Ultraviolet-curable coating composition
By using a solvent-free UV-curable coating composition containing oligomers with specific functional groups and ceramic beads, the problems of odor and viscosity increase during application of existing coating compositions are solved, resulting in a coating film with excellent iodine resistance, stain resistance, adhesion and scratch resistance, thereby improving the surface hardness and appearance of flooring materials.
Patent Information
- Application Number
- CN202410490109.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-23
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-23
AI Technical Summary
Existing coating compositions produce odors and increase viscosity during application, leading to decreased iodine resistance, stain resistance, adhesion, and gloss of the coating film, as well as insufficient surface hardness of the flooring material.
A solvent-free, UV-curable coating composition is used, comprising 9-functional urethane (meth)acrylate oligomers, 6-functional urethane (meth)acrylate oligomers, 3 or more functional (meth)acrylate monomers, 2-functional (meth)acrylate monomers, ceramic beads, and a photoinitiator, to adjust the drying speed and surface tension of the coating film and form an excellent coating film.
It forms a coating film with excellent iodine resistance, stain resistance, adhesion and scratch resistance, solves the problems of odor and increased viscosity, and improves the surface hardness and appearance characteristics of flooring materials.
Smart Images

Figure BDA0004805103680000121 
Figure BDA0004805103680000131 
Figure BDA0004805103680000132
Abstract
Description
Technical Field
[0001] This invention relates to a UV-curable coating composition with excellent iodine resistance and scratch resistance. Background Technology
[0002] After installation, flooring materials are exposed to external environments prone to discoloration or contamination. Therefore, to prevent this and improve appearance, a coating is typically formed on the surface of the flooring material. In the case of the most widely used PVC flooring material, techniques are employed to ensure the scratch resistance and stain resistance of the flooring material by coating the surface with thermosetting resins or waxes. As an example, Korean Patent Publication No. 10-1335571 discloses a polyurethane coating composition for waterproof flooring materials containing carbon nanotubes.
[0003] However, floor materials treated with existing coating compositions suffer from insufficient surface hardness. Furthermore, existing coating compositions using solvents experience increased viscosity during application, leading to reduced iodine resistance, stain resistance, and adhesion of the coating film, while increasing gloss. Additionally, they generate odors due to volatile organic compounds (VOCs). Summary of the Invention
[0004] (The problem the invention aims to solve)
[0005] This invention provides a solvent-free, UV-curable coating composition that solves the problems of odor and viscosity increase during application, and can form a coating film with excellent iodine resistance, stain resistance, adhesion, gloss, and scratch resistance.
[0006] (The measures taken to solve the problem)
[0007] The present invention provides an ultraviolet-curable coating composition comprising a 9-functional urethane (meth)acrylate oligomer, a 6-functional urethane (meth)acrylate oligomer, a (meth)acrylate monomer with more than 3 functional groups, a (meth)acrylate monomer with 2 functional groups and an alkoxylated (meth)acrylate monomer with more than 2 functional groups, ceramic beads, and a photoinitiator.
[0008] (The effect of the invention)
[0009] The coating composition of the present invention exhibits excellent iodine resistance and can form a coating film with excellent stain resistance, adhesion, gloss, and scratch resistance. Furthermore, the coating composition of the present invention is a solvent-free coating, which solves the problems of existing solvent-based coatings generating odors and volatile organic compounds and increasing viscosity during coating operations. The coating composition of the present invention can be used as a coating for the surface of flooring materials (e.g., PVC flooring materials). Detailed Implementation
[0010] The present invention will now be described in detail. However, the present invention is not limited to the following description, and the constituent elements may be used in various modifications or selective combinations as needed. Therefore, it should be understood that all modifications, equivalents, or substitutions included within the concept and scope of the present invention are applicable.
[0011] The term "weight average molecular weight" as used in this specification is determined by conventional methods known in the art, such as gel permeation chromatography (GPC). "Viscosity" is determined by conventional methods known in the art, such as using a Brookfield viscometer at room temperature (25°C). Functional group values, such as "acid value," are determined by conventional methods known in the art, such as titration. "Particle size (D50)" is determined by conventional methods known in the art, such as using a laser particle size analyzer.
[0012] The UV-curable coating composition of the present invention comprises: a 9-functional group urethane(meth)acrylate oligomer, a 6-functional group urethane(meth)acrylate oligomer, a (meth)acrylate monomer with 3 or more functional groups, a (meth)acrylate monomer with 2 functional groups, an alkoxylated (meth)acrylate monomer with 2 or more functional groups, a ceramic bead, and a photoinitiator. In this invention, when using 9-functional urethane (meth)acrylate oligomers with a weight-average molecular weight of 4,000 to 7,000 g / mol, 6-functional urethane (meth)acrylate oligomers with a weight-average molecular weight of 1,000 to 3,000 g / mol, and ceramic beads with an average particle size (D50) of 7 to 13 μm, the dispersibility of the ceramic beads in the coating composition becomes excellent, and the drying speed and surface tension of the coating film are adjusted so that the ceramic beads are uniformly coated on the coating film surface. As a result, a coating film with excellent scratch resistance and appearance properties can be formed.
[0013] As needed, the coating composition of the present invention may further include additives such as adhesion promoters, dispersants, surface conditioners, polymerization inhibitors, and matting agents commonly used in the field of UV-curable coatings.
