Positive electrode active material and sodium ion secondary battery
By using Na oxide particles with a P2-type structure and specific element composition in the cathode active material, the problem of insufficient energy density of the cathode active material in the existing technology is solved, and higher gravimetric energy density and charge and discharge performance are achieved.
Patent Information
- Application Number
- CN202410460766.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-29
AI Technical Summary
There is still room for improvement in the gravimetric energy density of existing cathode active materials with a P2-type structure.
Use Na-containing oxide particles as the positive electrode active material, which have a P2 type structure, contain Mn, Ni and Co elements, have an average particle diameter of 2.0 μm or more, an average aspect ratio of 1.0 or more and 3.0 or less, and go through a specific firing process. and Na doping method to ensure the chemical composition and structural characteristics of the oxide particles.
The gravimetric energy density of the cathode active material is significantly increased, achieving higher charge and discharge performance and stability.
Smart Images

Figure CN118867151A_ABST
Abstract
Description
Technical Field
[0001] The present application discloses a positive electrode active material and a sodium ion secondary battery. Background Art
[0002] Patent Documents 1 and 2 disclose Na-containing oxides having a P2-type structure and a predetermined chemical composition. The Na-containing oxides having the P2-type structure are used as positive electrode active materials of sodium ion secondary batteries.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-201588
[0006] Patent Document 2: Japanese Patent Application Publication No. 2017-045600 Summary of the invention
[0007] Problems to be solved by the invention
[0008] The weight energy density of conventional positive electrode active materials having a P2 type structure still has room for improvement.
[0009] Means for solving problems
[0010] The present application discloses the following multiple solutions as means for solving the above-mentioned problems.
[0011] <Option 1>
[0012] A positive electrode active material, comprising oxide particles containing Na, wherein the oxide particles containing Na have a P2 type structure, the oxide particles containing Na contain at least one element of Mn, Ni and Co, Na and O as constituent elements, the oxide particles containing Na have an average particle size of 2.0 μm or more, and the oxide particles containing Na have an average aspect ratio of 1.0 or more and 3.0 or less.
[0013] <Option 2>
[0014] The positive electrode active material according to claim 1, wherein the Na-containing oxide particles contain more than 0.35 mol of Na per 1 mol of O as a constituent element.
[0015] <Option 3>
[0016] The positive electrode active material according to claim 1 or 2, wherein the oxide particles containing Na have a a Mn x-p Ni y-q Co z-rM p+q+r The chemical composition represented by O2, wherein 0<a≤1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
[0017] <Option 4>
[0018] The positive electrode active material according to any one of embodiments 1 to 3, wherein the oxide particles containing Na have a Mn x-p Ni y-q Co z-r M p+q+r O2 represents a chemical composition, wherein 0<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
[0019] <Option 5>
[0020] The positive electrode active material according to any one of embodiments 1 to 4, wherein the oxide particles containing Na have a a Mn x-p Ni y-q Co z-r M p+q+r O2 represents a chemical composition, wherein 0.70<a≤1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
[0021] <Option 6>
[0022] The positive electrode active material comprises oxide particles containing Na, wherein the oxide particles containing Na have a P2 type structure, and the oxide particles containing Na have a structure composed of Na a Mn x-p Ni y-q Co z-r M p+q+rO2 represents a chemical composition, wherein 0.70<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
[0023] <Option 7>
[0024] The positive electrode active material according to claim 6, wherein the oxide particles containing Na have a a Mn x- p Ni y-q Co z-r M p+q+r O2 represents a chemical composition, wherein 0.70<a≤1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
[0025] <Option 8>
[0026] The positive electrode active material according to any one of schemes 1 to 7, wherein the P2 type structure has The following is the c-axis length.
[0027] <Option 9>
[0028] A sodium ion secondary battery comprising a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, wherein the positive electrode active material layer contains the positive electrode active material according to any one of aspects 1 to 8.
[0029] Effects of the Invention
[0030] The positive electrode active material disclosed in the present invention has excellent gravimetric energy density. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 An example of a flow of a method for producing a Na-containing oxide having a P2 type structure is shown.
[0032] Figure 2 An example of the structure of a sodium ion secondary battery is schematically shown.
[0033] Figure 3 X-ray diffraction patterns of the positive electrode active materials according to Examples 1 to 3 are shown.
[0034] Figure 4 The X-ray diffraction pattern of the positive electrode active material according to Comparative Example 1 is shown.
[0035] Figure 5 A cross-sectional SEM image of the positive electrode active material according to Example 1 is shown.
[0036] Figure 6 A SEM image of the appearance of the positive electrode active material according to Example 1 is shown.
[0037] Description of Reference Numerals
[0038] 100 Sodium ion secondary battery
[0039] 10 Positive electrode active material layer
[0040] 20 Electrolyte layer
[0041] 30 Negative electrode active material layer
[0042] 40 positive electrode collector
[0043] 50 Negative electrode collector DETAILED DESCRIPTION
[0044] 1. Positive electrode active material
[0045] 1.1 First Form
[0046] The positive electrode active material involved in the first form includes oxide particles containing Na. The oxide particles containing Na have a P2 type structure. The oxide particles containing Na contain at least one element of Mn, Ni and Co, and Na and O as constituent elements. The oxide particles containing Na have an average particle size of 2.0 μm or more. The oxide particles containing Na have an average aspect ratio of 1.0 or more and 3.0 or less.
[0047] 1.1.1 Crystal structure
[0048] The oxide particles containing Na involved in the first form have at least a P2-type structure (belonging to the space group P63mc) as a crystal structure. The oxide particles containing Na may have a crystal structure other than the P2-type structure while having the P2-type structure. As a crystal structure other than the P2-type structure, for example, various crystal structures (P3-type structures, etc.) formed when Na is separated from the P2-type structure and Na is inserted into the P2-type structure can be listed. The oxide particles containing Na may have a P2-type structure as a main phase. Depending on the charge and discharge state, the crystal structure that becomes the main phase of the oxide particles containing Na may change.
[0049] The oxide particles containing Na involved in the first form may be single crystals consisting of one microcrystal, or may be polycrystalline having a plurality of microcrystals. For oxide particles containing Na, it is believed that the end faces of the microcrystals become the entrance and exit of the intercalation. That is, in the case where the microcrystals of the oxide particles containing Na are small, the entrance and exit of the intercalation increase, and the effect of reducing the reaction resistance can be expected; the effect of reducing the movement distance of the sodium ions and thus reducing the diffusion resistance; the effect of reducing the absolute amount of expansion and contraction during charging and discharging, and the effect of being difficult to produce cracks, etc. For example, the diameter of the microcrystals constituting the oxide particles containing Na may be 0.1 μm or more and 5.0 μm or less, 0.5 μm or more and 4.0 μm or less, or 1.0 μm or more and 3.0 μm or less. It should be noted that "microcrystals" and "diameter of microcrystals" can be obtained by observing the oxide particles containing Na using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when observing the oxide particles containing Na, a closed area surrounded by a grain boundary is observed, and the area is regarded as a "microcrystal". For the crystallite, the maximum Feret diameter is determined and regarded as the "diameter of the crystallite". Furthermore, if the oxide particle containing Na is composed of a single crystal, the particle itself can be called a crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can also be obtained by EBSD or XRD. For example, the diameter of the crystallite can be calculated based on the Scherrer equation by the half-maximum full width of the diffraction line of the XRD pattern. When the diameter of the crystallite determined by any method of the oxide particle containing Na is within the above range, it is easy to exert higher performance. The crystallite constituting the oxide particle containing Na may have a first surface exposed on the surface of the oxide, and the first surface may be planar.
