Device for manufacturing preform of pole piece, method for manufacturing pole piece, and pole piece
By adjusting the length ratio of the forming channel and the material accumulation zone of the electrode preform preparation device, and combining the embedding part and the cross-shaped structure, the problems of powder falling and extruder blockage in dry preparation were solved, realizing continuous and uniform electrode preparation and improving the strength and toughness of the electrode.
Patent Information
- Application Number
- CN202310473655.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-27
AI Technical Summary
The dry preparation process has problems such as powder falling off easily, uneven feeding, inability to form continuously and damage to the substrate. In addition, the use of lubricant can cause extruder blockage, affecting the uniformity of electrode thickness and quality.
An electrode preform preparation device is used to achieve continuous and uniform extrusion by setting an appropriate ratio between the cross-sectional area of the forming channel and the length of the material accumulation area, combined with the embedding part and the cross-shaped structure, and adjusting the raw material pressure.
A continuous, uniformly thick electrode preform was obtained, which improved the strength and toughness of the electrode and is suitable for the preparation of positive and negative electrodes for lithium-ion batteries, sodium-ion batteries and supercapacitors.
Smart Images

Figure CN118849368B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrode preparation, and more particularly to an apparatus for preparing a preform for preparing an electrode, a method for preparing an electrode using the apparatus for preparing a preform for an electrode, and an electrode prepared by the method thereof. Background Technology
[0002] Currently, common electrode fabrication processes can be divided into dry and wet methods. In the wet method, as described in Patent Document 1, the active material, conductive agent, and emulsion or solution-like binder are first mixed to form a slurry. This slurry is then uniformly coated onto the surface of the current collector. The solvent in the slurry is removed by drying to obtain a dry electrode, and the density of the active material is further increased by rolling. This wet method suffers from problems such as cumbersome processes, toxic solvents, and high and difficult recycling costs. In contrast, in the dry method, the binder and active material (conductive material) are mixed and then calendered to form a self-supporting film. This self-supporting film is then bonded to the current collector to form the electrode. Compared to the wet method, the dry method eliminates coating and drying processes, making it simpler. Furthermore, the dry method is more environmentally friendly by eliminating the use of solvents and the associated slurry coating.
[0003] However, the dry preparation process also presents the following technical problems. If the mixed raw material powder is directly fed into a roller press for rolling, the powder may fall through the roller gaps, resulting in uneven feeding. Furthermore, it cannot be formed into sheets in one step; repeated folding and rolling are required, leading to inconsistent forming and significant performance differences between different batches of electrodes. Additionally, if the powder is placed on a substrate and rolled using a roller press, it may cause damage to the substrate or uneven electrode thickness.
[0004] In response to this, dry manufacturing processes sometimes incorporate a step before or instead of roll forming: forming a preform of the electrode sheet using an extruder. In this extrusion step, as described in Patent Document 2, lubricants and extrusion aids such as calcium stearate or polyethylene wax are typically added. However, a problem arises if the lubricant or extrusion aid is reduced or eliminated to increase the proportion of active material in the raw material, the powdered raw material may become clogged in the extruder and fail to extrude.
[0005] Therefore, in order to solve the above problems, improve the uniformity of electrode thickness, enhance product quality, and obtain high-strength, high-toughness, and continuous electrodes, it is necessary to further explore electrode preparation equipment and processes.
[0006] Existing technology
[0007] Patent documents
[0008] Patent Document 1: CN112072063
[0009] Patent Document 2: CN112420986 Summary of the Invention
[0010] The present invention was made in view of the above-mentioned situation in the prior art, and its object is to provide an apparatus for preparing a preform of an electrode sheet that can obtain a continuous and uniform thickness, an electrode sheet preparation method using the preform preparation apparatus, and an electrode sheet with high strength and high toughness obtained by the method.
[0011] An apparatus for preparing a preform of an electrode sheet according to one aspect of the present invention extrudes electrode sheet raw material into a preform of an electrode sheet, and includes: a barrel having an extrusion channel arranged along the axial direction of the barrel as the extrusion direction; a feed rod disposed inside the barrel, the feed rod conveying the electrode sheet raw material from the feed end side of the barrel to the discharge end side of the barrel and extruding the electrode sheet raw material located at the discharge end side of the barrel; and an extrusion head located at the discharge end side of the barrel, having a forming channel extending through the extrusion head along the extrusion direction, the extrusion channel and the forming channel being connected and connected. An accumulation zone is provided inside the extrusion channel, one end of the accumulation zone overlapping the end face of the feed rod near the extrusion head side in the extrusion direction, and the other end of the accumulation zone overlapping the end face of the extrusion head feed side. The length of the accumulation zone along the extrusion direction is set to l (mm), and the cross-sectional area of the forming channel, viewed along the extrusion direction, is set to S (mm²). 2 If the cross-sectional area S of the forming channel decreases, then the length l of the material accumulation area decreases.
[0012] In the electrode preform preparation apparatus of the present invention, as the electrode raw material is conveyed from the feed end side of the barrel to the discharge end side of the barrel, the feed rod applies pressure to the electrode raw material located in the accumulation zone of the extrusion channel and extrudes it from the forming channel of the extrusion head, thereby obtaining an electrode preform. When the length of the accumulation zone along the extrusion direction increases, the amount of raw material remaining in the accumulation zone increases, and the pressure applied to the raw material in this zone also increases accordingly. Furthermore, when the cross-sectional area S of the forming channel decreases, the pressure applied to the raw material further increases. As a result, when the pressure of the raw material applied to this zone is too high, it may cause the powdery raw material to clog the extrusion head and prevent extrusion. Therefore, in the preform preparation apparatus of the present invention, the following condition is satisfied: as the cross-sectional area S of the forming channel decreases, the length l of the accumulation zone decreases, that is, by appropriately setting the cross-sectional area of the forming channel and the length of the accumulation zone, a continuous electrode preform with uniform thickness can be obtained.