[0014] 9-functional group urethane (meth)acrylate oligomers
[0015] The UV-curable coating composition of the present invention comprises a 9-functional urethane (meth)acrylate oligomer. The 9-functional urethane (meth)acrylate oligomer is the main component of the dried coating film, which can improve scratch resistance, iodine resistance, adhesion, etc.
[0016] The aforementioned 9-functional urethane (meth)acrylate oligomers can be 9-functional aliphatic urethane (meth)acrylate oligomers. Using 9-functional aliphatic urethane (meth)acrylate oligomers increases the hardness and curing density of the coating film, thereby further improving iodine resistance and scratch resistance, and ensuring excellent physical properties of the coating, such as preventing yellowing.
[0017] The weight-average molecular weight (Mw) of the aforementioned 9-functional urethane (meth)acrylate oligomers can be from 4,000 to 7,000 g / mol, for example, from 5,000 to 6,000 g / mol. When the weight-average molecular weight of the aforementioned 9-functional urethane (meth)acrylate oligomers is within the range described above, the compatibility with ceramic beads is excellent and the crosslinking density of the coating film is increased, thereby improving scratch resistance, appearance, and adhesion. When the weight-average molecular weight of the aforementioned 9-functional urethane (meth)acrylate oligomers is less than the range described above, the viscosity is too low, resulting in reduced iodine resistance and gloss of the coating film. When it exceeds the range described above, the crosslinking density increases significantly, leading to a decrease in the elasticity of the coating film, thereby reducing iodine resistance, stain resistance, and scratch resistance.
[0018] The viscosity (25°C) of the aforementioned 9-functional urethane (meth)acrylate oligomer can be from 70,000 to 90,000 cps, for example, from 75,000 to 85,000 cps. When the viscosity of the aforementioned 9-functional urethane (meth)acrylate oligomer is within the range described above, workability is excellent, thereby improving appearance and adhesion. When the viscosity of the aforementioned 9-functional urethane (meth)acrylate oligomer is less than the range described above, due to the excessively low viscosity, a coating film cannot be formed, or the adhesion and iodine resistance of the coating film will decrease. When the viscosity exceeds the range described above, the workability of the coating deteriorates, thereby reducing the appearance of the coating film.
[0019] As needed, the above-mentioned 9-functional urethane (meth)acrylate oligomers can also be used in combination with reactive oligomers (e.g., polyester (meth)acrylate oligomers). In this case, the curing properties, moisture resistance, thermal cycling resistance, and heat resistance of the coating film are improved, and the leveling property, workability, adhesion, and flexibility of the coating composition are further improved.
[0020] The content of the aforementioned 9-functional urethane (meth)acrylate oligomer, based on the total weight of the coating composition, can be 10 to 30% by weight, for example, 15 to 25% by weight. When the content of the aforementioned 9-functional urethane (meth)acrylate oligomer is within the range described above, maintaining an appropriate crosslinking density can improve the curability, moisture resistance, iodine resistance, scratch resistance, etc., of the coating film. When the content of the aforementioned 9-functional urethane (meth)acrylate oligomer is less than the range described above, the crosslinking density decreases due to the low viscosity, resulting in reduced heat resistance and adhesion. When it exceeds the range described above, the workability deteriorates due to the high viscosity of the composition, thus reducing the appearance of the coating film.
[0021] 6-functional carbamate (meth)acrylate oligomers
[0022] The UV-curable coating composition of the present invention comprises a hexafunctional urethane (meth)acrylate oligomer. The hexafunctional urethane (meth)acrylate oligomer is the main component of the dried coating film, which can improve scratch resistance, iodine resistance, etc. In particular, in the present invention, a high-functionality urethane (meth)acrylate oligomer, which is a mixture of hexafunctional and non-functional urethane (meth)acrylate oligomers, is used, thereby increasing the hardness and curing density of the coating film, and thus further improving iodine resistance and scratch resistance.
[0023] The aforementioned hexafunctional urethane (meth)acrylate oligomers can be hexafunctional aromatic urethane (meth)acrylate oligomers. When using hexafunctional aromatic urethane (meth)acrylate oligomers, excellent compatibility with ceramic beads and increased crosslinking density of the coating film are achieved, thereby improving scratch resistance, appearance, and adhesion.
[0024] The weight-average molecular weight (Mw) of the aforementioned hexafunctional urethane (meth)acrylate oligomers can be from 1,000 to 3,000 g / mol, for example, from 1,500 to 2,000 g / mol. When the weight-average molecular weight of the aforementioned hexafunctional urethane (meth)acrylate oligomers is within the range described above, the compatibility with ceramic beads is excellent and the crosslinking density of the coating film is increased, thereby improving scratch resistance, appearance, and adhesion. When the weight-average molecular weight of the aforementioned hexafunctional urethane (meth)acrylate oligomers is less than the range described above, the viscosity is too low, resulting in reduced iodine resistance and gloss of the coating film. When it exceeds the range described above, the crosslinking density increases significantly, leading to a decrease in the elasticity of the coating film, thereby reducing iodine resistance, stain resistance, and scratch resistance.
[0025] The viscosity (at 25°C) of the aforementioned hexafunctional urethane (meth)acrylate oligomers can be from 20,000 to 50,000 cps, for example, from 30,000 to 40,000 cps. When the viscosity of the aforementioned hexafunctional urethane (meth)acrylate oligomers is within the range described above, workability is excellent, thereby improving appearance and adhesion. When the viscosity of the aforementioned hexafunctional urethane (meth)acrylate oligomers is less than the range described above, due to the excessively low viscosity, a coating film cannot be formed, or the adhesion and iodine resistance of the coating film will decrease. When the viscosity exceeds the range described above, the workability of the coating deteriorates, thereby reducing the appearance of the coating film.