[0050] The Na-containing oxide particles involved in the first embodiment have a predetermined average particle size (D50) and a predetermined average aspect ratio. In order to achieve such an average particle size and average aspect ratio, in the present embodiment, a specific process described later is used when manufacturing the Na-containing oxide particles. According to the understanding of the inventors, the c-axis length of the P2-type structure of the Na-containing oxide particles obtained through such a specific process is likely to become smaller than before. For example, the P2-type structure in the Na-containing oxide particles involved in the first embodiment may have The P2-type structure may have a c-axis length of Above and The following c-axis length. It should be noted that the lattice constants (a-axis length, b-axis length and c-axis length) of the P2-type structure can be determined by the X-ray diffraction pattern of the oxide particles containing Na by full pattern fitting. The software uses PDXL2 from Rigaku Corporation. Among them, "X-ray diffraction pattern of oxide particles containing Na" refers to a pattern obtained under the following conditions. That is, for oxide particles containing Na, an X-ray diffraction device (Rigaku, fully automatic multi-purpose X-ray diffraction device SmartLab) is used, CuKα is used as a ray source, and a 2θ / θ scan is performed with a tube voltage of 45kV, a tube current of 200mA, a step width of 0.02°, and a scanning speed of 1° / min to obtain an X-ray diffraction pattern.
[0051] 1.1.2 Chemical composition
[0052] The Na-containing oxide particles involved in the first form contain at least one element of Mn, Ni and Co, and Na and O as constituent elements. Among them, when the Na-containing oxide particles contain at least Na, and Mn, and one or both of Ni and Co, and O as constituent elements, in particular, when at least Na, Mn, Ni, Co and O are contained as constituent elements, it is easy to obtain higher performance. Alternatively, when the Na-containing oxide particles contain at least Na, Mn, Fe and O as constituent elements, it is also easy to obtain higher performance. In addition, in the Na-containing oxide particles involved in the first form, as a constituent element, more than 0.35 moles of Na may be contained relative to 1 mole of O. There is no particular limit on the upper limit of the amount of Na relative to O. In the Na-containing oxide particles involved in the first form, as a constituent element, more than 0.35 moles and less than 0.50 moles, or more than 0.38 moles and less than 0.45 moles of Na may be contained relative to 1 mole of O. Such Na-containing oxide particles containing more than 0.35 mol of Na per 1 mol of O tend to have an excellent weight energy density as a positive electrode active material.
[0053] The Na-containing oxide particles according to the first embodiment may have Na a Mn x-p Ni y-q Co z-r M p+q+rO2 (wherein 0<a≤1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) A chemical composition represented by. In the case where the oxide particles containing Na have such a chemical composition, it is easy to maintain the P2 type structure. In the above chemical composition, a is greater than 0, and can be greater than 0.10, greater than 0.20, greater than 0.30, greater than 0.40, greater than 0.50, greater than 0.60 or greater than 0.70, and is less than 1.00, and can be less than 0.90. In addition, x is 0 or more, and may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is 1.00 or less, and may be less than 1.00, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, or less than 0.50. In addition, y is 0 or more, and may be greater than 0, 0.10 or more, or 0.20 or more, and is 1.00 or less, and may be less than 1.00, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In addition, z is greater than 0, may be greater than 0, greater than 0.10, greater than 0.20 or greater than 0.30, and is less than 1.00, may be less than 1.00, less than 0.90, less than 0.80, less than 0.70, less than 0.60, less than 0.50, less than 0.40 or less than 0.30. Element M contributes little to charge and discharge. In this regard, in the above-mentioned chemical composition, it is easy to ensure high charge and discharge capacity by p+q+r being less than 0.17. p+q+r may be less than 0.16, less than 0.15, less than 0.14, less than 0.13, less than 0.12, less than 0.11 or less than 0.10. On the other hand, by including element M, the P2 type structure is easily stabilized. In the above chemical composition, p+q+r is greater than 0, and may be greater than 0.01, greater than 0.02, greater than 0.03, greater than 0.04, greater than 0.05, greater than 0.06, greater than 0.07, greater than 0.08, greater than 0.09, or greater than 0.10. The composition of O is approximately 2, but is not limited to exactly 2.0, and may vary.
[0054] The Na-containing oxide particles according to the first embodiment may have Na a Mn x-p Ni y-q Co z-r M p+q+rO2 (wherein 0<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) The chemical composition represented by the first embodiment may include a Na-containing oxide particle. a Mn x-p Ni y-q Co z-r M p+q+r O2 (wherein 0.70<a≤1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1 and 0≤p+q+r<0.17, element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) Chemical composition represented. In the past, it was difficult to produce oxide particles containing Na having a P2 type structure and such a chemical composition, but in this embodiment, as the manufacturing conditions of the oxide particles containing Na having a P2 type structure, the specific conditions described later are adopted, so that the oxide particles containing Na having a P2 type structure and such a chemical composition can be obtained. The oxide particles containing Na having such a chemical composition have excellent weight energy density as a positive electrode active material.
[0055] 1.1.3 Shape
[0056] The Na-containing oxide particles involved in the first embodiment may be solid particles, hollow particles, or particles having voids. The Na-containing oxide particles involved in the first embodiment have excellent weight energy density as a positive electrode active material by having the following average aspect ratio and average particle size.
[0057] 1.1.3.1 Aspect Ratio
[0058] The P2 type structure is a hexagonal system, the diffusion coefficient of Na ions is large, and crystals are easy to grow in a specific direction. In particular, as a transition metal element constituting the P2 type structure, in the case of containing at least one of Mn, Ni and Co, the crystals are easy to grow into a plate-like shape in a specific direction. Therefore, the oxide particles containing Na with the P2 type structure usually become plate-like particles with a large aspect ratio and a biased growth direction of the crystal in a specific direction. Specifically, the oxide particles containing Na with the P2 type structure usually become plate-like particles with an average aspect ratio significantly exceeding 3.0. Among them, the ends of the plate-like particles become the entrance and exit of the intercalation. According to the present inventors, the proportion of the portion of the plate-like particles with a large aspect ratio that contributes to the intercalation tends to become smaller in the overall particle, and the weight energy density is easily reduced.
[0059] The Na-containing oxide particles involved in the first form suppress the bias of the growth direction of the crystal and have an aspect ratio below a certain level. Specifically, the Na-containing oxide particles involved in the first form have an average aspect ratio of 1.0 to 3.0. By having an average aspect ratio of the Na-containing oxide particles having a P2-type structure of 3.0 or less, the weight energy density as a positive electrode active material is easily increased. The average aspect ratio of the Na-containing oxide particles involved in the first form may be 1.0 to 2.9, 1.0 to 2.8, 1.0 to 2.7, 1.0 to 2.6, 1.0 to 2.5, or 1.0 to 2.4.
[0060] Furthermore, the "average aspect ratio" of the oxide particles containing Na is measured as follows. That is, a scanning electron microscope (SEM) or a transmission electron microscope (TEM) is used to observe the cross section of the oxide particles containing Na (when the oxide particles containing Na are included in the positive electrode active material layer described later, it is the cross section of the positive electrode active material layer) to determine the shape of the oxide particles containing Na. In this shape, the largest Feret diameter is determined and regarded as the "major diameter". In addition, in this shape, the largest diameter orthogonal to the "major diameter" is regarded as the "minor diameter". The ratio of the "major diameter" to the "minor diameter" (major diameter / minor diameter) is regarded as the "aspect ratio" of the oxide particles containing Na. For each oxide particle containing Na, the "aspect ratio" is calculated, and its arithmetic average is regarded as the "average aspect ratio".
