Optical glass and optical element

By adjusting the content and molar ratio of various oxide components, optical glass with low F content and low Gd2O3 content is prepared, which solves the problem that high refractive index and low dispersion optical glass is difficult to achieve in the existing technology, and achieves low-cost, high-performance optical glass. Performance optical glass and production of optical components.

CN118851562APending Publication Date: 2024-10-29HOYA OPTICAL TECH (WEIHAI) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310494726.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult to produce optical glass with high refractive index and low dispersion at low cost with existing technology, especially due to the volatility of F and the rising unit price of Gd2O3, which makes it difficult to control the F content and Gd2O3 content, affecting the performance of the glass.

Method used

By adjusting the component content and molar ratio of SiO2, B2O3, La2O3, Y2O3, ZnO, ZrO2, TiO2, WO3, Bi2O3, Nb2O5, Li2O, Na2O, K2O, MgO, CaO, SrO, BaO and F, an oxidation method was prepared. Optical glass with low F content and low Gd2O3 content in its material-based glass composition, achieving high refractive index and low dispersion.

Benefits of technology

We have successfully provided optical glass with low F content and low Gd2O3 content. It has high refractive index and low dispersion, is suitable for the manufacturing of optical components, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004212218230000141
    Figure BDA0004212218230000141
  • Figure BDA0004212218230000151
    Figure BDA0004212218230000151
  • Figure BDA0004212218230000161
    Figure BDA0004212218230000161
Patent Text Reader

Abstract

The invention relates to optical glass, which comprises the following components in percentage by mole: 0% to 15% (inclusive) of SiO2, 40% to 90% (inclusive) of B2O3, 0% to 5% (inclusive) of ZnO, 5% to 40% (inclusive) of La2O3, 1% to 20% (inclusive) of Y2O3, 0% to 3% (inclusive) of Gd2O3, 0% to less than 1% of Yb2O3 and 0% to 15% (inclusive) of ZrO2 in a glass composition on the basis of oxides, wherein the content of SiO2 is 0% to 15%, the content of B2O3 is 40% to 90%, the content of ZnO is 0% to 5%, the content of La2O3 is 5% to 40%, and the content of Y2O3 is 1% to 20%. The content of TiO2 is from 0% to 2% (inclusive), the content of WO3 is from 0% to 2% (inclusive), the content of Bi2O3 is from 0% to 2% (inclusive), the content of Nb2O5 is from 0% to 2% (inclusive), the total content of Li2O, Na2O and K2O is from 0% to 5% (inclusive), the total content of MgO, CaO, SrO and BaO is from 0% to 5% (inclusive), the molar ratio of the content of B2O3 to the content of Y2O3 is 15 or less, and the molar ratio of the content of B2O3 to the total content of ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 is 15 to 50 (inclusive). The molar ratio of the content of La2O3 to the total content of ZrO2, ZnO, Nb2O5, and TiO2 is 4 or more, and the molar% of the element F excluding the total content of the glass composition on the basis of oxides is 0-3% inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to optical glass and optical elements. Background Art

[0002] In recent years, optical glasses having a high refractive index and low dispersion have been proposed as materials for optical elements (see, for example, Patent Documents 1 and 2).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent document 1: CN102910816A

[0006] Patent Document 2: Japanese Patent Application Laid-Open No. 2002-128539 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] Patent document 1 (CN102910816A) discloses a glass composition containing a large amount of F (fluorine) as a glass composition for achieving high refractive index and low dispersion (see the embodiment of CN102910816A). However, since F is a volatile component, it is not easy to control the refractive index and dispersion (specifically, the Abbe number) of the glass to a desired range due to the volatilization of F for a glass containing a large amount of F. In addition, in order to produce a glass containing a large amount of F, special production equipment is required to prevent the volatilized F from affecting the environment.

[0009] On the other hand, Patent Document 2 (Japanese Patent Publication No. 2002-12853) discloses a glass composition containing a large amount of Gd2O3 as a glass composition for achieving high refractive index and low dispersion (see Examples of Japanese Patent Publication No. 2002-12853). However, since Gd2O3 is an expensive component with a high unit price in recent years, a glass with a low Gd2O3 content is desired for the purpose of reducing the cost of glass.

[0010] In view of the above, an object of one embodiment of the present invention is to provide an optical glass having a low F content and a low Gd2O3 content and having a high refractive index and low dispersion.

[0011] Technical solutions for solving technical problems

[0012] The present inventors have repeatedly conducted intensive studies and have found that by adjusting the contents of various components in the following manner, a high refractive index and low dispersion can be achieved in a glass composition with a low F content and a low Gd2O3 content.

[0013] One embodiment of the present invention is as follows.