[0026] As needed, the above-mentioned hexafunctional urethane (meth)acrylate oligomers can also be used in combination with reactive oligomers (e.g., polyester (meth)acrylate oligomers). In this case, the curability, moisture resistance, thermal cycling resistance, and heat resistance of the coating film are improved, and the leveling properties, workability, adhesion, and flexibility of the coating composition are further enhanced.
[0027] The content of the aforementioned hexafunctional urethane (meth)acrylate oligomers, based on the total weight of the coating composition, can be 5 to 15% by weight, for example, 7 to 13% by weight. When the content of the aforementioned hexafunctional urethane (meth)acrylate oligomers is within the range described above, maintaining an appropriate crosslinking density can improve the curability, moisture resistance, iodine resistance, and scratch resistance of the coating film. When the content of the aforementioned hexafunctional urethane (meth)acrylate oligomers is less than the range described above, the crosslinking density decreases due to the low viscosity, resulting in reduced heat resistance and adhesion. When the content exceeds the range described above, the workability deteriorates due to the high viscosity of the composition, leading to a decline in the appearance of the coating film.
[0028] As an example, the aforementioned 9-functional urethane (meth)acrylate oligomer and the aforementioned 6-functional (meth)acrylate oligomer can be mixed in a weight ratio of 1:0.2 to 1, for example, a weight ratio of 1:0.3 to 0.8. When the oligomers are used in the aforementioned ratio, curing properties and crosslinking density are improved, thereby improving the coating's iodine resistance, scratch resistance, stain resistance, adhesion, and other physical properties. Furthermore, excellent compatibility with ceramic beads further enhances scratch resistance.
[0029] (meth)acrylate monomers
[0030] The UV-curable coating composition of the present invention comprises (meth)acrylate monomers. The (meth)acrylate monomers are auxiliary components for drying the coating film, improving the flowability, leveling, and workability of the coating composition, and enhancing the iodine resistance, scratch resistance, and adhesion of the coating film. In particular, the (meth)acrylate monomers replace solvents to increase the hardness and cured density of the coating film, and can solve the problems of increased viscosity and the generation of VOCs (volatile organic compounds) and odors during application.
[0031] The aforementioned (meth)acrylate monomers comprise (meth)acrylate monomers with three or more functional groups, (meth)acrylate monomers with two functional groups, and alkoxylated (meth)acrylate monomers with two or more functional groups. The UV-curable coating composition of the present invention uses a mixture of three monomers with different functional groups, thereby providing improved stain resistance and scratch resistance due to increased crosslinking density of the coating film.
[0032] (Meth)acrylate monomers with 3 or more functional groups
[0033] (Meth)acrylate monomers with 3 or more functional groups are (meth)acrylate monomers having 3 or more polymerizable functional groups, for example, 3 to 6 as polymerizable unsaturated groups. As another example, (meth)acrylate monomers with 3 or more functional groups are (meth)acrylate monomers having 3 or 4 polymerizable unsaturated groups, which play a role in improving the scratch resistance of the coating film and reducing the shrinkage of the coating film.
[0034] Non-limiting examples of the aforementioned (meth)acrylate monomers with three or more functional groups include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and other trifunctional (meth)acrylate monomers; tetrafunctional (meth)acrylate monomers such as pentaerythritol tetra(meth)acrylate and ditrimethylolpropane tetra(meth)acrylate; and dipentaerythritol poly(meth)acrylate, etc., which can be used alone or in mixtures of two or more. As an example, the aforementioned (meth)acrylate monomers with three or more functional groups can be trifunctional (meth)acrylate monomers, for example, trimethylolpropane tri(meth)acrylate.
[0035] The molecular weight of the (meth)acrylate monomers with three or more functional groups can be from 100 to 500 g / mol, for example, from 200 to 400 g / mol. When the molecular weight of the (meth)acrylate monomers with three or more functional groups is within the range described above, the crosslinking density of the coating composition increases, thereby improving stain resistance, gloss, and adhesion. When the molecular weight of the (meth)acrylate monomers with three or more functional groups is less than the range described above, the crosslinking efficiency and intermolecular bonding force decrease, thereby reducing iodine resistance and heat resistance. When the molecular weight exceeds the range described above, the curing reaction slows down, thereby reducing adhesion.
[0036] The viscosity (at 25°C) of the aforementioned (meth)acrylate monomers with three or more functional groups can be from 800 to 2,000 cps, for example, from 1,000 to 1,800 cps. Maintaining an appropriate viscosity for the coating composition when the viscosity of the (meth)acrylate monomers with three or more functional groups is within the aforementioned range improves appearance, gloss, workability, and adhesion. When the viscosity of the (meth)acrylate monomers with three or more functional groups is less than the aforementioned range, the coating film cannot be formed due to excessively low viscosity, or the adhesion and heat resistance of the coating film will decrease. When the viscosity exceeds the aforementioned range, the workability of the coating deteriorates, resulting in a decline in appearance.
[0037] The content of the aforementioned (meth)acrylate monomers with three or more functional groups can be 2 to 15% by weight, for example, 5 to 10% by weight, based on the total amount of the coating composition. When the content of the aforementioned (meth)acrylate monomers with three or more functional groups is within the range described above, the crosslinking density of the coating composition increases, thereby improving stain resistance, gloss, and adhesion. When the content of the aforementioned (meth)acrylate monomers with three or more functional groups is less than the range described above, the crosslinking density decreases due to the low viscosity, thereby reducing the degree of crosslinking, adhesion, and scratch resistance. When the content exceeds the range described above, the viscosity becomes too high, resulting in reduced film flexibility, thereby decreasing gloss and appearance.