[0013] In the apparatus for preparing the electrode preform of the present invention, the diameter of the accumulation zone can be set to a (mm) when viewed along the extrusion direction, thus satisfying: 0.01≤l / a≤0.8. Therefore, by appropriately setting the aspect ratio of the accumulation zone and appropriately setting the pressure of the raw material applied in the accumulation zone, a continuous electrode preform with uniform thickness can be smoothly extruded.
[0014] In the apparatus for preparing the preform of the electrode sheet according to the present invention, an insert portion may be provided at the feed side end of the extrusion head, which is embedded in the extrusion channel, and the outer diameter of the insert portion is the same as the diameter of the extrusion channel. By providing the insert portion embedded in the extrusion channel, the length of the accumulation zone can be adjusted in a simpler way without changing the structure of the barrel or feed rod, and the pressure of the raw material applied in the accumulation zone can be appropriately set, thereby smoothly extruding a continuous preform of the electrode sheet with uniform thickness.
[0015] In the apparatus for preparing the preform of the electrode sheet of the present invention, the length of the forming channel can be set to h (mm) when viewed along the extrusion direction, which satisfies: 0.01≤l / (l+h)≤0.5.
[0016] In the apparatus for preparing the preform of the electrode sheet according to the present invention, the length of the insert portion along the extrusion direction can be set to m (mm), which satisfies: m ≤ hm. Therefore, by appropriately setting the lengths of the accumulation zone and the forming channel, and appropriately setting the pressure of the raw material applied to the accumulation zone, a continuous, uniformly thick preform of the electrode sheet can be smoothly extruded.
[0017] In the apparatus for preparing the preform of the electrode sheet of the present invention, when viewed along the extrusion direction, the length of the longest axis of the cross section of the forming channel is set to b (mm), which satisfies: 0.5≤b / a≤1.
[0018] In the apparatus for preparing the preform of the electrode sheet according to the present invention, when viewed along the extrusion direction, the length of the longest axis of the cross-section of the forming channel is set to b (mm), and the length of the shortest axis of the cross-section of the forming channel is set to c (mm), thus satisfying: 0.15≤c / b≤1. Therefore, by appropriately setting the cross-sectional area of the forming channel and appropriately setting the pressure of the raw material applied to the accumulation zone, a continuous preform of the electrode sheet with uniform thickness can be smoothly extruded.
[0019] In the apparatus for preparing the preform of the electrode sheet of the present invention, when viewed along the extrusion direction, at least one set of cross-shaped structures is provided at the end of the feed rod near the extrusion head along the extrusion direction. This avoids the surface roughness of the raw material caused by threaded structures of the feed rod, and allows for more uniform mixing of the raw material.
[0020] Another aspect of the electrode preparation method of the present invention includes the following steps: a mixing step, in which an active material, a conductive agent and a binder are mixed as raw materials for the electrode; an extrusion molding step, in which the mixed raw materials for the electrode are extruded and molded using the electrode preform preparation apparatus described above to obtain a continuous preform; a calendering step, in which the preform is calendered to obtain a film; and a composite step, in which the film is composited with a current collector to obtain an electrode.
[0021] In the preparation method of the electrode sheet of the present invention, the mass content of the binder may be 0.5%-5%, and the binder includes at least one of the following: polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polyvinyl chloride (PVC), styrene-butadiene rubber (SBR), polyethylene (PE), polypropylene (PP), ultra-high molecular weight polyethylene (UHMWPE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyamide (PA), polyacrylonitrile (PAN), polyimide (PI), polymethyl methacrylate (PMMA), polyacrylic acid (PAA), nitrile rubber (NBR), polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), and sodium carboxymethyl cellulose (CMC).
[0022] In the preparation method of the electrode of the present invention, the active material may include at least one of the following: lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP), titanium aluminum phosphate (LATP), lithium lanthanum titanate (LLTO), lithium lanthanum zirconium oxide (LLZO), lithium phosphorus oxynitride (LiPON), sulfide solid electrolyte, activated carbon, graphite, soft carbon, hard carbon, graphene, carbon fiber, carbon nanotubes, mesophase microspheres, silicon, silicon dioxide, silicon monoxide, silicon carbide (SiC), lithium titanate, sodium salt of transition metal oxide, and Prussian blue materials.
[0023] In the electrode preparation method of the present invention, the conductive agent may include at least one of conductive carbon black, acetylene black, SuperP, Ketjen black, carbon nanotubes, graphene, and conductive graphite. Therefore, the electrode preparation method of the present invention can be applied to the preparation of positive and negative electrodes and solid electrolyte membranes for common lithium-ion batteries, sodium-ion batteries, and supercapacitors.
[0024] In the preparation method of the electrode sheet of the present invention, a solvent or processing aid may also be added in the mixing step. The solvent or processing aid includes at least one of NMP, ethanol, ethylene glycol, glycerol, isopropanol, n-propanol, water, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, vinylene carbonate, propylene carbonate, ethyl acetate, acetone, polyethylene wax, liquid paraffin, paraffin, calcium stearate, and naphtha.