[0061] 1.1.3.2 Average particle size
[0062] As described above, in the prior art, the Na-containing oxide particles having a P2-type structure become plate-like particles with a large aspect ratio and a crystal growth direction biased in a specific direction. In the prior art, if the growth of the P2 phase is to be suppressed, the average particle size of the Na-containing oxide particles becomes extremely small, and there is a concern about excessive agglomeration (aggregation) between particles, etc., and in addition, it is possible that a sufficient amount of P2 phase cannot be obtained. As a result of these, the Na-containing oxide particles of the prior art are difficult to ensure sufficient weight energy density. The Na-containing oxide particles involved in the first form can eliminate such problems by having the above-mentioned average aspect ratio and having a size greater than a certain value. Specifically, the Na-containing oxide particles involved in the first form have an average particle size of more than 2.0 μm. The average particle size of the Na-containing oxide particles involved in the first form may be greater than 2.0 μm and less than 5.0 μm, greater than 2.0 μm and less than 4.0 μm, or greater than 2.0 μm and less than 3.0 μm.
[0063] The “average particle size” of the oxide particles containing Na refers to the particle size at 50% of the cumulative value in the volume-based particle size distribution using a laser diffraction / scattering method (D50, median diameter).
[0064] 1.1.4 Others
[0065] As described above, the positive electrode active material involved in the first form has excellent weight energy density by including oxide particles containing Na having the above-mentioned specific average particle size and average aspect ratio. The positive electrode active material involved in the first form may only include the above-mentioned oxide particles containing Na, or may also include positive electrode active materials (other positive electrode active materials) other than the above-mentioned oxide particles containing Na. From the viewpoint of further improving the above-mentioned effect, the proportion of other positive electrode active materials in the positive electrode active material as a whole may be a small amount. For example, when the whole of the positive electrode active material is set to 100% by mass, the content of the above-mentioned oxide particles containing Na may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.
[0066] 1.2 Second Form
[0067] The positive electrode active material according to the second embodiment includes oxide particles containing Na. The oxide particles containing Na have a P2 type structure. The oxide particles containing Na have a structure composed of Na a Mn x-p Ni y-q Coz-r M p+q+r O2 (wherein, 0.70<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W).
[0068] 1.2.1 Crystal structure
[0069] The oxide particles containing Na involved in the second form are similar to the oxide particles containing Na involved in the first form, and as a crystal structure, they have at least a P2-type structure (belonging to the space group P63mc). The oxide particles containing Na may have a crystal structure other than the P2-type structure while having the P2-type structure. As crystal structures other than the P2-type structure, for example, various crystal structures (P3-type structures, etc.) formed when Na is separated from the P2-type structure and Na is inserted into the P2-type structure can be listed. The oxide particles containing Na may have a P2-type structure as the main phase. Depending on the charge and discharge state, the crystal structure that becomes the main phase of the oxide particles containing Na may change.
[0070] The oxide particles containing Na involved in the second form may be single crystals composed of one microcrystal or polycrystals having multiple microcrystals, similarly to the oxide particles containing Na involved in the first form. As described above, for oxide particles containing Na, it is believed that the end faces of the microcrystals become the entrance and exit of the intercalation. That is, in the case where the crystallites of the oxide particles containing Na are small, the effects of increasing the entrance and exit of the intercalation and reducing the reaction resistance can be expected; the effect of shortening the movement distance of the sodium ions and reducing the diffusion resistance; the effect of reducing the absolute amount of expansion and contraction during charging and discharging and making it difficult to crack, etc. For example, the diameter of the crystallites constituting the oxide particles containing Na may be greater than 0.1 μm and less than 5.0 μm, greater than 0.5 μm and less than 4.0 μm, or greater than 1.0 μm and less than 3.0 μm. The crystallites constituting the oxide particles containing Na may have a first surface exposed on the surface of the oxide, and the first surface may be planar.
[0071] The second embodiment of the Na-containing oxide particles has a P2-type structure and a predetermined chemical composition. In order to achieve such a crystal structure and chemical composition, in the present embodiment, a specific process described later is used when manufacturing the Na-containing oxide particles. According to the understanding of the inventors, the c-axis length of the P2-type structure of the Na-containing oxide particles obtained through such a specific process is likely to become smaller than before. For example, the P2-type structure in the Na-containing oxide particles involved in the second embodiment may have The P2-type structure may have a c-axis length of Above and The following c-axis length. The method for measuring lattice constants such as c-axis length is as described above.
[0072] 1.2.2 Chemical composition
[0073] The Na-containing oxide particles according to the second embodiment have Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (wherein 0.70<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) The second embodiment of the oxide particles containing Na may have a composition consisting of Na a Mn x-p Ni y-q Co z-r M p+q+rO2 (wherein 0.70<a≤1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1 and 0≤p+q+r<0.17, element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) Chemical composition represented. In the past, it was difficult to produce Na-containing oxide particles having a P2-type structure and such a chemical composition, but in the present embodiment, as a manufacturing condition for Na-containing oxide particles having a P2-type structure, by adopting specific conditions, Na-containing oxide particles having a P2-type structure and such a chemical composition can be obtained. Na-containing oxide particles having such a chemical composition have a high weight energy density as a positive electrode active material. a is greater than 0.70, may be 0.75 or more, or 0.80 or more, and is less than 1.00, and may be less than 0.90 or less than 0.90. In addition, x may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be less than 1.00, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.60 or less, 0.50 or less, or less than 0.50. In addition, y may be greater than 0, 0.10 or more, greater than 0.10, or 0.20 or more, and may be less than 0.50, 0.45 or less, or 0.40 or less. In addition, z may be greater than 0, greater than 0.10, greater than 0.10, greater than 0.20, or greater than 0.30, and may be less than 1.00, less than 0.90, less than 0.80, less than 0.70, less than 0.60, less than 0.50, less than 0.50, less than 0.40, or less than 0.30. p+q+r is greater than 0, and may be greater than 0.01, greater than 0.02, greater than 0.03, greater than 0.04, greater than 0.05, greater than 0.06, greater than 0.07, greater than 0.08, greater than 0.09, or greater than 0.10, and may be less than 0.17, less than 0.16, less than 0.15, less than 0.14, less than 0.13, less than 0.12, less than 0.11, or less than 0.10. The composition of O is approximately 2, but is not limited to exactly 2.0, and may vary.
[0074] 1.2.3 Shape
[0075] The Na-containing oxide particles according to the second embodiment may be solid particles, hollow particles, or particles having voids. The Na-containing oxide particles according to the second embodiment may have the following average aspect ratio and average particle size.
[0076] 1.2.3.1 Aspect Ratio
[0077] The Na-containing oxide particles involved in the second form suppress the deviation of the growth direction of the crystal and may have an aspect ratio below a certain value. Specifically, the Na-containing oxide particles involved in the second form may have an average aspect ratio of 1.0 to 3.0. By having an average aspect ratio of Na-containing oxide particles of a P2-type structure of 3.0 or less, the weight energy density of the positive electrode active material can be further increased. The average aspect ratio of the Na-containing oxide particles involved in the second form may be 1.0 to 2.9, 1.0 to 2.8, 1.0 to 2.7, 1.0 to 2.6, 1.0 to 2.5, or 1.0 to 2.4. The method for determining the "average aspect ratio" is as described above.