[0014] [1] An optical glass comprising, in a glass composition expressed in mol % on an oxide basis,

[0015] The SiO2 content is 0.00% or more and 15.00% or less,

[0016] The B2O3 content is 40.00% or more and 90.00% or less,

[0017] The ZnO content is 0.00% or more and 5.00% or less,

[0018] The La2O3 content is 5.00% or more and 40.00% or less,

[0019] The Y2O3 content is 1.00% or more and 20.00% or less,

[0020] The Gd2O3 content is 0.00% or more and 3.00% or less,

[0021] The Yb2O3 content is 0.00% or more and less than 1.00%,

[0022] The ZrO2 content is 0.00% or more and 15.00% or less,

[0023] The TiO2 content is 0.00% or more and 2.00% or less,

[0024] The WO3 content is 0.00% or more and 2.00% or less,

[0025] The Bi2O3 content is 0.00% or more and 2.00% or less,

[0026] The Nb2O5 content is 0.00% or more and 2.00% or less,

[0027] The total content of Li2O, Na2O and K2O (Li2O+Na2O+K2O) is 0.00% or more and 5.00% or less,

[0028] The total content of MgO, CaO, SrO and BaO (MgO+CaO+SrO+BaO) is 0.00% or more and 5.00% or less,

[0029] The molar ratio of B2O3 to Y2O3 (B2O3 / Y2O3) is 15.00 or less,

[0030] The molar ratio of the B2O3 content to the total content of ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is 15.00 or more and 50.00 or less,

[0031] The molar ratio of La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2 (La2O3 / (ZrO2+ZnO+Nb2O5+TiO2)) is 4.00 or more, and

[0032] The content of the F element expressed as mol% with respect to 100 mol% of the total content of the glass composition based on the oxides (hereinafter also referred to as "F content") is 0.00% to 3.00%.

[0033] [2] The optical glass according to [1], wherein a ZnO content is 0.00% to 2.00%.

[0034] [3] The optical glass according to [1] or [2], wherein a ZnO content is 0.00% to 1.70%.

[0035] [4] The optical glass according to any one of [1] to [3], wherein the Yb2O3 content is 0.00% to 0.20%.

[0036] [5] The optical glass according to any one of [1] to [4], wherein the refractive index nd is 1.73000 or more and 1.77000 or less.

[0037] [6] The optical glass according to any one of [1] to [5], wherein the Abbe number νd is 52.00 or more and 53.00 or less.

[0038] [7] The optical glass according to any one of [1] to [6], wherein the refractive index nd and the Abbe number νd satisfy: nd ≥ 2.20000 - 0.00871*νd.

[0039] [8] The optical glass according to any one of [1] to [7], wherein a value calculated from the refractive index nd and the specific gravity d as (nd-1) / d is 0.173 or more.

[0040] [9] The optical glass according to any one of [1] to [8],

[0041] The ZnO content is 0.00% or more and 1.70% or less,

[0042] The Yb2O3 content is 0.00% or more and 0.20% or less,

[0043] The refractive index nd is greater than or equal to 1.73000 and less than or equal to 1.77000,

[0044] The Abbe number νd is 52.00 or more and 53.00 or less,

[0045] The refractive index nd and the Abbe number νd satisfy:

[0046] nd ≥ 2.20000 - 0.00871 * νd, and

[0047] The value calculated by (nd-1) / d from the refractive index nd and the specific gravity d is 0.173 or more.

[0048]

[10] An optical element comprising the optical glass according to any one of [1] to [9].

[0049] Effects of the Invention

[0050] According to one aspect of the present invention, it is possible to provide an optical glass having a low F content and a low Gd2O3 content and having a high refractive index and low dispersion, and an optical element composed of the optical glass. DETAILED DESCRIPTION

[0051] [Optical glass]

[0052] In the present invention and this specification, the glass composition of the optical glass is expressed as a glass composition based on oxides expressed in mol%. Here, "glass composition based on oxides" refers to a glass composition obtained by conversion assuming that all glass raw materials are decomposed during melting and exist as oxides in the glass. In a glass composition expressed in mol%, the glass composition is expressed on a molar basis (mol%, molar ratio). Hereinafter, with respect to a glass composition expressed in mol%, "mol%" will be referred to as "%".

[0053] In the present invention and this specification, the F content of the optical glass is the content (unit: mol %) expressed as the mol % of the F element relative to 100 mol % of the total content of the glass composition based on the above oxides and calculated as an excluded ratio.

[0054] In the present invention and this specification, the content of a constituent component of 0%, 0.0% or 0.00%, or not contained or not introduced, means that the constituent component is not substantially contained, and means that the content of the constituent component is below the impurity level. Below the impurity level means, for example, less than 0.01%. "0%" can mean, for example, "0.0%" or "0.00%".

[0055] The glass composition in the present invention and this specification can be obtained, for example, by methods such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). For example, quantitative analysis is performed on each element using ICP-AES. Thereafter, the analysis value is converted to an oxide expression. For example, the analysis value of ICP-AES sometimes includes a measurement error of about ±5% of the analysis value. Therefore, the value of the oxide expression converted from the analysis value sometimes also includes an error of about ±5%.

[0056] In the present invention and this specification, the refractive index refers to the refractive index nd at the d-ray (wavelength 587.56 nm) of helium.

[0057] In the present invention and this specification, the Abbe number νd is used as a value indicating a property related to dispersion, and is represented by the following formula.

[0058] νd=(nd-1) / (nF-nC)

[0059] In the above formula, nF is the refractive index of blue hydrogen at F-ray (wavelength 486.13 nm), and nC is the refractive index of red hydrogen at C-ray (656.27 nm).

[0060] Hereinafter, the above-mentioned optical glass (may be simply referred to as "glass") will be described in more detail.