[0025] In the electrode preparation method of the present invention, the amount of solvent or processing aid added in the mixing step may be less than 80% of the total amount of the mixture including the solvent or processing aid and the raw materials of the electrode.
[0026] In the electrode preparation method of the present invention, the content of solvent or processing aid may be 0. In the electrode preparation method of the present invention, the extrusion of the raw material can be further improved by adding solvent or processing aid. However, it should be understood that, without adding solvent or processing aid, continuous, high-strength, and high-toughness electrode sheets can also be prepared according to the electrode preparation method of the present invention.
[0027] In the electrode preparation method of the present invention, the electrode preform preparation apparatus may be configured such that the feed rod rotates at a speed of 10-150 rpm during the extrusion molding step. Therefore, by appropriately setting the feed rod rotation speed, a high-strength film can be obtained.
[0028] In the electrode preparation method of the present invention, the electrode preform preparation device may be configured such that the extrusion molding temperature is 60°C-200°C during the extrusion molding step.
[0029] Another aspect of the electrode of the present invention is prepared by the apparatus for preparing the preform of the electrode described above.
[0030] Another aspect of the electrode of the present invention is prepared by the electrode preparation method described above.
[0031] Invention Effects
[0032] In the electrode preform preparation apparatus of the present invention, by appropriately setting the cross-sectional area of the forming channel and the length of the material accumulation area, that is, satisfying the relationship that as the cross-sectional area S of the forming channel decreases, the length l of the material accumulation area decreases, a continuous electrode preform with uniform thickness can be obtained. Attached Figure Description
[0033] Figure 1 This is a schematic cross-sectional view of an apparatus for preparing a preform of an electrode sheet according to the present invention.
[0034] Figure 2This schematically illustrates an apparatus for preparing a preform of an electrode sheet according to the present invention, along... Figure 1 A diagram of the cross section of line AA in the diagram.
[0035] Figure 3 This schematically illustrates the cross-shaped structure of the apparatus for preparing the preform of the electrode sheet according to the present invention, along... Figure 1 A diagram of the cross section of the BB line.
[0036] Figure 4 This is a flowchart schematically illustrating the preparation method of the electrode.
[0037] Figure 5 This is a graph showing the tensile strength of a self-supporting diaphragm versus rotational speed.
[0038] Figure 6 These are photographs of an electrode preform prepared by the electrode preform preparation apparatus according to the present invention, and a self-supporting film prepared by the electrode preparation method according to the present invention.
[0039] Figure 7 This is a photograph of a preform of an electrode sheet prepared by the electrode sheet preform preparation apparatus according to the present invention.
[0040] Figure Labels
[0041] apparatus for preparing electrode preforms 1
[0042] Raw material 2 of electrode
[0043] 10 feed cylinders
[0044] Extrusion channel 100
[0045] Material accumulation area 1001
[0046] Feed bar 30
[0047] Cross-shaped structure 301
[0048] Extruder 40
[0049] Molding channel 401
[0050] Embedded part 402 Detailed Implementation
[0051] The following describes the apparatus for preparing the preform of the electrode sheet according to the present invention, the method for preparing the electrode sheet using the apparatus for preparing the preform of the electrode sheet, and the electrode sheet prepared by the method. In the description of the figures, the same or equivalent elements are labeled with the same symbols, and repeated descriptions are sometimes omitted.
[0052] [Apparatus for preparing electrode preforms]
[0053] One aspect of the present invention provides an apparatus for preparing a preform of an electrode by extruding raw material into an electrode. Figure 1 This is a schematic cross-sectional view of an apparatus for preparing a preform of an electrode sheet according to the present invention. Figure 1 In this process, the axial direction of the barrel, i.e., the extrusion direction of the raw material of the electrode, is set as the X direction, the height direction of the barrel is set as the Z direction, and the direction perpendicular to the X and Z directions is set as the Y direction.
[0054] like Figure 1 As shown, the apparatus 1 for preparing the preform of the electrode includes: a barrel 10, a feed rod 30 disposed within the barrel 10, and an extrusion head 40 connected to the barrel 10 by, for example, a threaded connection. The barrel 10 has an extrusion channel 100 along its axial direction, i.e., the extrusion direction (X direction). The feed rod 30 conveys the electrode raw material 2 from the feed end side of the barrel 10 along the extrusion channel 100 to the discharge end side of the barrel 10, and extrudes the electrode raw material located at the discharge end side of the barrel 10. The feed rod 30 is typically a screw and is coaxial with the barrel 10. Thus, by rotating the screw, the electrode raw material located between the threads is conveyed from the feed end to the discharge end of the barrel 10. Furthermore, it should be understood that the feed rod 30 is not limited to a screw structure; it can be used as long as it can convey the electrode raw material 2 from the feed end side to the discharge end side of the barrel 10. An extruder head 40 is located at the discharge end of the barrel 10. A forming channel 401 is provided through the extruder head 40 along the extrusion direction (X direction). The extrusion channel 100 and the forming channel 401 are connected and connected. The extrusion channel 100 and the forming channel 401 are coaxially configured. A material accumulation area 1001 is provided in the extrusion channel 100. In the extrusion direction (X direction), one end of the material accumulation area 1001 overlaps with the end face of the feed rod 30 near the extruder head 40, and the other end of the material accumulation area 1001 overlaps with the end face of the feed side of the extruder head 40.
[0055] like Figure 1 As shown, when the length of the material accumulation area 1001 along the extrusion direction (X direction) is set to l (mm), and the cross-sectional area of the forming channel when viewed along the extrusion direction is set to S (mm²), 2 The following condition is met: as the cross-sectional area S of the forming channel decreases, the length l of the material accumulation area decreases.