[0078] 1.2.3.2 Average particle size
[0079] The Na-containing oxide particles involved in the second embodiment may have an average particle size of 2.0 μm or more. The average particle size of the Na-containing oxide particles involved in the second embodiment may be 2.0 μm or more and 5.0 μm or less, 2.0 μm or more and 4.0 μm or less, or 2.0 μm or more and 3.0 μm or less. The method for measuring the "average particle size" of the Na-containing oxide particles is as described above.
[0080] 1.2.4 Others
[0081] As described above, the positive electrode active material involved in the second form has excellent weight energy density by including oxide particles containing Na having the above-mentioned specific chemical composition. The positive electrode active material involved in the second form may be composed only of the above-mentioned oxide particles containing Na, or may include positive electrode active materials (other positive electrode active materials) other than the above-mentioned oxide particles containing Na. From the viewpoint of further improving the above-mentioned effect, the proportion of other positive electrode active materials in the positive electrode active material as a whole may be a small amount. For example, when the whole of the positive electrode active material is set to 100% by mass, the content of the above-mentioned oxide particles containing Na may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.
[0082] 2. Method for producing positive electrode active material
[0083] The oxide particles containing Na in the first and second aspects described above can be produced, for example, by the following method. Figure 1As shown, a method for producing Na-containing oxide particles having a P2-type structure according to one embodiment includes:
[0084] S1: obtaining a precursor containing at least one element of Mn, Ni and Co;
[0085] S2: coating the surface of the precursor with a Na source to obtain a composite;
[0086] S3: sintering the composite to obtain an oxide containing Na and having a P2-type structure. Wherein, S3 comprises:
[0087] S3-1: pre-sintering the composite at a temperature of 300° C. or higher and less than 700° C. for 2 hours or higher and 10 hours or lower;
[0088] S3-2: After the preliminary calcination, the composite is subjected to main calcination at a temperature of 700° C. to 1100° C. for 30 minutes to 48 hours; and
[0089] S3-3: Following the main calcination, the composite is cooled in the atmosphere from a temperature T1 of 200°C or higher to a temperature T2 of 100°C or lower.
[0090] 2.1S1
[0091] In S1, a precursor containing at least one element of Mn, Ni and Co is obtained. The precursor may contain at least Mn, and one or both of Ni and Co, and may contain at least Mn, Ni and Co. The precursor may be a salt containing at least one element of Mn, Ni and Co. For example, the precursor may be at least one of carbonate, sulfate, nitrate and acetate. Alternatively, the precursor may be a compound other than a salt. For example, the precursor may be a hydroxide. The precursor may be a hydrate. The precursor may be a combination of multiple compounds. The precursor may be in various shapes. For example, the precursor may be in the form of particles, or may be spherical particles as described later. There is no particular limitation on the particle size of the particles formed by the precursor. The composition of the precursor may be appropriately determined in a manner corresponding to the composition of the oxide containing Na as the final product.
[0092] In S1, an ion source that can form a precipitate with transition metal ions in an aqueous solution and a transition metal compound containing at least one element of Mn, Ni and Co are used, and a coprecipitation method (coprecipitation method) is adopted to obtain a precipitate as the above-mentioned precursor. Thus, spherical particles as a precursor are easily obtained. "An ion source that can form a precipitate with transition metal ions in an aqueous solution" can be, for example, at least one selected from sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide and sodium oxide. The transition metal compound can be the above-mentioned salt, hydroxide, etc. containing at least one element of Mn, Ni and Co. Specifically, in S1, after the ion source and the transition metal compound are made into solutions respectively, each solution is dripped and mixed, so that a precipitate as a precursor can be obtained. At this time, as a solvent, for example, water is used. At this time, as a base, various sodium compounds can be used, and in addition, an ammonia solution can be added to adjust the alkalinity. In the case of the coprecipitation method, for example, by preparing an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate, each aqueous solution is dripped and mixed, so as to obtain a precipitate as a precursor. Alternatively, the precursor can also be obtained by a sol-gel method. In particular, spherical particles as a precursor can be easily obtained by a coprecipitation method.
[0093] In S1, the precursor may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W. These elements M, for example, have the function of stabilizing the P2 type structure. There is no particular limitation on the method for obtaining the precursor containing element M. In the case where the precursor is obtained by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dripped and mixed to obtain a precursor containing at least one of Mn, Ni and Co and also containing element M. Alternatively, in the manufacturing method of the present disclosure, element M is not added in S1, and element M can be doped when Na-doping sintering is performed in S2 and S3 described later.
[0094] 2.2S2
[0095] In S2, the surface of the precursor obtained by S1 is coated with a Na source to obtain a composite. The Na source can be a salt containing Na such as carbonates and nitrates, or a compound other than salts such as sodium oxide and sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor can be determined by adding the Na disappearance portion during the subsequent calcination.
[0096] In S2, there is no particular limitation on the coverage of the Na source on the surface of the precursor. For example, in S2, the above-mentioned composite can be obtained by coating more than 40 area%, more than 50 area%, more than 60 area% or more than 70 area% of the surface of the above-mentioned precursor with a Na source. Alternatively, in S2, the above-mentioned composite can be obtained by coating less than 40 area%, less than 35 area% or less than 30 area% of the surface of the above-mentioned precursor with a Na source. If the coverage of the Na source is small, then when the composite is fired, P2 type crystals are easy to grow on the surface of the composite. On the other hand, if the coverage of the Na source is large, then when the composite is fired, the crystallites of the P2 type crystals are easy to become smaller, and the growth of the P2 type crystals is easy to be suppressed.
[0097] In S2, the method for coating the surface of the above-mentioned precursor with a Na source is not particularly limited. For example, by mixing the precursor and the Na source in a dry or wet manner, the surface of the precursor can be coated with a Na source. Alternatively, a tumbling flow coating method or a spray drying method can be used to coat the surface of the precursor with a Na source. That is, a coating solution in which the Na source is dissolved is prepared, and the coating solution is dried while contacting the surface of the precursor or after contact. By adjusting the conditions (temperature, time, number of times, etc.) of the coating, the coverage of the Na source on the surface of the precursor can be controlled.
[0098] In S2, the precursor may be coated with the M source together with the Na source. For example, in S2, the precursor obtained by S1, the Na source, and the M source containing at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W may be mixed to obtain a composite. The M source may be, for example, a salt containing the element M such as a carbonate or a sulfate, or a compound other than a salt such as an oxide or a hydroxide. The amount of the M source for the precursor may be determined according to the chemical composition of the oxide containing Na after sintering.
[0099] 2.3S3
[0100] In S3, the composite obtained in S2 is fired to obtain an oxide containing Na and having a P2 type structure. S3 includes the above-mentioned S3-1, S3-2 and S3-3.