[0061] <Glass composition>

[0062] SiO2 is a glass-forming oxide, and is a component that helps to increase the viscosity of the glass and reduce the tendency of devitrification. In addition, SiO2 is a component that lowers the refractive index, increases vd, decreases the specific gravity, increases the glass transition temperature Tg, and decreases the degree of coloration. The glass transition temperature Tg and the degree of coloration will be explained later. The SiO2 content of the above-mentioned glass is 0.00% or more, and can be 0.00% or more than 0.00%, preferably 0.50% or more, and is more preferably in the order of 1.00 or more, 2.00 or more, 3.00 or more, 4.00 or more, 5.00 or more, 6.00 or more, and 6.50 or more.

[0063] On the other hand, in order to easily obtain homogeneous glass, it is preferred to suppress the deterioration of the solubility of the glass. From this point of view, the SiO2 content of the above-mentioned glass is 15.00% or less, preferably 14.00% or less, and more preferably in the order of 13.00% or less, 12.00% or less, 11.00% or less, 10.00% or less, 9.00% or less, 8.00% or less, and 7.50% or less.

[0064] The B2O3 content of the above-mentioned glass is 40.00% or more. B2O3 is a glass-forming oxide like SiO2. In addition, B2O3 is a component that lowers the refractive index, increases vd, decreases the specific gravity, and lowers the glass transition temperature Tg. By making the B2O3 content 40.00% or more, the devitrification resistance of the glass can be improved, and low dispersion can be easily obtained. The B2O3 content of the above-mentioned optical glass is preferably 45.00% or more, and is more preferably in the order of 50.00% or more, 55.00% or more, 57.00% or more, 59.00% or more, and 61.00% or more.

[0065] On the other hand, B2O3 is a component that is relatively volatile among various glass components. From the viewpoint of suppressing the change of glass composition, the B2O3 content of the above-mentioned glass is 90.00% or less, preferably 85.00% or less, and more preferably in the order of 80.00% or less, 75.00% or less, 72.00% or less, 70.00% or less, 68.00% or less, 66.00% or less, and 64.00% or less.

[0066] The ZnO content of the above-mentioned glass is 0.00% or more, and can be 0.00% or more. ZnO is a component that can increase the refractive index, reduce vd, increase the specific gravity and improve chemical durability. In addition, ZnO is a component that has the effects of lowering the melting temperature, liquidus temperature and glass transition temperature Tg of the glass. From the viewpoint of inhibiting the crystallization of the glass, the ZnO content of the above-mentioned glass is 5.00% or less, preferably 4.50% or less, and more preferably in the order of 4.00% or less, 3.50% or less, 3.00% or less, 2.50% or less, 2.00% or less, 1.70% or less, 1.50% or less, 1.00% or less and 0.50% or less.

[0067] La2O3 is a component that helps to give the glass a high refractive index and low dispersion. The La2O3 content of the above glass is 5.00% or more, preferably 7.50% or more, and more preferably 10.00% or more, 12.50% or more, 15.00% or more, and 17.50% or more in this order.

[0068] On the other hand, from the viewpoint of suppressing devitrification of glass and lowering specific gravity, the La2O3 content of the above-mentioned glass is less than 40.00%, preferably less than 37.50%, and more preferably less than 35.00%, less than 32.50%, less than 30.00%, less than 27.50%, less than 25.00%, and less than 22.50%.

[0069] Y2O3 is a component that helps to give the glass a high refractive index and low dispersion like La2O3. The Y2O3 content of the above glass is 1.00% or more, preferably 2.00% or more, and more preferably 3.00% or more, 4.00% or more, 5.00% or more, and 6.00% or more in this order.

[0070] On the other hand, from the viewpoint of suppressing devitrification of the glass and lowering the specific gravity, the Y2O3 content of the above-mentioned glass is less than 20.00%, preferably less than 18.00%, and more preferably less than 16.00%, less than 14.00%, less than 12.00%, and less than 10.00%.

[0071] The Gd2O3 content of the above-mentioned glass is 0.00% or more, and can be 0.00% or more. Gd2O3 is an arbitrary component that helps to increase the refractive index of the glass and also helps to make the glass low-dispersion, just like La2O3. However, Gd2O3 is a component with a high unit price and a large specific gravity, so when it is contained in the glass, it is preferably contained in as small an amount as possible. The Gd2O3 content of the above-mentioned glass is 3.00% or less, preferably 2.50% or less, and more preferably in the order of 2.00% or less, 1.50% or less, 1.00% or less, and 0.50% or less, and the most preferred is 0.00%.

[0072] The Yb2O3 content of the above-mentioned glass is 0.00% or more, and can be 0.00% or more. Yb2O3 is an arbitrary component that contributes to the high refractive index and low dispersion of the glass. Yb2O3 is a particularly expensive raw material among rare earth raw materials, so it is preferred that the Yb2O3 content is low. The Yb2O3 content of the above-mentioned glass is less than 1.00%, preferably less than 0.50%, more preferably less than 0.20%, further preferably less than 0.10%, and most preferably 0.00%.

[0073] The molar ratio of B2O3 to Y2O3 in the glass (B2O3 / Y2O3) is 15.00 or less, preferably 14.00 or less, and more preferably 13.00 or less, 12.00 or less, 11.00 or less, 10.00 or less, and 9.00 or less in this order. The molar ratio (B2O3 / Y2O3) may be, for example, more than 0.00, 1.00 or more, 2.00 or more, 3.00 or more, 4.00 or more, 5.00 or more, or 6.00 or more.