[0056] In existing dry manufacturing processes, electrode raw materials include binders such as polytetrafluoroethylene (PTFE). These binders are fibrousized into a network structure, thus binding the substances within the electrode raw material. Increasing the binder content in the raw material improves both the binding of the substances and the ease with which the binder, being an organic polymer, can be extruded. However, from a battery performance perspective, lower binder content results in a higher proportion of active material, increasing the electrode's energy density. However, when the binder content is low, for example, 0.5%-5% by mass, the powdered raw material is mostly inorganic, making it difficult to deform and prone to clogging the extruder. Therefore, improving the extrusion apparatus to smoothly extrude powdered raw materials with less binder into continuous, uniformly thick electrode preforms is crucial.
[0057] The inventors discovered that when the length l of the accumulation zone 1001 along the extrusion direction (X direction) increases, the pressure of the raw material applied to that zone also increases due to the increased amount of raw material remaining in the accumulation zone. Furthermore, when the cross-sectional area S of the forming channel 401 decreases, the pressure of the raw material applied to that zone further increases. Excessive pressure can cause powdery raw material with less binder to clog the extruder head 40, preventing extrusion. Therefore, in the preform preparation apparatus of the present invention, by appropriately setting the cross-sectional area of the forming channel 401 and the length of the accumulation zone 1001, i.e., satisfying the relationship that the length l of the accumulation zone decreases as the cross-sectional area S of the forming channel decreases, excessive pressure applied to the raw material, preventing extrusion, can be avoided, thereby obtaining a continuous preform of electrode sheets with uniform thickness.
[0058] In addition, such as Figure 1 , 2 As shown, when viewed along the extrusion direction (X direction), the diameter of the accumulation zone 1001 is set to a (mm). The electrode preform preparation apparatus 1 of the present invention satisfies: 0.01 ≤ l / a ≤ 0.8. Therefore, by appropriately setting the aspect ratio of the accumulation zone 1001, the pressure of the raw material applied in the accumulation zone 1001 can be appropriately set, and the raw material can be further smoothly extruded into a continuous electrode preform. In addition, in order to further improve the appearance of the extruded electrode preform, that is, to obtain a dense and smooth electrode preform (refer to...), Figure 7 (a) is preferred, 0.08 ≤ l / a ≤ 0.5. Compared to preforms with a bamboo-like texture on the surface (refer to...). Figure 7 (b) A dense and smooth electrode preform is more conducive to obtaining electrodes with uniform thickness in subsequent processes.
[0059] In addition, such as Figure 2 As shown, the forming channel 401 can be designed with different cross-sections according to requirements, thereby obtaining preforms of electrode sheets with different cross-sectional shapes. Specifically, the cross-sectional shape of the forming channel 401 can be as follows: Figure 2 As shown in (a) to (c), the shapes are circular, elliptical, and rounded rectangles, but irregular shapes such as wavy or arc-shaped can also be used. Therefore, the cross-sectional shape and size of the molded body can be freely adjusted simply by changing the extrusion head 40.
[0060] like Figure 2 As shown, the length of the longest axis of the cross-section of the forming channel 401 is set as b (mm), and the length of the shortest axis of the cross-section of the forming channel 401 is set as c (mm). The electrode preform preparation apparatus 1 of the present invention satisfies: 0.5≤b / a≤1, 0.15≤c / b≤1. Therefore, by appropriately setting the cross-sectional area of the forming channel 401, the pressure applied to the raw material can be appropriately set, thereby smoothly extruding a continuous electrode preform with uniform thickness.
[0061] Furthermore, in the electrode preform preparation apparatus 1 of the present invention, an insert portion 402 is provided at the feed side end of the extrusion head 40. The insert portion 402 is embedded within the extrusion channel 100. The outer diameter of the insert portion 402 is equal to the diameter of the extrusion channel 100. In the present invention, "equal" means that, in addition to being completely equal, it can also be equal to values that include minor differences or manufacturing errors within a preset range. For example, when multiple values are all contained within ±5% of the average of the multiple values, the multiple values are defined as equal.
[0062] like Figure 1 As shown, when viewed along the extrusion direction (X direction), if the length of the forming channel 401 is set to h (mm) and the length of the insert 402 along the extrusion direction is set to m (mm), then the electrode preform preparation apparatus 1 of the present invention satisfies: 0.01≤l / (l+h)<0.5, m≤hm.
[0063] As described above, by reducing the length l of the material accumulation area 1001 of the extrusion channel 100, the pressure of the raw material applied to the electrode in the material accumulation area 1001 can be reduced, preventing the raw material from blocking the extrusion port of the extrusion head 40 and facilitating the extrusion of the raw material. To reduce the length l of the material accumulation area 1001, the length of the barrel 10 can be shortened directly or the length of the feed rod 30 can be increased. However, the inventors have discovered that by providing an embedding part 402 embedded in the extrusion channel 100, the effect of shortening the length l of the material accumulation area 1001 can also be achieved. Therefore, when it is necessary to adjust the length of the material accumulation area 1001 to match the change in extrusion conditions caused by the change in the composition of the raw material, the structure of the feed rod 30 and the barrel 10 can be changed without altering them. Instead, only the existing finished extrusion head can be processed. For example, by machining the end of the extrusion head 40 near the barrel 10, an embedding part 402 with an outer diameter equal to the inner diameter of the extrusion channel 100 can be formed, thereby achieving the adjustment of the length l of the material accumulation area 1001 and realizing structural parameter control at a lower cost.