[0038] 2-functional group (meth)acrylate monomer
[0039] The 2-functional (meth)acrylate monomer is used in combination with the above-mentioned 3-functional or higher (meth)acrylate monomers to replace solvents and improve coating shrinkage.
[0040] The aforementioned difunctional (meth)acrylate monomers can be, for example, alkylene glycol dimethacrylate monomers such as hexanediol dimethacrylate, polyethylene glycol dimethacrylate, glycerine dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, dipropylene glycol dimethacrylate, tripropylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, etc. As an example, the aforementioned difunctional (meth)acrylate monomer can be tripropylene glycol dimethacrylate.
[0041] The molecular weight of the aforementioned difunctional (meth)acrylate monomer can be from 100 to 400 g / mol, for example, from 150 to 350 g / mol. When the molecular weight of the aforementioned difunctional (meth)acrylate monomer is within the range described above, the crosslinking density of the coating composition increases, thereby improving stain resistance, gloss, and adhesion. When the molecular weight of the difunctional (meth)acrylate monomer is less than the range described above, the crosslinking efficiency decreases, thereby reducing iodine resistance and appearance. When it exceeds the range described above, the crosslinking density increases significantly, leading to a decrease in the elasticity of the coating film, thereby reducing appearance, adhesion, and heat resistance.
[0042] The viscosity (at 25°C) of the aforementioned difunctional (meth)acrylate monomer can be from 1 to 30 cps, for example, from 5 to 15 cps. Maintaining an appropriate viscosity for the coating composition when the viscosity of the difunctional (meth)acrylate monomer is within the aforementioned range improves appearance, gloss, workability, and adhesion. When the viscosity of the difunctional (meth)acrylate monomer is less than the aforementioned range, the heat resistance of the coating film decreases due to the excessively low viscosity; when it exceeds the aforementioned range, the workability of the coating deteriorates, resulting in a decline in appearance.
[0043] The content of the aforementioned difunctional (meth)acrylate monomers, based on the total amount of the coating composition, can be 20 to 35% by weight, for example, 25 to 30% by weight. When the content of the aforementioned difunctional (meth)acrylate monomers is within the range described above, the crosslinking density of the coating composition increases, thereby improving stain resistance, gloss, and adhesion. When the content of the difunctional (meth)acrylate monomers is less than the range described above, the viscosity of the coating composition increases, thereby reducing flowability and leveling properties. When it exceeds the range described above, the viscosity of the composition is very low, and the curing properties decrease, thereby reducing workability and adhesion.
[0044] Alkoxylated (meth)acrylate monomers with two or more functional groups
[0045] Alkoxylated (meth)acrylate monomers with two or more functional groups are polymerizable alkoxylated (meth)acrylate monomers having two or more polymerizable functional groups, for example, two to five unsaturated groups that are polymerizable. The alkoxylated (meth)acrylate monomers with two or more functional groups are used in combination with the aforementioned (meth)acrylate monomers with three or more functional groups and (meth)acrylate monomers with two functional groups to replace solvents and improve the hardness, curing density and iodine resistance of the coating film.
[0046] In the above-mentioned alkoxylated (meth)acrylate monomers with two or more functional groups, the alkoxy group can be, for example, an alkoxy group having 1 to 5 carbon atoms, or, as another example, an alkoxy group having 2 or 3 carbon atoms.
[0047] The aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups can be, for example, monomers of ethoxylated polypropylene glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, ethoxylated glycerine tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, etc. As an example, the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups can be ethoxylated bisphenol A dimethacrylate (BPA(EO)2DMA).
[0048] The molecular weight of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups can be from 300 to 600 g / mol, for example, from 350 to 550 g / mol. When the molecular weight of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups is within the range described above, the crosslinking density of the coating composition increases, thereby improving stain resistance, gloss, and adhesion. When the molecular weight of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups is less than the range described above, the heat resistance and cold / heat resistance of the coating film decrease due to the low viscosity. When it exceeds the range described above, the crosslinking density increases, leading to a decrease in the elasticity of the coating film, thereby reducing appearance, adhesion, and heat resistance.
[0049] The viscosity (at 25°C) of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups can be from 800 to 1,600 cps, for example, from 1,000 to 1,400 cps. When the viscosity of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups is within the range described above, maintaining an appropriate viscosity of the coating composition can improve appearance, gloss, workability, and adhesion. When the viscosity of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups is less than the range described above, due to the low viscosity, a coating film cannot be formed, or the iodine resistance and stain resistance of the coating film will decrease. When the viscosity exceeds the range described above, the workability of the coating deteriorates, thereby reducing gloss and adhesion.
[0050] The content of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups can be from 0.5% to 10% by weight, for example, from 2% to 8% by weight, based on the total amount of the coating composition. When the content of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups is within the range described above, the crosslinking density of the coating composition increases, thereby improving stain resistance, gloss, and adhesion. When the content of the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups is less than the range described above, curability and crosslinking density decrease, thereby reducing the strength and adhesion of the coating film. When it exceeds the range described above, the viscosity becomes too high, leading to reduced workability and iodine resistance.