[0101] 2.3.1S3-1
[0102] In S3-1, for the composite, pre-sintering is performed at a temperature of 300°C to 700°C for 2 hours to 10 hours. In S3-1, after the composite is arbitrarily formed, pre-sintering can be performed. The pre-sintering is performed at a temperature lower than that of the main sintering. If the pre-sintering is insufficient, in order to generate a sufficient amount of P2 phase in S3-2, the main sintering needs to be high temperature and long time, and the P2 phase may grow abnormally. In addition, if the pre-sintering in S3-1 is insufficient, it is difficult to dope a sufficient amount of Na, and it may be difficult to obtain the P2 phase with a specific chemical composition. By sufficiently performing the pre-sintering, the P2 phase is appropriately generated in the main sintering, and at the same time, the generation of crystalline phases other than the P2 phase can be suppressed, and the shape of the P2-type oxide particles containing Na can be easily and appropriately controlled. That is, in S3-1, by setting the pre-sintering temperature to be 300°C or higher and lower than 700°C and the pre-sintering time to be 2 hours or higher and lower than 10 hours, the composite can be sufficiently pre-sintered, and the oxide particles containing Na having a P2 type structure obtained through S3-2 and S3-3 described later become oxide particles having a predetermined average aspect ratio and average particle size. In addition, by sufficiently pre-sintering the composite, it is possible to have a predetermined chemical composition in S3-2 and S3-3, and at the same time, the P2 type structure is appropriately generated. The pre-sintering temperature may be 400°C or higher and lower than 700°C, 450°C or higher and lower than 700°C, 500°C or higher and lower than 700°C, 550°C or higher and lower than 700°C, or 550°C or higher and lower than 650°C. The calcination time may be 2 to 8 hours, 3 to 8 hours, 4 to 8 hours, 5 to 8 hours, or 5 to 7 hours. The calcination atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere.
[0103] 2.3.2S3-2
[0104] In S3-2, following the above-mentioned pre-calcination, the main calcination is carried out for more than 30 minutes and less than 48 hours for the composite at a temperature of more than 700°C and less than 1100°C. In S3-2, the main calcination temperature of the composite is more than 700°C and less than 1100°C, preferably more than 800°C and less than 1000°C. If the main calcination temperature is too low, the P2 phase is not generated. If the main calcination temperature is too high, the O3 phase is easily generated instead of the P2 phase. There is no particular limitation on the heating conditions from the pre-calcination temperature to the main calcination temperature. The main calcination time is, as described above, more than 30 minutes and less than 48 hours. However, the shape of the oxide containing Na can be controlled by the main calcination time. As described above, in the method disclosed in the present invention, when the coverage of the Na source in the composite is 40 area% or more, when the composite is calcined, it is easy to form small P2-type crystals on its surface. In the method disclosed in the present invention, the abnormal growth of P2 type crystals is suppressed by growing P2 type crystals along the surface of the complex. As a result, the shape of the oxide particles containing Na becomes a shape having a specified average aspect ratio and average particle size. If the main firing time is too short, the generation of the P2 phase becomes insufficient. On the other hand, if the main firing time is too long, the P2 type crystals grow excessively and the specified average aspect ratio and average particle size cannot be achieved. According to the inventors, when the main firing time is more than 30 minutes and less than 3 hours, the oxide particles containing Na tend to become particles having a specified average aspect ratio and average particle size.
[0105] 2.3.3S3-3
[0106] In S3-3, following the above-mentioned main calcination, the composite is rapidly cooled (cooled at a temperature drop rate of 20°C / min or more) from a temperature T1 of more than 200°C to a temperature T2 of less than 100°C. The above-mentioned preliminary calcination and main calcination are performed, for example, in a heating furnace. In step S3-3, for example, after the main calcination of the composite is performed in a heating furnace, it is cooled to an arbitrary temperature T1 of more than 200°C in the heating furnace. After reaching the temperature T1, the calcined product is taken out of the heating furnace and rapidly cooled outside the furnace to an arbitrary temperature T2 of less than 100°C. Temperature T1 is an arbitrary temperature of more than 200°C, and can be an arbitrary temperature of more than 250°C. Temperature T2 is an arbitrary temperature of less than 100°C, and can be an arbitrary temperature of less than 50°C, and can be the cooling end temperature. In the specified temperature range from temperature T1 to temperature T2, moisture easily penetrates into the interlayers of the P2 type structure due to atomic vibration, molecular motion, etc. It is believed that when the composite body (Na-containing oxide having a P2-type structure) after the main firing is cooled, the time in the temperature region where moisture easily penetrates is shortened (i.e., rapid cooling), so that the amount of moisture penetrating into the interlayers of the P2-type structure is reduced. In this regard, in step S3-3, when the composite body after the main firing is cooled, it is cooled in a dry atmosphere outside the furnace from an arbitrary temperature T1 above 200°C to an arbitrary temperature T2 below 100°C, and the cooling rate from temperature T1 to temperature T2 becomes high (e.g., 20°C / min or more), so that moisture is difficult to penetrate into the interlayers of the P2-type structure, and the collapse of the P2-type structure can be suppressed. As a result, Na-containing oxide particles having a P2-type structure and a predetermined chemical composition can be obtained.
[0107] According to the above method, the Na-containing oxide particles according to the first embodiment and the Na-containing oxide particles according to the second embodiment can be produced.
[0108] 3. Sodium ion secondary battery
[0109] The positive electrode active material according to the embodiment includes the above-mentioned specific oxide containing Na. This positive electrode active material can be used as a positive electrode active material of a sodium ion secondary battery, for example. Figure 2 The structure of a sodium ion secondary battery according to one embodiment is schematically shown in FIG. Figure 2 As shown, a sodium ion secondary battery 100 according to one embodiment includes a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. The positive electrode active material layer 10 includes the positive electrode active material according to the above-mentioned embodiment.
[0110] 3.1 Positive electrode active material layer
[0111] The positive electrode active material layer 10 contains at least the positive electrode active material involved in the above-mentioned embodiment, and may further optionally contain an electrolyte, a conductive aid, a binder, etc. Furthermore, the positive electrode active material layer 10 may also contain various additives. The content of each of the positive electrode active material, electrolyte, conductive aid, binder, etc. in the positive electrode active material layer 10 can be appropriately determined according to the target battery performance. For example, when the positive electrode active material layer 10 as a whole (solid component as a whole) is set to 100% by mass, the content of the positive electrode active material may be 40% by mass or more, 50% by mass or more, or 60% by mass or less, and may be 100% by mass or less or 90% by mass or less. There is no particular limitation on the shape of the positive electrode active material layer 10, for example, it may be a sheet-shaped positive electrode active material layer 10 having a substantially flat surface. There is no particular limitation on the thickness of the positive electrode active material layer 10, for example, it may be 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.
[0112] 3.1.1 Positive electrode active material
[0113] For the positive electrode active material, as described above. That is, the positive electrode active material includes the oxide particles containing Na involved in the first form and / or the oxide particles containing Na involved in the second form. As described above, the positive electrode active material may only include the above-mentioned oxide particles containing Na, or may also include the above-mentioned oxide particles containing Na while also including the positive electrode active material (other positive electrode active materials) other than it. From the viewpoint of further improving the effect of the technology disclosed in the present invention, the proportion of other positive electrode active materials in the positive electrode active material as a whole may be a small amount. For example, when the whole of the positive electrode active material is set to 100% by mass, the content of the above-mentioned oxide particles containing Na may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.
[0114] 3.1.2 Electrolytes
[0115] The electrolyte that may be contained in the positive electrode active material layer 10 may be a solid electrolyte, a liquid electrolyte (electrolyte), or a combination thereof. As for the solid electrolyte, a solid electrolyte known as a solid electrolyte for a sodium ion secondary battery may be used. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, the inorganic solid electrolyte has excellent ion conductivity and heat resistance. As the inorganic solid electrolyte, Na3Zr2PSi2O 12 , Na2O-11Al2O3 and other oxides; NaBH4, NaB 10 H10 、NaCB9H 10 、NaCB 11 H 12 , NaB 12 Cl 12 Such hydrides and borides; Na3PS4, Na3SbS4, Na 2.88 Sb 0.88 W 0.12 S4 and other sulfides; at least one of NaPF6, NaBF4 and other fluorides. The solid electrolyte may be, for example, in the form of particles. Only one solid electrolyte may be used alone, or two or more may be used in combination. The electrolyte may, for example, contain sodium ions as carrier ions. The electrolyte may be an aqueous electrolyte or a non-aqueous electrolyte. The composition of the electrolyte may be the same as the composition known as the electrolyte of a sodium ion secondary battery. For example, as an electrolyte, a product in which a sodium salt is dissolved at a specified concentration in a carbonate-based solvent can be used. As carbonate-based solvents, for example, fluoroethylene carbonate (FEC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), etc. may be listed. As sodium salts, for example, NaPF6 may be listed.