[0064] In addition, such as Figure 1 and Figure 3 As shown, at least one set of feed rods 30 can also be provided at the end near the extruder head 40 along the extrusion direction (X direction). Figure 1 The structure (group 3) has a cross-shaped cross section. Because powdered raw materials tend to leave thread-like residue during feeding via a screw feed rod 30, resulting in an uneven surface, a cross-shaped structure at the end of the feed rod, near the accumulation zone, allows for more uniform mixing of the raw materials, resulting in a smooth surface and uniform thickness of the extruded preform.
[0065] [Preparation methods for electrode sheets]
[0066] Another aspect of the present invention provides a method for preparing an electrode using the above-described electrode preform preparation apparatus 1. For example... Figure 4 As shown, the preparation method of this electrode includes: a mixing step, in which an active material, a conductive agent, and a binder are mixed as raw materials for the electrode; an extrusion molding step, in which the mixed raw materials are extruded using an electrode preform preparation apparatus to obtain a continuous preform; a calendering step, in which the preform is calendered using, for example, a roll press to obtain a film; and a composite step, in which the film is composited with a current collector using, for example, a roll press to obtain the electrode. The film obtained by the roll press in the calendering step can be a self-supporting film capable of maintaining its shape without disintegrating.
[0067] The adhesive has a mass content of 0.5%-5%, and the adhesive includes at least one of the following: polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polyvinyl chloride (PVC), styrene-butadiene rubber (SBR), polyethylene (PE), polypropylene (PP), ultra-high molecular weight polyethylene (UHMWPE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyamide (PA), polyacrylonitrile (PAN), polyimide (PI), polymethyl methacrylate (PMMA), polyacrylic acid (PAA), nitrile rubber (NBR), polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), and sodium carboxymethyl cellulose (CMC).
[0068] The active materials include at least one of the following: lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP), titanium aluminum phosphate (LATP), lithium lanthanum titanate (LLTO), lithium lanthanum zirconium oxide (LLZO), lithium phosphorus oxy nitrogen (LiPON), sulfide solid electrolytes, activated carbon, graphite, soft carbon, hard carbon, graphene, carbon fiber, carbon nanotubes, mesophase microspheres, silicon, silicon dioxide, silicon monoxide, silicon carbide (SiC), lithium titanate, sodium salts of transition metal oxides, and Prussian blue materials.
[0069] The conductive agent includes at least one of the following: conductive carbon black, acetylene black, Super P, Ketjen black, carbon nanotubes, graphene, and conductive graphite. Therefore, the electrode preparation method of the present invention can be applied to the preparation of positive and negative electrodes and solid electrolyte membranes for common lithium-ion batteries, sodium-ion batteries, and supercapacitors.
[0070] In addition, during the mixing step, a solvent or processing aid is added, including at least one of the following: N-methylpyrrolidone (NMP), ethanol, ethylene glycol, glycerol, isopropanol, n-propanol, water, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, vinylene carbonate, propylene carbonate, ethyl acetate, acetone, polyethylene wax, liquid paraffin, paraffin wax, calcium stearate, and naphtha.
[0071] In the mixing step, the amount of solvent or processing aid added is less than 80% of the total mixture including the solvent or processing aid and the electrode raw materials, and the content of solvent or processing aid can also be 0. By adding solvent or processing aid, the extrusion of the raw materials can be improved. However, it should be understood that without adding solvent or processing aid (i.e., when using a dry preparation process), continuous, high-strength, and high-toughness dry-processed electrodes can also be prepared according to the electrode preparation method of the present invention.
[0072] Preferably, in the extrusion molding step, the apparatus for preparing the preform of the electrode sheet is configured such that the feed rod rotates at a speed of 10-150 rpm. (As described later...) Figure 5 As shown, by setting the rotation speed of the feed rod to 10-150 rpm, a high-strength diaphragm with a strength of over 0.9 MPa can be obtained.
[0073] Preferably, in the extrusion molding step, the apparatus for preparing the preform of the electrode sheet is configured such that the extrusion molding temperature is 60℃-200℃. By setting the extrusion conditions, such as the rotation speed of the feed rod and the extrusion molding temperature, it is beneficial to extrude a continuous, uniformly thick, and flat preform of the electrode sheet.
[0074] Another aspect of the present invention provides an electrode prepared using an apparatus for preparing a preform of an electrode as described above and an electrode preparation method as described above.
[0075] It should be noted that the electrode sheet provided by the present invention has the same technical effects as the preparation apparatus for the preform of the electrode sheet and the electrode sheet preparation method described above. To avoid repetition, the implementation method of the electrode sheet will not be described again.
[0076] [Example]
[0077] <Relationship between the structure of the preform preparation device and the extrusion state of the preform>
[0078] The inventors conducted the following experiments to confirm the extrusion state of the preforms of the electrode sheets prepared according to different preform preparation devices, based on two aspects: whether continuous extrusion is possible and the appearance of the extruded preforms.
[0079] Example 1-1
[0080] Prepare Figure 1 The apparatus shown is for preparing a preform of an electrode sheet. The feed rod 30 is a screw with a diameter of 20 mm, a length-to-diameter ratio of 10, a pitch of 20 mm, and a groove depth of 3.8 mm. The diameter 'a' of the accumulation zone is the same as the screw diameter, 20 mm. The length 'l' of the accumulation zone is 10 mm. The cross-sectional shape of the forming channel 401 of the extrusion head 40 is as follows: Figure 2 The circle shown in (a) has an inner diameter of 10 mm. The area S of the forming channel is (3.14*5*5) mm². 2 The length m of the insert 402 is 10mm, and the length h of the molding channel 401 is 40mm.