[0074] The ZrO2 content of the above-mentioned glass is 0.00% or more, and may be 0.00% or more. ZrO2 is a component that helps to improve the chemical durability of the glass and increase the refractive index. The ZrO2 content of the above-mentioned glass is preferably 0.40% or more, and more preferably in the order of 0.80% or more, 1.20% or more, 1.60% or more, and 2.00% or more.

[0075] On the other hand, from the viewpoint of achieving the desired low dispersion and low specific gravity, the ZrO2 content of the above-mentioned glass is less than 15.00%, preferably less than 13.00%, and more preferably less than 11.00%, less than 9.00%, less than 7.00%, less than 5.00%, and less than 3.00%.

[0076] In the above glass, the contents of TiO2, WO3 and Bi2O3 are each greater than 0.00%, and may be 0.00% or greater.

[0077] TiO2, WO3 and Bi2O3 are components that help to give glass a high refractive index and low dispersion. By making the respective contents below 2.00%, the decrease in the transmittance of the glass with respect to ultraviolet to visible light (especially wavelengths below 500nm) can be suppressed. From this point of view, the respective contents of TiO2, WO3 and Bi2O3 are below 2.00%, preferably below 1.50%, more preferably below 1.00%, further preferably below 0.50%, and most preferably 0.00%.

[0078] The Nb2O5 content of the above glass is 0.00% or more, and may be 0.00% or more. Nb2O5 is a component that helps to impart high refractive index and low dispersion to the glass.

[0079] On the other hand, Nb2O5 is a component that has a high raw material unit price, increases the specific gravity of the glass, and affects the transmittance of the glass to ultraviolet light to visible light. Considering the above points, the Nb2O5 content of the above glass is 2.00% or less, preferably 1.50% or less, more preferably 1.00% or less, further preferably 0.50% or less, and most preferably 0.00%.

[0080] ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 are all components that contribute to imparting high refractive index and low dispersion to the glass. Adjusting the molar ratio of the B2O3 content to the total content of these components contributes to achieving high refractive index and low dispersion in a glass composition with low F content and Gd2O3 content. Regarding the molar ratio of the B2O3 content of the above-mentioned glass to the total content of ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3 (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)), if the value of this molar ratio is small, the refractive index nd of the glass increases and the Abbe number νd becomes low, and if the value of this molar ratio is large, the refractive index nd of the glass decreases and the Abbe number νd becomes high. From the viewpoint of achieving high refractive index and low dispersion, the molar ratio of the above-mentioned glass (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is greater than 15.00 and less than 50.00. The molar ratio (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is preferably greater than 16.00, and more preferably in the order of greater than 17.00, greater than 18.00, greater than 19.00, greater than 20.00, and greater than 21.00. In addition, the molar ratio (B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3)) is preferably less than 45.00, and more preferably in the order of less than 40.00, less than 35.00, less than 30.00, and less than 25.00.

[0081] La2O3, ZrO2, ZnO, Nb2O5 and TiO2 are all components that contribute to the high refractive index of glass, but ZrO2, ZnO, Nb2O5 and TiO2 contribute less to the low dispersion of glass than La2O3. Adjusting the molar ratio of La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2 helps to achieve high refractive index and low dispersion in glass compositions with low F content and Gd2O3 content. From the viewpoint of achieving high refractive index and low dispersion, the molar ratio of La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2 in the above optical glass (La2O3 / (ZrO2+ZnO+Nb2O5+TiO2)) is 4.00 or more, preferably 4.50 or more, and more preferably 5.00 or more, 5.50 or more, 6.00 or more, 6.50 or more, and 7.00 or more in this order. The molar ratio (La2O3 / (ZrO2+ZnO+Nb2O5+TiO2)) can be, for example, 20.00 or less, 19.00 or less, 18.00 or less, 17.00 or less, or 16.00 or less.

[0082] The total content of Li2O, Na2O and K2O (Li2O+Na2O+K2O) of the glass is 0.00% or more and 5.00% or less. The total content (Li2O+Na2O+K2O) may be 0.00% or more.

[0083] As for alkali metal oxides, Rb2O and Cs2O are expensive components and are not suitable for general-purpose glass compared with Li2O, Na2O and K2O. From the viewpoint of maintaining the thermal stability, chemical durability, weather resistance and machinability of the glass and improving the meltability of the glass, lowering the glass transition temperature Tg and lowering the specific gravity of the glass, the total content of Li2O, Na2O and K2O in the above-mentioned glass (Li2O+Na2O+K2O) is 0.00% or more and 5.00% or less. The total content (Li2O+Na2O+K2O) is preferably 4.00% or less, and more preferably 3.00% or less, 2.00% or less and 1.00% or less in this order.

[0084] The Li2O content is 0.00% or more, and may be 0.00% or more. From the viewpoint of further improving the thermal stability of the glass, suppressing the decrease in the glass transition temperature (thereby improving the machinability), improving chemical durability and weather resistance, the Li2O content is preferably 5.00% or less, and more preferably 4.00% or less, 3.00% or less, and 2.00% or less in this order.

[0085] The content of each of Na2O, K2O, Rb2O and Cs2O is 0.00% or more, and may be 0.00% or more. Na2O, K2O, Rb2O and Cs2O all have the effect of improving the melting property of glass, but if their content increases, the thermal stability, chemical durability, weather resistance and machinability of glass tend to decrease. Therefore, the content of each of Na2O, K2O, Rb2O and Cs2O is preferably 5.00% or less, and more preferably 4.00% or less, 3.00% or less, and 2.00% or less in this order.