[0051] As an example, the aforementioned (meth)acrylate monomers with three or more functional groups, the aforementioned (meth)acrylate monomers with two or more functional groups, and the aforementioned alkoxylated (meth)acrylate monomers with two or more functional groups can be mixed in a weight ratio of 1:1 to 5:0.1 to 1.5, for example, in a weight ratio of 1:3 to 4:0.4 to 0.8. When the monomers are used in the aforementioned mixing ratios, appropriate viscosity is maintained and curability is improved, thereby improving the physical properties of the coating film, such as iodine resistance, scratch resistance, stain resistance, and adhesion, and further improving the viscosity adjustment and odor reduction effects during operation.
[0052] Ceramic beads
[0053] The UV-curable coating composition of the present invention comprises spherical ceramic beads. The ceramic beads further enhance the scratch resistance of the coating film.
[0054] The ceramic beads mentioned above can be alkali aluminosilicate ceramic beads, zirconia ceramic beads, alumina ceramic beads, etc. For example, the ceramic beads mentioned above can be alkali aluminosilicate ceramic beads.
[0055] When amorphous ceramic beads are used as the aforementioned ceramic beads, the ceramic beads protrude from the coating surface, resulting in a decrease in the appearance and gloss of the coating, and a reduction in the hardness and scratch resistance of the formed coating. Conversely, when spherical ceramic beads are used and the coating is formed with a thickness equal to the average particle size of the aforementioned ceramic beads, the appearance and gloss of the coating are not reduced due to increased impact resistance, thereby improving the scratch resistance of the coating.
[0056] The average particle size (D50) of the aforementioned ceramic beads can be 7 to 13 μm, for example, 9 to 11 μm. When the average particle size of the ceramic beads is within the range described above, the compatibility with urethane (meth)acrylate oligomers increases, thereby improving scratch resistance and adhesion. When the average particle size of the ceramic beads is smaller than the range described above, the low porosity reduces the binding with oligomers and monomers, resulting in decreased scratch resistance and appearance. When the average particle size exceeds the range described above, the high porosity leads to a decrease in appearance and an excessive increase in surface roughness, resulting in decreased adhesion and stain resistance.
[0057] The content of the ceramic beads can be 1 to 8% by weight, for example, 2 to 6% by weight, based on the total weight of the coating composition. When the content of the ceramic beads is within the range described above, the compatibility with the urethane (meth)acrylate oligomer increases, thereby improving scratch resistance and adhesion. When the content of the ceramic beads is less than the range described above, the crosslinking density with the urethane (meth)acrylate oligomer is low, thus reducing stain resistance and scratch resistance during film formation. When the content exceeds the range described above, the reaction with the coating composition leads to reduced storability and workability.
[0058] Photoinitiator
[0059] The UV-curable coating composition of the present invention comprises a spherical photoinitiator. A photoinitiator is a component that initiates photopolymerization upon excitation by ultraviolet (UV) light or the like; if it is a photoinitiator well-known in the art, it can be used without limitation.
[0060] Non-limiting examples of photoinitiators that can be used include MICURE BP, JRCURE MBF, Irgacure 184, Irgacure 369, Irgacure 651, Irgacure 819, Irgacure 907, Benzionalkylether, Benzophenone, Benzyl dimethylkatal, Hydroxycyclohexyl phenylacetone, Chloroacetophenone, 1,1-Dichloroacetophenone, Diethoxyacetophenone, and Hydroxyacetophenone. Acetophenone, 2-chlorothioxanthone, 2-ethylanthraquinone (2-ETAQ), 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, methylbenzoylformate, Bis(2,4,6-trimethylbenzoyl)phenylphosphine (e.g., oxide), 2-hydroxy-2-methyl-1-phenylpropane-1-one, etc. They can be used alone or in combination of two or more.
[0061] As for the maximum absorption wavelength of the aforementioned photoinitiator, it is not particularly limited as long as it can absorb ultraviolet light; for example, it can be in the range of 200 to 410 nm.
[0062] As an example, the aforementioned photoinitiator may comprise a first photoinitiator with a melting point of 40 to 55°C, for example, 47 to 49°C, and a second photoinitiator with a melting point of 65 to 80°C, for example, 70 to 75°C. In the case of comprising the two photoinitiators described above, the coating strength and adhesion can be further improved due to proper curing with the ceramic beads.
[0063] The content of the aforementioned photoinitiator, based on the total amount of the coating composition, can be from 0.1 to 10% by weight, for example, from 1 to 8% by weight. As an example, based on the total amount of the coating composition, it may contain 0.1 to 4% by weight, for example, 1 to 3% by weight of the aforementioned first photoinitiator, and 0.1 to 6% by weight, for example, 2 to 5% by weight of the aforementioned second photoinitiator. When the content of the aforementioned photoinitiator is less than the range described above, reduced curability or lack of curing will lead to decreased coating film strength and adhesion, and wrinkles will occur due to the lack of curing. On the other hand, when the content of the aforementioned photoinitiator exceeds the range described above, contamination or low polymerization degree caused by unreacted photoinitiators will lead to reduced adhesion.
[0064] additive
[0065] In addition to the components described above, the coating compositions according to the present invention may selectively further include additives commonly used in the art, depending on the intended use and environment of the coating composition. As an example, the coating compositions of the present invention may further include additives such as adhesion promoters, dispersants, surface conditioners, polymerization inhibitors, and matting agents, as needed.