[0116] 3.1.3 Conductive additives
[0117] As the conductive aid that can be contained in the positive electrode active material layer 10, for example, carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), Ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel can be listed. The conductive aid can be, for example, in the form of particles or fibers, and its size is not particularly limited. The conductive aid can be used alone or in combination of two or more.
[0118] 3.1.4 Adhesives
[0119] As the binder that can be contained in the positive electrode active material layer 10, for example, butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. can be listed. Only one type of binder can be used alone, or two or more types can be used in combination.
[0120] 3.2 Electrolyte layer
[0121] The electrolyte layer 20 contains at least an electrolyte. When the sodium ion secondary battery 100 is a solid battery (a battery containing a solid electrolyte, which may be a battery in which a liquid electrolyte is used in part of the electrolyte, or a fully solid battery without a liquid electrolyte), the electrolyte layer 20 contains a solid electrolyte and may further optionally contain a binder, etc. In this case, there is no particular limitation on the content of the solid electrolyte and the binder, etc. in the electrolyte layer 20. On the other hand, when the sodium ion secondary battery 100 is an electrolyte battery, the electrolyte layer 20 contains an electrolyte, and may further have a diaphragm (separator) for preventing contact between the positive electrode active material layer 10 and the negative electrode active material layer 30 while maintaining the electrolyte. There is no particular limitation on the thickness of the electrolyte layer 20, for example, it may be 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.
[0122] As the electrolyte contained in the electrolyte layer 20, it can be appropriately selected from the electrolytes exemplified as the electrolytes that can be contained in the above-mentioned positive electrode active material layer 10. In addition, for the binder that can be contained in the electrolyte layer 20, it can be appropriately selected from the binders exemplified as the binders that can be contained in the above-mentioned positive electrode active material layer 10. Electrolytes and binders can be used alone or in combination of two or more. The separator can be any separator commonly used in sodium ion secondary batteries, for example, separators composed of resins such as polyethylene (PE), polypropylene (PP), polyester and polyamide can be listed. The separator can be a single-layer structure or a multi-layer structure. As a multi-layer structure separator, for example, a 2-layer structure separator of PE / PP, or a 3-layer structure separator of PP / PE / PP or PE / PP / PE can be listed. The separator can be composed of non-woven fabrics such as cellulose non-woven fabrics, resin non-woven fabrics, and glass fiber non-woven fabrics.
[0123] 3.3 Negative electrode active material layer
[0124] The negative electrode active material layer 30 contains at least a negative electrode active material, and further, may optionally contain an electrolyte, a conductive aid, a binder, etc. Furthermore, the negative electrode active material layer 30 may also contain various additives. The content of each of the negative electrode active material, electrolyte, conductive aid, binder, etc. in the negative electrode active material layer 30 can be appropriately determined according to the target battery performance. For example, when the entire negative electrode active material layer 30 (the entire solid component) is set to 100 mass%, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less or 90 mass% or less. There is no particular limitation on the shape of the negative electrode active material layer 30, for example, it may be a sheet-shaped negative electrode active material layer having a substantially flat surface. There is no particular limitation on the thickness of the negative electrode active material layer 30, for example, it may be 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.
[0125] As the negative electrode active material, various materials having a potential (charge and discharge potential) of absorbing and releasing sodium ions that is lower than that of the positive electrode active material of the present disclosure described above can be used. The negative electrode active material may be, for example, an inorganic negative electrode active material such as metallic sodium, a negative electrode active material composed of an organic compound, or a combination thereof. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be a general shape of a negative electrode active material for a battery. For example, the negative electrode active material may be in the form of particles. The negative electrode active material particles may be primary particles, or secondary particles formed by the aggregation of multiple primary particles. The average particle size (D50) of the negative electrode active material particles may be, for example, greater than 1 nm, greater than 5 nm, or greater than 10 nm, and may also be less than 500 μm, less than 100 μm, less than 50 μm, or less than 30 μm. Alternatively, the negative electrode active material may be in the form of a sheet (foil, film) such as sodium foil. That is, the negative electrode active material layer 30 may be composed of a sheet of negative electrode active material.
[0126] As the electrolyte that can be contained in the negative electrode active material layer 30, for example, the above-mentioned solid electrolyte, electrolyte solution or a combination thereof can be cited. As the conductive additive that can be contained in the negative electrode active material layer 30, the above-mentioned carbon material and the above-mentioned metal material can be cited. The binder that can be contained in the negative electrode active material layer 30 can be appropriately selected from the binders exemplified as the binders that can be contained in the above-mentioned positive electrode active material layer 10. The electrolyte and the binder can be used alone or in combination of two or more.
[0127] 3.4 Positive electrode collector
[0128] like Figure 2As shown, the sodium ion secondary battery 100 may include a positive electrode collector 40 in contact with the above-mentioned positive electrode active material layer 10. As for the positive electrode collector 40, any positive electrode collector generally used as a positive electrode collector of a battery can be adopted. In addition, the positive electrode collector 40 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, etc. The positive electrode collector 40 may be composed of a metal foil or a metal mesh. In particular, the metal foil has excellent handling properties. The positive electrode collector 40 may be composed of a plurality of foils. As metals constituting the positive electrode collector 40, Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel may be listed. In particular, from the perspective of ensuring oxidation resistance, etc., the positive electrode collector 40 may contain Al. For the purpose of adjusting resistance, etc., the positive electrode collector 40 may have some coating on its surface. In addition, the positive electrode current collector 40 may be a product obtained by plating or vapor-depositing the above-mentioned metal on a metal foil or a substrate. In addition, when the positive electrode current collector 40 is composed of a plurality of metal foils, some layers may be present between the plurality of metal foils. The thickness of the positive electrode current collector 40 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or less, and may be 1 mm or less or 100 μm or less.
[0129] 3.5 Negative electrode collector
[0130] like Figure 2 As shown, the sodium ion secondary battery 100 may include a negative electrode collector 50 in contact with the above-mentioned negative electrode active material layer 30. As for the negative electrode collector 50, any negative electrode collector generally used as a negative electrode collector of a battery can be used. In addition, the negative electrode collector 50 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, etc. The negative electrode collector 50 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, the metal foil has excellent handling properties. The negative electrode collector 50 may be composed of a plurality of foils and sheets. As metals constituting the negative electrode collector 50, Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, etc. may be listed. In particular, from the viewpoint of ensuring reduction resistance, etc., the negative electrode collector 50 may contain at least one metal selected from Cu, Ni and stainless steel. For the purpose of adjusting resistance, etc., the negative electrode collector 50 may have some coating on its surface. In addition, the negative electrode current collector 50 may be a product obtained by plating or vapor-depositing the above-mentioned metal on a metal foil or a substrate. In addition, when the negative electrode current collector 50 is composed of a plurality of metal foils, some layers may be present between the plurality of metal foils. The thickness of the negative electrode current collector 50 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or less, and may be 1 mm or less or 100 μm or less.