[0086] The total content of MgO, CaO, SrO and BaO (MgO+CaO+SrO+BaO) of the above-mentioned glass is 0.00% or more, and can be 0.00% or more. Alkaline earth metal oxides facilitate the melting of glass raw materials and are therefore components that help to produce homogeneous glass. From the viewpoint of achieving devitrification suppression and desired optical properties of the glass, the total content of the above-mentioned glass (MgO+CaO+SrO+BaO) is 5.00% or less, preferably 4.00% or less, and more preferably 3.00% or less, 2.00% or less, and 1.00% or less in that order.

[0087] The content of each of MgO, CaO, SrO and BaO is 0.00% or more, and may be 0.00% or more. From the viewpoint of achieving devitrification suppression of glass and desired optical properties, the content of each of MgO, CaO, SrO and BaO is preferably 5.00% or less, more preferably 4.00% or less, and more preferably 3.00% or less, 2.00% or less, and 1.00% or less in this order.

[0088] F is a component that makes the glass less dispersive, and is also a component that can improve melting properties and lower the glass transition temperature Tg by adding a small amount. However, glass containing a large amount of F is not preferred for the reasons previously described. Therefore, in the above-mentioned glass, the content (F content) calculated as an excluded ratio expressed by the mole % of the F element relative to the total content of the glass composition based on the oxide is 100 mol %, which is expressed as the mole % of the F element is greater than 0.00% and less than 3.00%. The F content can be 0.00% or more than 0.00%. The F content is preferably less than 2.50%, and is more preferably less than 2.00%, less than 1.50%, less than 1.00%, and less than 0.50% in this order, and the most preferred is 0.00%.

[0089] Regarding other glass components, considering environmental impact, the As2O3 content is preferably 0.10% or less, more preferably 0.01% or less, and most preferably 0.00%. Also, considering environmental impact, the PbO content is preferably 1.00% or less, more preferably 0.50% or less, 0.10% or less, and most preferably 0.00%.

[0090] Ta2O5 is an expensive component. From the viewpoint of reducing the cost of glass, the Ta2O5 content is preferably 2.00% or less, more preferably 1.50% or less, 1.00% or less, 0.50% or less, and most preferably 0.00%.

[0091] Sb2O3 is a component that can be added as a clarifier. By adding a small amount, it can also play a role in suppressing the decrease in light transmittance caused by the mixing of impurities such as Fe, but if the amount of Sb2O3 added is increased, the coloring of the glass tends to increase. Therefore, the amount of Sb2O3 added is preferably 0.00% or more and 0.10% or less, more preferably 0.00% or more and 0.08% or less, and further preferably 0.00% or more and 0.05% or less. The Sb2O3 content calculated by the exclusion ratio refers to the Sb2O3 content expressed in mass % when the sum of the contents of glass components other than Sb2O3 is set to 100 mass %.

[0092] SnO2 can also be added as a clarifier, but if it is added in an amount exceeding 1.00% in the exclusion ratio, the glass will be colored or Sn will become the starting point of nucleation when the glass is heated, softened, and re-formed by press forming, resulting in a tendency to devitrification. Therefore, it is preferred that the amount of SnO2 added be 0.00% or more and 1.00% or less in the exclusion ratio, more preferably 0.00% or more and 0.50% or less, and particularly preferably not added. The SnO2 content calculated in the exclusion ratio refers to the content of SnO2 expressed in mass % when the sum of the contents of the glass components other than SnO2 is set to 100 mass %.

[0093] <Glass Physical Properties>

[0094] (Refractive index nd)

[0095] The glass may be a high refractive index glass by having the glass composition. From the viewpoint of usefulness as a material for optical elements, the refractive index nd of the glass is preferably 1.73000 or more, more preferably 1.74000 or more, and further preferably 1.75000 or more. In addition, from the viewpoint of usefulness as a material for optical elements, the refractive index nd of the glass may be 1.77000 or less, preferably 1.76000 or less.

[0096] (Abbe number νd)

[0097] The glass can exhibit low dispersion by having the glass composition. From the viewpoint of usefulness as a material for an optical element, the Abbe number νd of the glass is preferably 52.00 or more and 53.00 or less.

[0098] The glass having the glass composition can satisfy the following formula 1. From the viewpoint of usefulness as a material for an optical element, an optical glass whose refractive index nd and Abbe number νd satisfy the following formula 1 is preferred.

[0099] Formula 1: nd ≥ 2.20000 - 0.00871 * νd

[0100] (proportion)

[0101] In the optical element constituting the optical system, the refractive power is determined by the refractive index of the glass constituting the optical element and the curvature of the optical functional surface (the surface where the light incident and emitted to be controlled) of the optical element. If the curvature of the optical functional surface is to be increased, the thickness of the optical element is also increased. As a result, the optical element becomes heavier. In contrast, if a glass with a high refractive index is used, a large refractive power can be obtained even without increasing the curvature of the optical functional surface.

[0102] In summary, if the increase in the specific gravity of glass can be suppressed and the refractive index can be increased, it is possible to achieve a reduction in the weight of an optical element having a certain refractive power.