[0081] Examples 1-2
[0082] The apparatus for preparing the preforms of the electrode sheets in Examples 1-2 is largely the same as that in Example 1, except that the length of the accumulation zone and the cross-sectional shape of the forming channel 401 of the extruder 40 are different. Specifically, the length l of the accumulation zone is 2.5 mm, and the cross-sectional shape of the forming channel 401 of the extruder 40 is... Figure 2 The rounded rectangle shown in (c) has a major axis b of 10mm and a minor axis c of 6mm. The area S of the forming channel is (4*6+3.14*3*3)mm². 2 .
[0083] Examples 1-3
[0084] The apparatus for preparing the electrode preforms in Examples 1-3 is largely the same as that in Example 1, except that the length of the accumulation zone and the cross-sectional shape of the forming channel 401 of the extruder 40 are different. Specifically, the length l of the accumulation zone is 1 mm, and the cross-sectional shape of the forming channel 401 of the extruder 40 is... Figure 2 The rounded rectangle shown in (c) has a major axis b of 10mm and a minor axis c of 4mm. The area S of the forming channel is (6*4+3.14*2*2)mm². 2 .
[0085] Examples 1-4 to 1-8
[0086] The apparatus for preparing the electrode preforms in Examples 1-4 to 1-8 is largely the same as that in Example 1-1, except that the length l of the accumulation zone is different. As described above, the length l of the accumulation zone is changed by changing the length m of the insert 402. That is, in Examples 1-4 to 1-8, the sum of the length m of the insert 402 and the length l of the accumulation zone is kept constant, and m is successively set to 15 mm, 19 mm, 18.4 mm, 19.6 mm, and 4 mm.
[0087] Comparative Example 1-1
[0088] The apparatus for preparing the preform of the electrode sheet in Comparative Example 1-1 is largely the same as that in Example 1-1, except that the length of the accumulation zone and the cross-sectional shape of the forming channel 401 of the extruder 40 are different. Specifically, the length l of the accumulation zone is 0 mm, and the cross-sectional shape of the forming channel 401 of the extruder 40 is... Figure 2 The rounded rectangle shown in (c) has a major axis b of 10mm and a minor axis c of 6mm. The area S of the forming channel is (4*6+3.14*3*3)mm². 2 .
[0089] Comparative Examples 1-2
[0090] The apparatus for preparing the preforms of the electrode sheets in Comparative Examples 1-2 is largely the same as that in Example 1-1, except that the length of the accumulation zone and the cross-sectional shape of the forming channel 401 of the extruder 40 are different. Specifically, the length l of the accumulation zone is 20 mm, and the cross-sectional shape of the forming channel 401 of the extruder 40 is... Figure 2 The rounded rectangle shown in (c) has a major axis b of 10mm and a minor axis c of 6mm. The area S of the forming channel is (4*6+3.14*3*3)mm². 2 .
[0091] <Experimental Evaluation Methods>
[0092] To prepare the preforms of the positive electrode, active material NCM811, conductive agent Super-P, and PTFE dry powder were weighed in a weight ratio of 96.5:1.5:2 and mixed using a high-speed mixer to obtain a mixture. This mixture was slowly added to the preparation apparatus for the preforms of the electrode sheets of Examples 1-1 to 1-8 and Comparative Examples 1-1 to 1-2. The feed rod speed was set to 60 rpm, and the extrusion molding temperature was set to 100°C, resulting in preforms 1-8 and Comparative Example preforms 1-2. The state of the preforms of the electrode sheets extruded from each preparation apparatus was confirmed. The experimental results are shown in Table 1.
[0093] To prepare the preform of the negative electrode sheet, artificial graphite and PTFE dry powder were weighed in a weight ratio of 98:2 and mixed using a high-speed mixer to obtain a mixture. This mixture was slowly added to the electrode sheet preform preparation apparatus of Example 1-1, with the feed rod speed set to 60 rpm and the extrusion molding temperature set to 100°C, to obtain preform 9. The state of the electrode sheet preform 9 extruded from the preparation apparatus was confirmed and is shown in Table 1.
[0094] [Table 1]
[0095]
[0096] By comparing preform 1 with comparative preforms 1 and 2, it can be seen that when the area S of the forming channel decreases, the amount of raw material remaining in the accumulation zone increases, leading to an increase in the pressure applied to the raw material in that zone. At this point, if the length l of the accumulation zone is increased from 10 mm to 20 mm, the pressure applied to the raw material in the accumulation zone becomes excessive, causing the powdery raw material to clog the extruder head and prevent extrusion. If the length of the accumulation zone is reduced to 0 mm (i.e., no accumulation zone is provided), the pressure applied to the raw material is insufficient, and the extrudate remains loose, failing to meet the density requirements of the preform. Furthermore, by comparing preforms 1 to 3, it can be seen that as the cross-sectional area S of the forming channel decreases, when the length l of the accumulation zone is also appropriately reduced, a continuous preform with uniform thickness of electrode sheet can still be obtained.
[0097] As can be seen from the preforms 4 to 8 in Table 1, the electrode preform preparation apparatus 1 according to Examples 1-4 to 1-8 above, by setting the embedding part 402 and appropriately setting the length l of the material accumulation area, can achieve dry continuous extrusion molding of inorganic powder with less binder without adding liquid additives. That is, it can extrude a continuous, high-density, uniformly thick electrode preform of at least 50 cm in a single pass. Using this preform for subsequent processing such as calendering is beneficial for obtaining electrode preforms that meet the requirements for winding and unwinding, have a strength of 1 MPa or more, and good flexibility.
