawing pass as B; Step S2: Determine the initial feed wire diameter of the orthodontic square wire before drawing based on the target cross-sectional area of ​​the orthodontic square wire; Step S3: Determine the deformation amount of the orthodontic square wire in each pull pass, and set the deformation amount of the pull pass as C; Step S4: Perform a series of drawing-rolling processes on the orthogonal square wire based on the deformation amount of the drawing passes and the deformation amount of the drawing passes. Step S4.1: Take a starting round wire with a diameter of φ, and set the width and height dimensions of the square die according to the target cross-sectional area S of the orthogonal square wire. Then, obtain the number of square dies G based on the deformation amount B and the deformation amount C of each drawing pass, i.e., the number of square dies G = = ; It is a rounding function; Step S4.2: Drawing is performed in a square die with a deformation of C in the g-th drawing pass, where the value of g is 0 < g ≤ G; Step S4.3: Determine whether the edge radius of curvature R of the nickel-titanium orthodontic square wire is greater than 110μm, whether the edge radius of curvature R of the TMA orthodontic square wire is greater than 90μm, and whether the edge radius of curvature R of the stainless steel orthodontic square wire is greater than 90μm. If they are true, proceed to step S4.4; if they are not true, proceed to step S4.

6. Step S4.4: Roll the orthogonal square wire using a flat wire rolling mill; Step S4.5: After rolling, determine whether the edge radius of the nickel-titanium orthogonal square wire is 90μm≤R≤110μm, whether the edge radius of the TMA orthogonal square wire is 70μm≤R≤90μm, and whether the edge radius of the stainless steel orthogonal square wire is 70μm≤R≤90μm. If they are true, proceed to step S4.7; if they are not true, proceed to step S4.

4. Step S4.6: judging whether the edge arc radius R of the orthodontic wire meets the target edge arc radius R 目 , if yes, the orthodontic wire preparation is completed; if no, step S4.7 is performed. Step S4.7: Perform drawing in a square die with a deformation of C in the (g+1)th drawing pass, where the value of g is 0 < g ≤ G; proceed to step S4.3; Step S5: Polish the orthodontic square wire to a mirror finish.

2. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 1, characterized in that: When the actual drawing deformation of the orthodontic square wire reaches the drawing deformation amount B, an intermediate annealing is required to eliminate the structural stress of the orthodontic square wire and reduce its hardness. The determination of the drawing deformation amount B of the orthodontic square wire includes the following steps. Step S1.1: Select a standard diameter orthodontic square wire, set N square molds with a deformation amount of 10% for each pass, and match the cross-sectional area S1 of the first square mold with the standard diameter orthodontic square wire. Step S1.2: Pass the standard diameter orthodontic square wire through N square dies in sequence and perform cold deformation drawing until the orthodontic square wire breaks in the nth square die. Calculate the sum of the deformation amount per pass from the first square die to the (n-1)th square die as the limit deformation amount A. The limit deformation amount per pass for breaking the orthodontic square wire is A; the value of n is 0 < n ≤ N. Step S1.3: Set the safety factor to 80%, that is, the deformation amount B of the orthodontic square wire after one drawing heat treatment is A×80%; when the actual drawing deformation amount of the orthodontic square wire reaches the deformation amount B after one drawing heat treatment, perform an intermediate annealing to eliminate the work hardening generated during the drawing deformation of the orthodontic square wire.

3. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 2, characterized in that: Let the target cross-sectional area of ​​the orthodontic square wire be S. Based on the deformation amount B after each drawing pass, the initial feed wire diameter φ of the orthodontic square wire before drawing is obtained as 2 × .

4. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 3, characterized in that: Determining the deformation C of the orthodontic square wire in each drawing pass includes the following steps: Step S3.1: Take the orthodontic square wire in its supplied condition and conduct a tensile test to measure the tensile strength of the orthodontic square wire. A tensile test was conducted on the orthodontic square wire in the solution-treated state to measure its tensile strength. ; The tensile strength of the orthodontic square wire was obtained. ;Right now ; Step S3.2: Take M square molds, design the deformation amount C of the M square molds to increase sequentially with a constant t, and design the cross-sectional area S of the M square molds to decrease sequentially with a constant z. Step S3.3: Set the theoretical tensile force value F when the orthodontic square wire enters the square die for drawing. The theoretical tensile force value F is the cross-sectional area S of the square die and the tensile strength of the orthodontic square wire during the drawing process. The product of, i.e., F = ×S; Insert the initial round wire with a diameter of φ into M square molds, and simultaneously measure the actual tension F when inserting it into the m-th square mold. m Meanwhile, based on the cross-sectional area S of the m-th square mold and its tensile strength... The theoretical tensile force F is obtained when the material is inserted into the m-th square mold; the value of m is in the range of 0 < m ≤ M. Step S3.4: judging whether the actual tensile force value F m is greater than the theoretical tensile force value F, if F m ≤ F, continue to perform the piercing and drawing of the (m+1)th square die; if F m > F, the drawing pass deformation C is C m-1 .

5. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 4, characterized in that: Step S4.4: Rolling the orthogonal square wire using a flat wire rolling mill further includes the following steps: The outer surfaces of two relatively moving rollers in the X direction contact the two sides of the orthogonal square wire in the width direction, and the outer surfaces of two relatively moving rollers in the Y direction contact the two sides of the orthogonal square wire in the height direction. By screwing in or unscrewing the roller pressing amount knob in the X and / or Y directions, the pressing amount of the rollers in the X and / or Y directions is controlled, so that the size of the orthogonal square wire in the width and height directions is further reduced, and the orthogonal square wire is squeezed towards the four edge arc directions, thereby reducing the gradually increasing radius of the four edge arcs generated by the square die drawing process.

6. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 5, characterized in that: The amount of downward pressure of the rolls in both the X and Y directions shall not exceed 0.05 mm each time.

7. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 5, characterized in that: The orthodontic round wire includes a TMA orthodontic round wire, a stainless steel orthodontic round wire, and a nickel-titanium orthodontic round wire; the target edge arc radius R of the TMA orthodontic round wire is 60±10 μm 目 The target edge arc radius R of the stainless steel orthodontic round wire is 60±10 μm 目 The target edge arc radius R of the nickel-titanium orthodontic round wire is 60±10 μm 目 The target edge arc radius R of the nickel-titanium orthodontic round wire is 80±10 μm.

8. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 5, characterized in that: The mirror polishing of the orthodontic square wire includes the following steps: Step S5.1: Place the orthodontic square wire into the placement groove that matches the outline of the orthodontic square wire, then apply water-soluble glue to both ends and the middle of the orthodontic square wire, and attach the orthodontic square wire to the bottom of the placement groove. Step S5.2: Using compressed air as power, select elastic polishing particles and use a programmed nozzle to bombard the orthodontic square wire placed inside the placement groove with polishing particles. At the same time, use the depressurization valve to adjust the speed of the nozzle spraying polishing particles so that the nozzle can reciprocate along the contour of the placement groove; the polishing particles after colliding with the orthodontic square wire are discharged from the leakage hole at the bottom of the placement groove. Step S5.3: After spraying, immerse the placement groove with the orthodontic square wire attached in water to dissolve the water-soluble glue, so that the orthodontic square wire is separated from the placement groove, and blow dry the moisture on the surface of the orthodontic square wire and the placement groove. Step S5.4: Flip the orthodontic wire and repeat steps S5.1, S5.2, and S5.3; Orthodontic square wires with surface oxide scale and scratches removed were obtained.

9. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 8, characterized in that: Surface roughness R of orthodontic round wire after mirror polishing a not more than 0.8 μm.

10. The preparation method for improving the torque expression accuracy of orthodontic square wire according to claim 8, characterized in that: The hardness value of the polishing particles is between 0.2 and 0.5 times the hardness value of the orthodontic square wire.

Citation Information

Patent Citations

  • Parallel wire roller pulling combined forming technology and production equipment thereof

    CN103128127A

  • Preparation method of beta-type titanium alloy dental arch wire

    CN116329306A