[0103] From the above viewpoints, the specific gravity of the above-mentioned glass is preferably below 4.50, and is more preferably in the order of below 4.40 and below 4.30. The lower the specific gravity, the more preferably it is from the viewpoint of lightweighting of optical elements. Therefore, for the specific gravity of the above-mentioned optical glass, the lower limit is not particularly limited. In one embodiment, the specific gravity can be above 3.50, above 3.75 or above 4.00. In the present invention and this specification, "specific gravity" is a value measured by the Archimedean method.

[0104] In addition, from the above viewpoints, the value calculated by (nd-1) / d based on the refractive index nd and specific gravity d of the above glass is preferably 0.173 or more, and more preferably in the order of 0.174 or more, 0.175 or more, 0.176 or more, 0.177 or more, and 0.178 or more. In addition, the value calculated by (nd-1) / d can be, for example, 0.200 or less or 0.190 or less.

[0105] (Coloring degree λ5, λ 80 )

[0106] The light transmittance of the glass (specifically, the light absorption end on the short wavelength side is suppressed from becoming longer wavelength) can be improved by adjusting the coloring degree λ5 and λ 80 The coloration degree λ5 represents the wavelength at which the spectral transmittance (including surface reflection loss) of glass with a thickness of 10±0.1 mm from the ultraviolet region to the visible region is 5%. 80 λ5 indicates the wavelength at which the spectral transmittance is 80% as measured by the method described for λ5. 80 It is a value measured in the wavelength range of 250 to 700 nm. For a glass sample having two parallel planes after optical polishing, the intensity of light perpendicularly incident on one of the planes is defined as I in , the intensity of the light emitted from the other side through the glass sample is set to I out When the spectral transmittance T(%) of the glass in the present invention and this specification is T(%)=I out / I in ×100 indicates.

[0107] According to the coloring degree λ5 and λ 80, the absorption end on the short wavelength side of the spectral transmittance can be quantitatively evaluated. For example, when lenses are bonded together using an ultraviolet curing adhesive to produce a bonded lens, ultraviolet rays are irradiated to the adhesive through the optical element to cure the adhesive. From the perspective of efficiently curing the ultraviolet curing adhesive, the absorption end on the short wavelength side of the spectral transmittance is preferably in the short wavelength region. As an indicator for quantitatively evaluating the absorption end on the short wavelength side, the coloring degrees λ5 and λ 80 More than one.

[0108] The glass preferably exhibits a λ5 of 300 nm or less. λ5 is more preferably 295 nm or less, 290 nm or less, and 285 nm or less in that order. Regarding λ5, the shorter the wavelength, the more preferred it is, and its lower limit is not particularly limited.

[0109] The optical glass can exhibit a λ of 550 nm or less or 500 nm or less, for example. 80 , preferably capable of presenting a λ below 400nm 80 . 80 The order of 395 nm or less, 390 nm or less, 385 nm or less, and 380 nm or less is more preferred. 80 The shorter the wavelength, the more preferred it is, and its lower limit is not particularly limited.

[0110] (Glass transition temperature Tg)

[0111] From the viewpoint of reducing the burden on the annealing furnace and the forming mold, the glass transition temperature Tg of the glass is preferably 750°C or less, and more preferably 745°C or less, 740°C or less, 735°C or less, 730°C or less, and 725°C or less in the order of being more preferably. On the other hand, from the viewpoint of machinability (specifically, the viewpoint that the glass is not easily broken during mechanical processing such as cutting, cutting, grinding, and polishing), the glass transition temperature Tg of the glass is preferably 600°C or more, more preferably 620°C or more, and further preferably 640°C or more. The glass transition temperature Tg is obtained by using a differential scanning calorimeter with a heating rate of 10°C / min.

[0112] <Method for manufacturing optical glass>

[0113] The optical glass can be obtained by weighing and blending raw materials such as oxides, carbonates, sulfates, nitrates, hydroxides, etc. in a manner to obtain the desired glass composition, fully mixing to obtain a mixed masterbatch, heating and melting in a melting container, degassing and stirring to produce a homogeneous and bubble-free molten glass, and shaping it. Specifically, it can be manufactured using a known melting method.

[0114] [Glass material for press molding, optical element blank, and method for producing the same]

[0115] Another embodiment of the present invention relates to:

[0116] A glass material for press molding composed of the above optical glass;

[0117] An optical element blank composed of the above optical glass.

[0118] According to another embodiment of the present invention, it is also possible to provide:

[0119] A method for producing a press-molding glass material, comprising the step of molding the optical glass into a press-molding glass material;

[0120] A method for manufacturing an optical element blank comprising the step of making an optical element blank by press-molding the above-mentioned optical glass press-molding glass material using a press-molding die;

[0121] A method for producing an optical element blank comprising the step of forming the optical glass into an optical element blank.

[0122] The optical element blank is an optical element base material that is similar in shape to the intended optical element, with a grinding allowance (surface layer removed by grinding) added to the shape of the optical element and a grinding allowance (surface layer removed by grinding) added as needed. The optical element is finished by grinding and polishing the surface of the optical element blank. In one embodiment, the optical element blank can be made by a method (also referred to as a direct pressing method) of pressing and forming molten glass obtained by melting the above-mentioned glass in an appropriate amount. In another embodiment, the optical element blank can also be made by solidifying the molten glass obtained by melting the above-mentioned glass in an appropriate amount.