[0098] Furthermore, as can be seen from the preform 9 in Table 1, when the composition of the powder raw material changes, the preform preparation device of the present invention can still obtain a continuous electrode preform with uniform thickness.
[0099] Furthermore, the appearance of the extruded continuous preform was further evaluated.
[0100] Examples 1-9
[0101] Prepare Figure 1 The apparatus shown is for preparing a preform of an electrode sheet. The feed rod 30 is a screw with a diameter of 20 mm, a length-to-diameter ratio of 10, a pitch of 20 mm, and a groove depth of 3.8 mm. The diameter 'a' of the accumulation zone is the same as the screw diameter, 20 mm. The length 'l' of the accumulation zone is 10 mm. The cross-sectional shape of the forming channel 401 of the extrusion head 40 is as follows: Figure 2 The circle shown in (a) has an inner diameter of 10 mm. The area S of the forming channel is (3.14*5*5) mm². 2 The length m of the insert 402 is 5mm, and the length h of the molding channel 401 is 40mm.
[0102] Examples 1-10 to 1-14
[0103] The apparatus for preparing the preforms of the electrode sheets in Examples 1-10 to 1-14 is largely the same as that in Examples 1-9, except that the length l of the accumulation zone is different.
[0104] <Experimental Evaluation Methods>
[0105] To prepare the preforms of the positive electrode, active material NCM811, conductive agent Super-P, and PTFE dry powder were weighed in a weight ratio of 96.5:1.5:2 and mixed using a high-speed mixer to obtain a mixture. This mixture was slowly added to the electrode preform preparation apparatus of Examples 1-9 to 1-14, with the feed rod speed set to 60 rpm and the extrusion molding temperature set to 100°C, yielding preforms 10-15. The state of the electrode preforms extruded from each preparation apparatus was confirmed. The experimental results are shown in Table 2.
[0106] [Table 2]
[0107]
[0108] As shown in Table 2, when 0.08≤l / a≤0.5, the extruded preform is dense and smooth, which helps to obtain electrode sheets with uniform thickness in subsequent processes.
[0109] <Relationship between feed bar speed and diaphragm tensile strength>
[0110] The inventors confirmed the relationship between the feed rod rotation speed of the electrode preform preparation device and the tensile strength of the film through the following experiments. By adjusting the rotation speed of the feed rod 30 of the electrode preform preparation device 1, the degree of fiberization of the binder can be controlled. This is beneficial for the subsequent calendering of the extrudate and obtaining a high-strength film, and also eliminates the need for the mixing equipment used to fiberize the binder in the traditional dry preparation process, thereby simplifying the process.
[0111] Example 2-1
[0112] According to the preparation apparatus and method of Embodiment 1-1 above, a strip-shaped electrode preform (such as...) is obtained. Figure 6 (as shown in (a)). The preform of the electrode was rolled four times using a roller press, with roll gaps set to 800 μm, 500 μm, 300 μm, and 100 μm, respectively, to obtain a self-supporting film with a thickness of 110 μm (as shown in (a)). Figure 6 (as shown in (b)).
[0113] Example 2-2
[0114] In a manner largely similar to Example 2-1, a self-supporting diaphragm was prepared, the only difference being that the feed rod speed was changed to 15 rpm.
[0115] Example 2-3
[0116] In a manner largely similar to Example 2-1, a self-supporting diaphragm was prepared, the only difference being that the feed rod rotation speed was changed to 110 rpm.
[0117] <Experimental Evaluation Methods>
[0118] The prepared membrane was cut into 100*10mm pieces. 2 Rectangular specimens were used for tensile strength testing using a tensile testing machine. The testing speed was 100 mm / min. Five specimens were tested for each sample, and the average value was taken as the test result.
[0119] The experimental results of Examples 2-1, 2-2, and 2-3 are shown in Figure 5 In the chart. From Figure 5 It can be seen that the tensile strength of the diaphragm obtained by Example 2-1 is above 0.9 MPa and has good flexibility, which can meet the requirements of subsequent unwinding and winding of the diaphragm.
[0120] While the present invention has been specifically described above in conjunction with the accompanying drawings and embodiments, it is to be understood that the above description does not limit the invention in any way. Those skilled in the art can make modifications and variations to the present invention as needed without departing from the essential spirit and scope of the invention, and all such modifications and variations fall within the scope of the present invention.
Claims
1. An apparatus for preparing a preform of an electrode sheet, comprising: extruding raw materials of an electrode sheet into a preform of an electrode sheet, and having: The barrel has an extrusion channel arranged along its axial direction, which is the extrusion direction. A feed rod, disposed inside the feed cylinder, conveys the raw material of the electrode sheet from the feed end side of the feed cylinder to the discharge end side of the feed cylinder and extrudes the raw material of the electrode sheet located at the discharge end side of the feed cylinder. An extrusion head, located at the discharge end of the barrel, has a forming channel extending through it along the extrusion direction. The extrusion channel and the forming channel are connected and interlocked. A material accumulation area is provided within the extrusion channel. In the extrusion direction, one end of the material accumulation area overlaps with the end face of the feed rod near the extrusion head, and the other end of the material accumulation area overlaps with the end face of the extrusion head on the feed side. The length of the material accumulation area along the extrusion direction is set as l (mm), and, Let S (mm²) be the cross-sectional area of the forming channel when viewed along the extrusion direction. 2 Then it satisfies: As the cross-sectional area S of the forming channel decreases, the length l of the material accumulation area decreases.