[0066] As the aforementioned adhesion promoter, adhesion promoters known in the art can be used without particular limitation, such as acid esters, polyester resins, and mixtures thereof. As an example, an acid ester with an acid value of 120 to 180 mg KOH / g and a specific gravity of 110 to 120 can be used. As another example, a polyester resin with a viscosity (23°C) of 9,000 cps and a solids content of 50% can be used.
[0067] As the aforementioned dispersant, dispersants known in the art can be used without particular limitation. For example, a pigment wetting and dispersing agent and a dispersing agent that functions as both a wetting and dispersing agent can be used in combination.
[0068] As the aforementioned surface conditioner, surface conditioners known in the art can be used without particular limitation; for example, a mixture of slip agents, defoamers, and release agents can be used. As an example, silicone acrylates can be used.
[0069] The aforementioned matting agents serve to adjust the viscosity and gloss of the coating composition, and there are no particular limitations as long as they are known in the art. For example, silica can be used.
[0070] The content of each of the above additives is not particularly limited; for example, it can be from 0.01 to 20% by weight based on the total amount of the coating composition.
[0071] There are no particular limitations on the preparation method of the coating composition of the present invention. For example, the coating composition of the present invention can be prepared by adding the aforementioned 9-functional urethane (meth)acrylate oligomer, 6-functional urethane (meth)acrylate oligomer, 3 or more functional (meth)acrylate monomers, 2-functional (meth)acrylate monomers, 2 or more functional alkoxylated (meth)acrylate monomers, ceramic beads, and photoinitiator, along with additives as needed, to a mixing device such as a dissolver or mixer, and then mixing at an appropriate temperature (e.g., room temperature) using conventional methods.
[0072] The UV-curable coating composition of the present invention is applicable to a variety of substrates, and is useful for surface treatment of PVC flooring materials, but is not limited thereto. According to one example, the UV-curable coating composition of the present invention, after being applied to the surface of a substrate and dried, can achieve a curing efficiency of less than 3,000 mJ / cm². 2 For example, 2,500 mJ / cm 2 Below (e.g., 1,500 to 2,500 mJ / cm) 2 It is cured under ultraviolet radiation to form a coating layer.
[0073] The present invention will now be described in more detail through embodiments. However, the embodiments described below are merely illustrative of the invention and are not intended to limit the scope of the invention in any way to the embodiments.
[0074] [Examples 1-19]
[0075] The UV-curable coating compositions of each embodiment were prepared according to the compositions described in Tables 1 and 2 below.
[0076] [Comparative Examples 1-12]
[0077] UV-curable coating compositions for each comparative example were prepared according to the compositions described in Table 3 below.
[0078] [Table 1]
[0079]
[0080]
[0081] [Table 2]
[0082]
[0083]
[0084] [Table 3]
[0085]
[0086]
[0087] A-1: 9-functional urethane acrylate oligomer (Mw: 5,570 g / mol, viscosity (25°C): 80,500 cps)
[0088] A-2: 9-functional urethane acrylate oligomer (Mw: 4,130 g / mol, viscosity (25°C): 72,000 cps)
[0089] A-3: 9-functional urethane acrylate oligomer (Mw: 6,730 g / mol, viscosity (25°C): 87,100 cps)
[0090] A-4: 9-functional urethane acrylate oligomer (Mw: 3,650 g / mol, viscosity (25°C): 67,000 cps)
[0091] A-5: 9-functional urethane acrylate oligomer (Mw: 7,290 g / mol, viscosity (25°C): 9,310 cps)
[0092] B-1: 6-functional urethane acrylate oligomer (Mw: 1,950 g / mol, viscosity (25°C): 34,500 cps)
[0093] B-2: 6-functional urethane acrylate oligomer (Mw: 1,230 g / mol, viscosity (25°C): 22,000 cps)
[0094] B-3: 6-functional urethane acrylate oligomer (Mw: 2,610 g / mol, viscosity (25°C): 47,300 cps)
[0095] B-4: 6-functional urethane acrylate oligomer (Mw: 917 g / mol, viscosity (25°C): 17,000 cps)
[0096] B-5: 6-functional urethane acrylate oligomer (Mw: 3,190 g / mol, viscosity (25°C): 5,210 cps)
[0097] C-1: 3-functional acrylate monomer (Pentaerythritol Triacrylate, molecular weight 298 g / mol, viscosity (25℃) 1,450 cps)
[0098] C-2: A 2-functional acrylate monomer (1,6-hexanediol diacrylate, molecular weight 226 g / mol, viscosity (25℃) 10 cps).
[0099] C-3: 2-functionalized alkoxylated acrylate monomer (ethoxylated bisphenol A dimethacrylate, molecular weight 452 g / mol, viscosity (25℃) 1,200 cps)
[0100] D-1: Ceramic beads (average size (D50) of alkali aluminosilicate particles is 10 μm)
[0101] D-2: Ceramic beads (average size (D50) of alkali aluminosilicate particles is 8μm)
[0102] D-3: Ceramic beads (average size (D50) of alkali aluminosilicate particles is 12μm)
[0103] D-4: Ceramic beads (average size (D50) of alkali aluminosilicate particles is 5μm)
[0104] D-5: Ceramic beads (average size (D50) of alkali aluminosilicate particles is 15μm)
[0105] E-1: Photoinitiator 1 (Benzophenone)
[0106] E-2: Photoinitiator 2 (Methyl Benzoylformate)
[0107] F: Adhesion enhancer (polyester resin, Tego Variplus 3350UV, Evonik Industries)
[0108] G: Dispersant (Dispers 670, Evonik Industries)
[0109] H: Surface conditioner (silicone acrylate, RAD2500, Evonik Industries)
[0110] I: Polymerization inhibitor (Eastman's hydroquinone, Eastman Chemical Company)
[0111] J: Matting agent (white colored micronized silica gel, SS SIL-375, S-Chemtech, South Korea)
[0112] [Physical Property Evaluation]
[0113] The physical properties of the UV-curable coating compositions prepared according to the experimental and comparative examples were determined by the following methods, and the results are shown in Tables 4 to 6 below.