[0131] 3.6 Other matters
[0132] In addition to the above-mentioned structure, the sodium ion secondary battery 100 may include pole pieces, terminals, and other obvious structures of the secondary battery. As for the sodium ion secondary battery 100, each of the above-mentioned structures can be contained inside the outer packaging body. As for the outer packaging body, any outer packaging body known as the outer packaging body of the battery can be used. In addition, a plurality of batteries 100 are electrically connected arbitrarily, and can be optionally overlapped to form a battery group. In this case, the battery group can be contained inside a known battery casing. The sodium ion secondary battery 100 may also include obvious structures such as necessary terminals. As the shape of the sodium ion secondary battery 100, for example, a coin type, a laminated body type, a cylindrical type, and a square type can be listed.
[0133] The sodium ion secondary battery 100 can be manufactured by applying a known method in addition to using the above-mentioned specific positive electrode active material. For example, it can be manufactured as follows. However, the manufacturing method of the sodium ion secondary battery 100 is not limited to the following method, and each layer can be formed by dry molding, etc.
[0134] (1) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used at this time is not particularly limited, and water or various organic solvents can be used. The positive electrode layer slurry is applied to the surface of the positive electrode collector using a scraper or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode collector to prepare a positive electrode.
[0135] (2) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used at this time is not particularly limited, and water or various organic solvents can be used. The negative electrode layer slurry is applied to the surface of the negative electrode collector using a scraper or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode collector to prepare a negative electrode.
[0136] (3) The layers are stacked in such a way that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having a negative electrode collector, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer and a positive electrode collector in this order. Other components such as terminals are installed on the laminate as needed.
[0137] (4) The stack is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with an electrolyte, the stack is immersed in the electrolyte, and the stack is sealed in the battery case, thereby preparing a secondary battery. In the case of an electrolyte battery, in the above-mentioned stage (3), the negative electrode active material layer, the separator, and the positive electrode active material layer may contain an electrolyte.
[0138] 4. Method for increasing the weight energy density of sodium ion secondary batteries
[0139] The technology disclosed in the present invention also has an aspect as a method for increasing the weight energy density of a sodium ion secondary battery. That is, the method for increasing the weight energy density of a sodium ion secondary battery disclosed in the present invention is characterized in that the positive electrode active material disclosed in the present invention is used in the positive electrode active material layer of the sodium ion secondary battery.
[0140] 5. Vehicles with sodium-ion secondary batteries
[0141] As described above, the positive electrode active material of the present disclosure has excellent weight energy density and is suitable as a positive electrode active material for a sodium ion secondary battery. Such a sodium ion secondary battery with a large weight energy density can be preferably used in a vehicle selected from at least one of a hybrid vehicle (HEV), a plug-in hybrid vehicle (PHEV) and an electric vehicle (BEV). That is, the technology disclosed in the present disclosure also has the following aspects: a vehicle having a sodium ion secondary battery, the sodium ion secondary battery having a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, and the positive electrode active material layer includes the positive electrode active material disclosed above.
[0142] Example
[0143] As described above, an embodiment of a positive electrode active material and a sodium ion secondary battery, etc., has been described, and the technology disclosed herein can be variously modified beyond the above-mentioned embodiment without departing from the scope of its purpose. The following examples are shown to explain the technology disclosed herein in more detail, but the technology disclosed herein is not limited to the following examples.
[0144] 1. Preparation of positive electrode active material
[0145] 1.1 Example 1
[0146] 1.1.1 Preparation of precursor
[0147] (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed to obtain a target composition ratio and dissolved in distilled water to a concentration of 1.2 mol / L to obtain a first solution. In addition, Na2CO3 was dissolved in distilled water in another container to a concentration of 1.2 mol / L to obtain a second solution.
[0148] (2) 1000 mL of pure water was placed in a reaction container (with baffles), and 500 mL of the first solution and 500 mL of the second solution were each dropped therein at a rate of about 4 mL / min.
[0149] (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product.
[0150] (4) The product is washed with pure water, separated into solid and liquid using a centrifuge, and the precipitate is recovered.
[0151] (5) The obtained precipitate was dried at 120°C overnight, crushed in a mortar, and then fine particles were removed by air flow classification to obtain precursor particles. The precursor particles were composite salts containing Mn, Ni, and Co. The molar ratio of Mn to Ni to Co in the precursor particles was Mn:Ni:Co=4:3:3.
[0152] 1.1.2 Fabrication of the complex
[0153] Weigh the precursor particles and Na2CO3 so that Na 0.9 Mn 0.4 Ni 0.3 Co 0.3 The weighed precursor and Na2CO3 were mixed in a mortar to obtain a composite.
[0154] 1.1.3 Firing of the composite
[0155] The composite was placed in an alumina crucible and sintered in air atmosphere to obtain an oxide containing Na and having a P2 type structure. The sintering conditions were as described below (1) to (7).
[0156] (1) An alumina crucible containing the above-mentioned composite is placed in a heating furnace in an air atmosphere.
[0157] (2) The temperature in the heating furnace was raised from room temperature (25°C) to 600°C over 115 minutes.
[0158] (3) The temperature in the heating furnace is maintained at 600° C. for 360 minutes for preliminary calcination.
[0159] (4) After the pre-sintering, the temperature in the heating furnace is raised from 600°C to 900°C over 100 minutes.
[0160] (5) Maintain the temperature in the heating furnace at 900°C for 60 minutes to perform main sintering.
[0161] (6) After the main firing, the temperature in the heating furnace was lowered from 900°C to 250°C over 120 minutes.
[0162] (7) The alumina crucible was taken out of the heating furnace at 250°C and allowed to cool outside the furnace in a dry atmosphere to 25°C over 10 minutes.
[0163] The fired product after being cooled in air was pulverized in a dry atmosphere using a mortar to obtain Na-containing oxide particles having a P2 type structure.
[0164] 1.2 Example 2
[0165] The same method as in Example 1 was used except that the composition of the precursor particles and the feed ratio of the precursor particles to Na2CO3 were changed. In Example 2, the molar ratio of Mn, Ni, and Co in the precursor particles was set to Mn:Ni:Co=5:3:2. In addition, the precursor particles and Na2CO3 were weighed so that Na 0.8 Mn 0.5 Ni 0.3 Co 0.2 Feed composition of O2.
[0166] 1.3 Example 3
[0167] The same method as in Example 1 was used except that the composition of the precursor particles and the feed ratio of the precursor particles to Na2CO3 were changed. In Example 3, the molar ratio of Mn, Ni, and Co in the precursor particles was set to Mn:Ni:Co=4:2:4. In addition, the precursor particles and Na2CO3 were weighed so that Na 0.8 Mn 0.4 Ni 0.2 Co 0.4 Feed composition of O2.
[0168] 1.4 Comparative Example 1
[0169] The same method as in Example 1 was used except that the composition of the precursor particles and the feed ratio of the precursor particles to Na2CO3 were changed and the fine particles after air flow classification were used as the precursor particles. In Comparative Example 1, the molar ratio of Mn, Ni and Co in the precursor particles was set to Mn:Ni:Co=5:2:3. In addition, the precursor particles and Na2CO3 were weighed so that Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 Feed composition of O2.
[0170] 2. Evaluation of positive electrode active materials
[0171] 2.1 Elemental analysis
[0172] Elemental analysis was performed on each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1 to determine the chemical composition. The results are shown in Table 1 below.