2. The apparatus for preparing the preform of the electrode sheet according to claim 1, wherein, When viewed along the extrusion direction, if the diameter of the accumulation zone is set as a (mm), then the following condition is met: 0.01≤l / a≤0.
8.
3. The apparatus for preparing the preform of the electrode sheet according to claim 1 or 2, wherein, An insert is provided at the feed side end of the extrusion head, which is embedded in the extrusion channel, and the outer diameter of the insert is the same as the diameter of the extrusion channel.
4. The apparatus for preparing the preform of the electrode sheet according to claim 1 or 2, wherein, When viewed along the extrusion direction, if the length of the forming channel is set to h (mm), then the following condition is met: 0.01≤l / (l+h)≤0.
5.
5. The apparatus for preparing the preform of the electrode sheet according to claim 3, wherein, When viewed along the extrusion direction, if the length of the forming channel is set to h (mm), then the following condition is met: 0.01≤l / (l+h)≤0.
5.
6. The apparatus for preparing the preform of the electrode sheet according to claim 5, wherein, If the length of the embedded part along the extrusion direction is set to m (mm), then m ≤ hm.
7. The apparatus for preparing the preform of the electrode sheet according to claim 1 or 2, wherein, When viewed along the extrusion direction, if the length of the longest axis of the cross-section of the forming channel is set as b (mm), then the following condition is satisfied: 0.5≤b / a≤1.
8. The apparatus for preparing the preform of the electrode sheet according to claim 1 or 2, wherein, When viewed along the extrusion direction, if the length of the longest axis of the cross-section of the forming channel is set as b (mm) and the length of the shortest axis of the cross-section of the forming channel is set as c (mm), then the following condition is satisfied: 0.15≤c / b≤1.
9. The apparatus for preparing the preform of the electrode sheet according to claim 1 or 2, wherein, When viewed along the extrusion direction, the end of the feed rod near the extrusion head has at least one set of cross-shaped structures along the extrusion direction.
10. A method for preparing an electrode sheet, comprising the following steps: The mixing step involves mixing active materials, conductive agents, and binders as raw materials for the electrode sheet. The extrusion molding step involves using the electrode preform preparation apparatus according to any one of claims 1 to 9 to extrude the mixed electrode raw materials to obtain a continuous preform. In the calendering step, the preform is calendered to obtain a film, and The composite step involves combining the membrane with the current collector to obtain the electrode.
11. The method for preparing the electrode according to claim 10, wherein, The adhesive has a mass content of 0.5%-5%, and the adhesive includes at least one of the following: polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polyvinyl chloride (PVC), styrene-butadiene rubber (SBR), polyethylene (PE), polypropylene (PP), ultra-high molecular weight polyethylene (UHMWPE), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyamide (PA), polyacrylonitrile (PAN), polyimide (PI), polymethyl methacrylate (PMMA), polyacrylic acid (PAA), nitrile rubber (NBR), polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), and sodium carboxymethyl cellulose (CMC).
12. The method for preparing the electrode according to claim 10 or 11, wherein, The active materials include at least one of the following: lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), lithium manganese iron phosphate (LMFP), titanium aluminum phosphate (LATP), lithium lanthanum titanate (LLTO), lithium lanthanum zirconium oxide (LLZO), lithium phosphorus oxy nitrogen (LiPON), sulfide solid electrolytes, activated carbon, graphite, soft carbon, hard carbon, graphene, carbon fiber, carbon nanotubes, mesophase microspheres, silicon, silicon dioxide, silicon monoxide, silicon carbide (SiC), lithium titanate, sodium salts of transition metal oxides, and Prussian blue materials.
13. The method for preparing the electrode according to claim 10 or 11, wherein, The conductive agent includes at least one of the following: conductive carbon black, acetylene black, Super P, Ketjen black, carbon nanotubes, graphene, and conductive graphite.
14. The method for preparing the electrode according to claim 10 or 11, wherein, In the mixing step, a solvent or processing aid is also added, including at least one of the following: N-methylpyrrolidone (NMP), ethanol, ethylene glycol, glycerol, isopropanol, n-propanol, water, ethylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, vinylene carbonate, propylene carbonate, ethyl acetate, acetone, polyethylene wax, liquid paraffin, paraffin wax, calcium stearate, and naphtha.
15. The method for preparing the electrode according to claim 14, wherein, In the mixing step, the amount of solvent or processing aid added is less than 80% of the total amount of the mixture including the solvent or processing aid and the raw materials of the electrode.
16. The method for preparing the electrode according to claim 14, wherein, The content of the solvent or processing aid is 0.
17. The method for preparing the electrode according to claim 10 or 11, wherein, In the extrusion molding step, the apparatus for preparing the preform of the electrode sheet is configured such that the rotation speed of the feed rod is 10-150 rpm.
18. The method for preparing the electrode according to claim 10 or 11, wherein, In the extrusion molding step, the apparatus for preparing the preform of the electrode sheet is configured such that the extrusion molding temperature is 60℃-200℃.
19. An electrode sheet prepared by an apparatus for preparing a preform of an electrode sheet according to any one of claims 1 to 9.
20. An electrode sheet prepared by the electrode sheet preparation method according to any one of claims 10 to 18.
Citation Information
Patent Citations
e-PTFE plunger extrusion technology
CN106738780A
Extrusion head for pole piece forming, forming device comprising extrusion head and forming method and preparation method of extrusion head