[0114] Sample preparation
[0115] The coating compositions of each embodiment and comparative example (thickness: 10-15 μm) were applied to PVC flooring material and then photocured (light intensity: 2,000 mJ / cm²). 2 Light intensity: 140mW / cm 2 Test pieces were prepared.
[0116] Appearance
[0117] The samples were visually inspected for defects such as roller marks, dewetting, and orange peel, and were evaluated as excellent (◎), good (○), fair (△), and poor (×).
[0118] Curing properties
[0119] At 2,000 mJ / 100 mW / cm 2 After curing the test pieces under the specified conditions, their appearance was observed and evaluated using the criteria of Excellent (◎), Good (○), Average (△), and Poor (×).
[0120] Adhesion
[0121] The cross-cut tape test was performed and evaluated according to ASTM D3359. A cross cutter was used to create 100 1mm x 1mm grids (10 horizontal and 10 vertical grids) on the surface. After applying and removing the NICHIBAN tape, the number of grids in which the coating remained adhered was counted, and the adhesion was evaluated according to the following criteria.
[0122] [Evaluation Criteria]
[0123] Excellent (◎): Coating adhesion maintains 99 or more grid squares.
[0124] Good (○): Coating adhesion remains above 95 and below 99.
[0125] General (△): Coating adhesion remains above 85 and below 95.
[0126] Defective (×): Coating adhesion remains less than 85 squares.
[0127] Stain resistance
[0128] Oil-based magic ink was applied to each test piece, and the erasability was checked after 5 minutes. The results were evaluated as excellent (◎), good (○), fair (△), and poor (×).
[0129] Iodine resistance
[0130] Iodine produced in China was dripped onto each test piece, and the erasure property was confirmed after 30 minutes. The results were evaluated as excellent (◎), good (○), fair (△), and poor (×).
[0131] luster
[0132] The gloss of each sample was measured using a glossmeter (60 degrees) and evaluated as excellent (◎), good (○), fair (△), and poor (×).
[0133] Scratch resistance
[0134] The degree of coating damage was observed according to the EN16094 test method, and the scratch resistance was evaluated according to the following criteria.
[0135] Excellent (◎): No scratches. Good (○): 1 or more but fewer than 10 scratches found.
[0136] General (△): 10 or more but less than 30 scratches identified.
[0137] Defective (×): More than 30 scratches detected
[0138] [Table 4]
[0139] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 <![CDATA[ 外观 ]]> ◎ ◎ ○ ◎ ◎ ○ ◎ ◎ ○ ◎ <![CDATA[ 固化性 ]]> ◎ ◎ ○ ○ ○ ◎ ◎ ◎ ◎ ◎ <![CDATA[ 附着性 ]]> ◎ ○ ◎ ◎ ◎ ◎ ○ ○ ◎ △ <![CDATA[ 耐污染性 ]]> ◎ ○ ○ ○ ◎ ◎ ○ ◎ ◎ ○ <![CDATA[ 耐碘性 ]]> ◎ ○ ○ ○ ◎ ◎ ○ ◎ ◎ ○ <![CDATA[ 光泽 ]]> ◎ ○ ◎ ◎ ◎ ◎ ◎ ◎ ○ ○ <![CDATA[ 抗划伤性 ]]> ◎ ◎ ◎ ○ ○ ○ ◎ ○ ◎ △
[0140] [Table 5]
[0141] Example 11 Example 12 Example 13 Example 14 Example 15 Example 16 Example 17 Example 18 Example 19 <![CDATA[ 外观 ]]> △ ◎ ○ ◎ △ ◎ ◎ ◎ ◎ <![CDATA[ 固化性 ]]> ○ ◎ ○ ◎ ○ ○ ◎ ◎ △ <![CDATA[ 附着性 ]]> ◎ ◎ ○ ◎ △ ○ ○ ◎ △ <![CDATA[ 耐污染性 ]]> ◎ ○ ◎ △ ◎ ◎ ○ △ ◎ <![CDATA[ 耐碘性 ]]> ◎ ○ ◎ △ ◎ ◎ ○ △ ◎ <![CDATA[ 光泽 ]]> △ ◎ ◎ ○ ○ ◎ ◎ △ ◎ <![CDATA[ 抗划伤性 ]]> ◎ ○ ◎ △ ◎ ◎ ◎ ○ ○
[0142] [Table 6]
[0143]
[0144]
[0145] As can be seen from the results in Tables 4 to 6 above, the UV-curable coating compositions of Examples 1-19 according to the present invention generally exhibited excellent physical properties in the tested items. Conversely, the UV-curable coating compositions of Comparative Examples 1-12, which deviated from the compositions of the present invention, generally exhibited poor physical properties compared to the examples.