[0123] Furthermore, in another aspect, an optical element blank can be produced by producing a press-molding glass material and press-molding the produced press-molding glass material.

[0124] The press forming of the press forming glass material can be performed by a known method of pressing the press forming glass material in a heated and softened state using a press forming mold. Both heating and press forming can be performed in the atmosphere. By annealing after press forming to reduce the strain inside the glass, a homogeneous optical element blank can be obtained.

[0125] In addition to materials called press-forming glass gobs supplied in their original state to press-forming for manufacturing optical element blanks, press-forming glass materials also include materials that are subjected to mechanical processing such as cutting, grinding, and polishing and are used for press-forming through press-forming glass gobs. As cutting methods, there are methods such as forming grooves in the portion to be cut on the surface of the glass plate by a method called scribing, applying local pressure to the groove portion from the back of the surface where the groove is formed, and cracking the glass plate at the groove portion, and cutting the glass plate with a cutting knife. In addition, as grinding and polishing methods, drum polishing and the like can be cited.

[0126] The press-forming glass material can be produced, for example, by pouring molten glass into a casting mold to form a glass plate and cutting the glass plate into a plurality of glass sheets. Alternatively, a press-forming glass drop can be produced by forming an appropriate amount of molten glass. The press-forming glass drop can be produced by reheating, softening, and press-forming the glass drop to produce an optical element blank. The method of reheating, softening, and press-forming the glass to produce an optical element blank is called a reheat pressing method in contrast to the direct pressing method.

[0127] [Optical element and method of manufacturing the same]

[0128] Another aspect of the present invention relates to an optical element composed of the above optical glass.

[0129] The optical element is made of the optical glass. In the optical element, one or more layers of coating such as a multilayer film such as an antireflection film may be formed on the glass surface.

[0130] According to one aspect of the present invention, there can be provided a method for producing an optical element, comprising the step of producing an optical element by grinding and / or polishing the optical element blank.

[0131] In the manufacturing method of the optical element, mechanical processing such as grinding and lapping can be performed by known methods. By fully cleaning and drying the surface of the optical element after processing, an optical element with high internal quality and surface quality can be obtained. In this way, an optical element composed of the optical glass can be obtained. As the optical element, various lenses such as spherical lenses, aspherical lenses, micro lenses, prisms, etc. can be exemplified.

[0132] Furthermore, the optical element composed of the above optical glass is also suitable as a lens constituting a joined optical element. As the joined optical element, an element obtained by joining lenses to each other (joined lens), an element obtained by joining a lens and a prism, etc. can be exemplified. For example, the joined optical element can be produced in the following manner: the joining surfaces of the two joined optical elements are precisely processed in a manner to have an inverted shape (for example, spherical grinding), and a UV-curable adhesive used in the bonding of the joined lenses is applied, and after pasting, ultraviolet rays are irradiated through the lens to cure the adhesive. In order to produce the joined optical element in this way, the above optical glass is preferred. By separately producing and joining the multiple optical elements to be joined using a plurality of glasses with different Abbe numbers νd, an element suitable for correcting chromatic aberration can be formed.

[0133] Example

[0134] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the embodiments shown in the examples.

[0135] [Example 1]

[0136] <Examples No. 1 to 57>

[0137] As raw materials for introducing each component, corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acid, etc. were used respectively so as to obtain the glass composition (unit: mol %) shown in the following table, and the raw materials were weighed and sufficiently mixed to form a blending raw material.

[0138] The blended raw materials were placed in a platinum crucible, heated and melted in a furnace set at 1350°C for two hours. After the molten glass was stirred and homogenized, it was poured into a preheated mold, cooled to near the glass transition temperature, and then directly placed in an annealing furnace. After being kept at a temperature around the glass transition temperature for about 30 minutes, it was gradually cooled at a gradual cooling rate of -30°C / hour for 4 hours, and then cooled in the furnace to room temperature, thereby obtaining the optical glasses No. 1 to 57 shown in the table below. None of these optical glasses contain F. The Sb2O3 content shown in the table below is the content calculated based on the exclusion ratio (unit: mass %).

[0139] The physical properties of the optical glass obtained in this way are shown in the following table.

[0140] The physical properties of the optical glass were measured by the methods shown below.

[0141] <Evaluation of physical properties of optical glass>

[0142] (1) Refractive index nd and Abbe number νd

[0143] The refractive index nd and the Abbe number νd of the obtained glass were measured by the refractive index measurement method according to the standards of the Japan Optical Glass Industries Association.

[0144] (2) Glass transition temperature Tg

[0145] Glass was fully pulverized in a mortar as a sample, and the glass transition temperature Tg was measured by a differential scanning calorimeter (DSC8271) manufactured by Rigaku Corporation using a platinum cell as a sample container at a heating rate of 10°C / min.

[0146] (3) Specific gravity

[0147] The specific gravity was measured using the Archimedean method.

[0148] (4) Coloring degree λ5, λ 80

[0149] The spectral transmittance T (%) was measured using a spectrophotometer using a glass sample with two optically polished flat surfaces facing each other and having a thickness of 10 ± 0.1 mm. The wavelength (nm) at which T is 5% is λ5, and the wavelength (nm) at which T is 80% is λ. 80 .