[0173] 2.2 Determination of crystal structure based on X-ray diffraction
[0174] For each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1, X-ray diffraction measurement was performed using CuKα as a radiation source, and X-ray diffraction patterns were obtained. Figure 3 The X-ray diffraction patterns of Examples 1 to 3 are shown in FIG. Figure 4 The X-ray diffraction pattern of Comparative Example 1 is shown in FIG. Figure 3 and 4 As shown, it can be seen that all positive electrode active materials of Examples 1 to 3 and Comparative Example 1 have a P2-type structure belonging to the space group P63mc. In addition, the lattice constants (a-axis length, b-axis length, c-axis length) of each P2-type structure of Examples 1 to 3 and Comparative Example 1 were obtained from each X-ray diffraction pattern. The results are shown in Table 1 below.
[0175] 2.3 Determination of average particle size
[0176] The average particle size (D50) of each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1 was measured. The results are shown in Table 1 below.
[0177] 2.4 Determination of average aspect ratio based on SEM observation
[0178] Each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1 was formed into pellets, subjected to CP processing, and then cross-sectionally observed using FE-SEM to measure the average aspect ratio. The results are shown in Table 1 below. Figure 5 , a SEM image of the positive electrode active material according to Example 1 formed into a pellet shape and observed in cross section is shown. Figure 6 2 shows the appearance of the positive electrode active material according to Example 1.
[0179] 3. Preparation of battery cells for evaluation
[0180] A coin cell was fabricated using each of the positive electrode active materials of Examples 1 to 3 and Comparative Example 1. The fabrication procedure of the coin cell is as follows.
[0181] (1) The positive electrode active material, acetylene black (AB) as a conductive aid, and polyvinylidene fluoride (PVdF) as a binder were weighed so that the mass ratio was positive electrode active material: AB: PVdF = 85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode composite slurry. The positive electrode composite slurry was coated on an aluminum foil and vacuum dried at 120° C. overnight to obtain a positive electrode as a laminate of a positive electrode active material layer and a positive electrode collector.
[0182] (2) As the electrolyte solution, a solution prepared by dissolving NaPF 6 to a concentration of 1 M in a solvent in which EC and DEC were mixed at a volume ratio of 1:1 was used.
[0183] (3) As the negative electrode, a metal sodium foil was prepared.
[0184] (4) A coin battery (CR2032) was fabricated using a positive electrode, an electrolyte and a negative electrode.
[0185] 4. Evaluation of charge and discharge characteristics
[0186] The coin cells of Examples 1 to 3 and Comparative Example 1 were charged and discharged at 0.1 C (1 C = 160 mA / g) in a voltage range of 1.0 to 4.8 V in a thermostatic chamber maintained at 25° C. to measure the capacity. The results are shown in Table 2 below.
[0187] 5. Evaluation results
[0188] For each of Examples 1 to 3 and Comparative Example 1, the chemical composition, average particle size (D50), average aspect ratio and lattice constant of the positive electrode active material, and the initial discharge capacity, average discharge potential and gravimetric energy density of the evaluated battery cell are shown.
[0189]
Table 1
[0190] (Table 1)
[0191]
[0192]
Table 2
[0193] Table 2
[0194]
[0195] As shown in Tables 1 and 2, the positive electrode active materials of Examples 1 to 3, in which D50 is larger than 2.0 μm and the average aspect ratio is smaller than 3.0, have excellent weight energy density compared to the positive electrode active material of Comparative Example 1, in which D50 is smaller than 2.0 μm and the average aspect ratio is larger than 3.0. In addition, the initial discharge capacity and average discharge potential of the positive electrode active materials of Examples 1 to 3 are equal to or higher than those of Comparative Example 1.
[0196] In addition, from the results shown in Tables 1 and 2, it can be seen that the positive electrode active materials according to Examples 1 to 3 having a predetermined chemical composition have a superior weight energy density compared to the positive electrode active material according to Comparative Example 1 having a chemical composition different from that of Examples 1 to 3.
[0197] 6. Supplement
[0198] It should be noted that, in the above-mentioned embodiments, the case where the precursor is obtained by the coprecipitation method is illustrated, but the precursor can also be obtained by methods other than this. In addition, in the above-mentioned embodiments, the case where the surface of the precursor is coated with a Na source by spray drying to obtain a composite is illustrated, but the composite can also be obtained by methods other than this. In addition, in the above-mentioned embodiments, as the oxide containing Na having a P2 type structure, an oxide having a prescribed chemical composition is illustrated, but the chemical composition of the oxide containing Na is not limited thereto. In addition, the oxide containing Na can be doped with an element M other than Mn, Ni and Co. For the element M, as described in the embodiment.
[0199] 7. Summary
[0200] As described above, it can be said that in the positive electrode active material including the oxide containing Na, when the oxide containing Na satisfies the following characteristics (1-1) to (1-4), the energy density of the positive electrode active material increases.
[0201] (1-1) The Na-containing oxide particles have a P2 type structure.
[0202] (1-2) The Na-containing oxide particles contain at least one element of Mn, Ni, and Co, and Na and O as constituent elements.
[0203] (1-3) The Na-containing oxide particles have an average particle size of 2.0 μm or more.
[0204] (1-4) The Na-containing oxide particles have an average aspect ratio of 1.0 to 3.0.
[0205] In addition, it can also be said that in the positive electrode active material including an oxide containing Na, when the oxide containing Na satisfies the following characteristics (2-1) and (2-2), the energy density of the positive electrode active material increases.
[0206] (2-1) The Na-containing oxide particles have a P2 type structure.
[0207] (2-2) The oxide particles containing Na have a Mn x-p Ni y-q Co z-r M p+q+rO2 (wherein, 0.70<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) represented by a chemical composition.
Claims
1. A positive electrode active material, comprising oxide particles containing Na, wherein the oxide particles containing Na have a P2 type structure, wherein the oxide particles containing Na contain at least one element of Mn, Ni and Co, Na and O as constituent elements, the oxide particles containing Na have an average particle size of 2.0 μm or more, and the oxide particles containing Na have an average aspect ratio of 1.0 or more and 3.0 or less.
2. The positive electrode active material according to claim 1, wherein The Na-containing oxide particles contain more than 0.35 mol of Na per mol of O as a constituent element.
3. The positive electrode active material according to claim 1 or 2, wherein The oxide particles containing Na have a Mn x-p Ni y-q Co z-r M p+q+r The chemical composition represented by O2, wherein 0<a≤1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
4. The positive electrode active material according to any one of claims 1 to 3, wherein The oxide particles containing Na have a Mn x-p Ni y-q Co z-r M p+q+r O2 represents a chemical composition, wherein 0<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
5. The positive electrode active material according to any one of claims 1 to 4, wherein The oxide particles containing Na have a Mn x-p Ni y-q Co z-r M p+q+r O2 represents a chemical composition, wherein 0.70<a≤1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
6. A positive electrode active material comprising oxide particles containing Na, wherein the oxide particles containing Na have a P2-type structure, and the oxide particles containing Na have a structure composed of Na a Mn x-p Ni y-q Co z-r M p+q+r O2 represents the chemical composition, where 0.70<a≤1.00, 0<x<1.00, 0<y<0.50, 0<z<1.00, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
7. The positive electrode active material according to claim 6, wherein The oxide particles containing Na have a Mn x- p Ni y-q Co z-r M p+q+r O2 represents a chemical composition, wherein 0.70<a≤1.00, 0.30<x<0.60, 0.10<y<0.40, 0.10<z<0.50, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
8. The positive electrode active material according to any one of claims 1 to 7, wherein The P2 type structure has The following is the c-axis length. 9 . A sodium ion secondary battery comprising a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material according to claim 1 .