[0146] Specifically, the UV-curable coating composition of Comparative Example 1, which uses a 9-functional urethane (meth)acrylate oligomer but has a weight-average molecular weight (A-4) that does not reach the lower limit of the scope of this invention, exhibits inferior curing properties, stain resistance, iodine resistance, and gloss. On the other hand, the UV-curable coating composition of Comparative Example 2, which uses a 9-functional urethane (meth)acrylate oligomer but has a weight-average molecular weight (A-5) that exceeds the upper limit of the scope of this invention, exhibits inferior appearance, curing properties, stain resistance, iodine resistance, and scratch resistance.
[0147] Although a hexafunctional urethane (meth)acrylate oligomer was used, the UV-curable coating composition of Comparative Example 3, which used a hexafunctional urethane (meth)acrylate oligomer (B-4) with a weight-average molecular weight that did not reach the lower limit of the scope of this invention, showed inferior curing properties, stain resistance, iodine resistance, and scratch resistance. On the other hand, the UV-curable coating composition of Comparative Example 4, which used a hexafunctional urethane (meth)acrylate oligomer, which used a hexafunctional urethane (meth)acrylate oligomer (B-5) with a weight-average molecular weight that exceeded the upper limit of the scope of this invention, showed inferior curing properties and scratch resistance.
[0148] Although ceramic beads were used, the UV-curable coating composition of Comparative Example 5, which used ceramic beads with an average particle size (D-4) that did not reach the lower limit of the scope of this invention, showed inferior appearance, gloss, and scratch resistance. On the other hand, the UV-curable coating composition of Comparative Example 6, which used ceramic beads, but used ceramic beads with an average particle size (D-5) that exceeded the upper limit of the scope of this invention, showed inferior appearance, adhesion, stain resistance, and iodine resistance.
[0149] The UV-curable coating composition of Comparative Example 7, which does not contain the 9-functional urethane (meth)acrylate oligomer (A) of the present invention, shows inferior appearance, stain resistance, gloss, and scratch resistance. The UV-curable coating composition of Comparative Example 8, which does not contain the 6-functional urethane (meth)acrylate oligomer (B) of the present invention, shows inferior appearance, stain resistance, gloss, and scratch resistance.
[0150] Furthermore, the UV-curable coating composition of Comparative Example 9, which does not contain the (meth)acrylate monomer (C-1) with three or more functional groups according to the present invention, exhibits inferior curing properties and adhesion; the UV-curable coating composition of Comparative Example 10, which does not contain the (meth)acrylate monomer (C-2) with two functional groups according to the present invention, exhibits inferior curing properties, stain resistance, iodine resistance, and gloss; and the UV-curable coating composition of Comparative Example 11, which does not contain the (meth)acrylate monomer (C-3) with two functional groups according to the present invention, exhibits inferior appearance, curing properties, adhesion, and gloss. The UV-curable coating composition of Comparative Example 12, which does not contain the ceramic beads (D) according to the present invention, exhibits inferior curing properties, adhesion, and scratch resistance.
Claims
1. A UV-curable coating composition, characterized in that, It contains 9-functional urethane (meth)acrylate oligomers, 6-functional urethane (meth)acrylate oligomers, 3 or more functional (meth)acrylate monomers, 2-functional (meth)acrylate monomers, 2 or more functional alkoxylated (meth)acrylate monomers, ceramic beads, and a photoinitiator. The weight-average molecular weight of the above-mentioned 9-functionalized urethane (meth)acrylate oligomers is 4,000 to 7,000 g / mol, and the viscosity at 25°C is 70,000 to 90,000 cps. The weight-average molecular weight of the above-mentioned six-functional urethane (meth)acrylate oligomers is 1,000 to 3,000 g / mol, and the viscosity at 25°C is 20,000 to 50,000 cps. The molecular weight of the (meth)acrylate monomers with three or more functional groups is 100 to 500 g / mol, and the viscosity at 25°C is 800 to 2,000 cps. The molecular weight of the aforementioned difunctional (meth)acrylate monomers ranges from 100 to 400 g / mol, and their viscosity at 25°C ranges from 1 to 30 cps. The molecular weight of the above-mentioned alkoxylated (meth)acrylate monomers with two or more functional groups is 300 to 600 g / mol, and the viscosity at 25°C is 800 to 1,600 cps. The ceramic beads mentioned above are spherical ceramic beads with an average particle size D50 of 7 to 13 μm. Relative to the total weight of the above-mentioned UV-curable coating composition, it comprises 10 to 30% by weight of the above-mentioned 9-functional urethane (meth)acrylate oligomer, 5 to 15% by weight of the above-mentioned 6-functional urethane (meth)acrylate oligomer, 2 to 15% by weight of the above-mentioned 3-functional or higher (meth)acrylate monomer, 20 to 35% by weight of the above-mentioned 2-functional (meth)acrylate monomer, 0.5 to 10% by weight of the above-mentioned 2-functional or higher alkoxylated (meth)acrylate monomer, 1 to 8% by weight of the above-mentioned ceramic beads, and 0.1 to 10% by weight of the above-mentioned photoinitiator.
2. The UV-curable coating composition according to claim 1, wherein, The above-mentioned (meth)acrylate monomers with 3 or more functional groups, the above-mentioned (meth)acrylate monomers with 2 functional groups, and the above-mentioned alkoxylated (meth)acrylate monomers with 2 or more functional groups are used in a weight ratio of 1:1 to 5:0.1 to 1.
5.
3. The UV-curable coating composition according to claim 1, wherein, The ceramic beads mentioned above are alkali aluminosilicate ceramic beads.
Citation Information
Patent Citations
Ultraviolet curing coating and preparation method thereof
CN104403554A
A ultraviolet-curable coating composition
CN113493644A