[0150]

[0151]

[0152]

[0153] [Example 2]

[0154] The various glasses obtained in Example 1 were used to prepare glass blocks (glass droplets) for press molding. The glass blocks were heated and softened in the atmosphere, and then press molded using a press mold to prepare lens blanks (optical element blanks). The prepared lens blanks were taken out of the press mold and annealed, and mechanical processing including grinding was performed to prepare spherical lenses composed of the various glasses prepared in Example 1.

[0155] [Example 3]

[0156] The molten glass prepared in Example 1 was pressed into a desired amount using a press-forming mold to prepare a lens blank (optical element blank). The prepared lens blank was taken out of the press-forming mold and annealed, and mechanical processing including grinding was performed to prepare a spherical lens composed of the various glasses prepared in Example 1.

[0157] [Example 4]

[0158] A glass block (optical element blank) produced by solidifying the molten glass produced in Example 1 was annealed and subjected to mechanical processing including grinding, thereby producing a spherical lens composed of the various glasses produced in Example 1.

[0159] [Example 5]

[0160] The spherical lens produced in Examples 2 to 4 is pasted with a spherical lens made of other types of glass to produce a joined lens. The joining surface of the spherical lens produced in Examples 2 to 4 is a convex surface, and the joining surface of the spherical lens made of other types of glass is a concave surface. The two joining surfaces are produced in such a way that the absolute values ​​of the radii of curvature are equal to each other. An ultraviolet curing adhesive for joining optical elements is applied to the joining surface, and the two lenses are pasted to each other using the joining surfaces. Thereafter, the adhesive applied to the joining surface is irradiated with ultraviolet rays through the spherical lens produced in Examples 2 to 4 to cure the adhesive.

[0161] The cemented lens was produced in the above manner. The cemented lens had a sufficiently high bonding strength and a sufficient optical performance.

[0162] The embodiments disclosed this time should be considered as illustrative and non-restrictive descriptions in all aspects. The scope of the present invention is indicated by the claims rather than the above description, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0163] For example, by adjusting the composition of the glass composition exemplified above as described in the specification, the optical glass according to one embodiment of the present invention can be obtained.

[0164] In addition, it is apparent that any combination of two or more items described as examples or as preferred ranges in the specification can be performed.

Claims

1. An optical glass, wherein, in a glass composition expressed in mol % on an oxide basis, The SiO2 content is 0.00% or more and 15.00% or less, The B2O3 content is 40.00% or more and 90.00% or less, The ZnO content is 0.00% or more and 5.00% or less, The La2O3 content is 5.00% or more and 40.00% or less, The Y2O3 content is 1.00% or more and 20.00% or less, The Gd2O3 content is 0.00% or more and 3.00% or less, The Yb2O3 content is 0.00% or more and less than 1.00%, The ZrO2 content is 0.00% or more and 15.00% or less, The TiO2 content is 0.00% or more and 2.00% or less, The WO3 content is 0.00% or more and 2.00% or less, The Bi2O3 content is 0.00% or more and 2.00% or less, The Nb2O5 content is 0.00% or more and 2.00% or less, The total content of Li2O, Na2O and K2O, i.e. Li2O+Na2O+K2O, is 0.00% or more and 5.00% or less, The total content of MgO, CaO, SrO and BaO, i.e., MgO+CaO+SrO+BaO, is 0.00% or more and 5.00% or less, The molar ratio of B2O3 to Y2O3, i.e., B2O3 / Y2O3, is 15.00 or less. The molar ratio of the B2O3 content to the total content of ZrO2, ZnO, Nb2O5, TiO2, WO3 and Bi2O3, i.e., B2O3 / (ZrO2+ZnO+Nb2O5+TiO2+WO3+Bi2O3), is 15.00 or more and 50.00 or less, The molar ratio of La2O3 content to the total content of ZrO2, ZnO, Nb2O5 and TiO2, i.e., La2O3 / (ZrO2+ZnO+Nb2O5+TiO2), is 4.00 or more, and The content of the F element expressed as mol% with respect to 100 mol% of the total content of the glass composition based on the oxides is calculated as an excluded ratio of 0.00% to 3.00%.

2. The optical glass according to claim 1, The ZnO content is 0.00% or more and 2.00% or less.

3. The optical glass according to claim 1, The ZnO content is 0.00% or more and 1.70% or less.

4. The optical glass according to claim 1, The Yb2O3 content is greater than or equal to 0.00% and less than or equal to 0.20%.

5. The optical glass according to claim 1, The refractive index nd is greater than or equal to 1.73000 and less than or equal to 1.77000.

6. The optical glass according to claim 1, The Abbe number νd is 52.00 or more and 53.00 or less.

7. The optical glass according to claim 1, The refractive index nd and the Abbe number νd satisfy: nd≥2.20000-0.00871*νd.

8. The optical glass according to claim 1, The value calculated by (nd-1) / d from the refractive index nd and the specific gravity d is 0.173 or more.

9. The optical glass according to claim 1, The ZnO content is 0.00% or more and 1.70% or less, The Yb2O3 content is 0.00% or more and 0.20% or less, The refractive index nd is greater than or equal to 1.73000 and less than or equal to 1.77000, The Abbe number νd is 52.0 or more and 53.0 or less, The refractive index nd and the Abbe number νd satisfy: nd ≥ 2.20000 - 0.00871 * νd, and The value calculated by (nd-1) / d from the refractive index nd and the specific gravity d is 0.173 or more. 10 . An optical element, comprising the optical glass according to claim 1 .