Method and system for preparing carbon nanotubes after deoxidizing coal bed gas
By combining chemical looping combustion and vapor deposition, and using a metal oxygen carrier and middlings coal for multiple deoxygenation treatments in a rotary kiln reactor, the impact of oxygen in coalbed methane on the quality and safety of carbon nanotubes was solved, achieving the preparation of high-quality and high-yield carbon nanotubes.
Patent Information
- Application Number
- CN202410874560.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-01
AI Technical Summary
Excessive oxygen content in coalbed methane can lead to quality and safety issues with carbon nanotubes. Existing technologies struggle to effectively remove oxygen to improve the quality and safety of carbon nanotube production.
A combination of chemical looping combustion and vapor deposition was used to deoxygenate coalbed methane through primary, secondary and tertiary deoxygenation using a metal oxygen carrier. The methane was then processed multiple times in a rotary kiln reactor using middlings coal and oxide catalysts, combined with centrifugation, sieving and acid washing operations, to prepare high-quality carbon nanotubes.
It effectively reduces the oxygen content in coalbed methane, improves the quality and production capacity of carbon nanotubes, reduces preparation costs, and ensures the safety of the preparation process.
Smart Images

Figure CN118877879A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of coalbed methane, and in particular to a method and system for preparing carbon nanotubes by deoxidizing coalbed methane. Background Art
[0002] Carbon nanotubes can be seen as a cylinder of graphene sheets, so they have excellent properties of graphite, such as heat resistance, corrosion resistance, thermal shock resistance, good heat transfer and electrical conductivity, high high temperature strength, self-lubricity and biocompatibility, etc. This makes it have a wide range of application prospects in the fields of energy, chemical and physical sensors, catalytic materials and composite materials.
[0003] In the method of preparing carbon nanotubes based on coalbed methane, when the coalbed methane contains too much oxygen, on the one hand, oxygen reacts with methane to cause explosion, and on the other hand, oxygen may affect the quality of the generated carbon nanotubes. Therefore, a method of preparing carbon nanotubes after deoxygenating coalbed methane is urgently needed to improve the quality and safety of the generated carbon nanotubes. Summary of the invention
[0004] This application proposes a method and system for preparing carbon nanotubes after deoxidizing coal bed gas. The specific scheme is as follows:
[0005] In one aspect, an embodiment of the present application provides a method for preparing carbon nanotubes after deoxidizing coal bed gas, comprising:
[0006] S1, selecting a first portion of washed medium coal, and crushing and screening the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range;
[0007] S2, selecting a second portion of the metal oxygen carrier and placing it into the rotary kiln reactor, introducing coalbed methane with a preset concentration and a preset volumetric space velocity, so as to perform primary deoxygenation on the coalbed methane by a chemical looping combustion method, reduce the oxygen content of the coalbed methane to below 3 vol%, and obtain the oxide of the metal oxygen carrier;
[0008] S3, placing the washed coal and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to less than 1 vol%;
[0009] S4, placing the washed medium coal in a rotary kiln reactor, introducing methane with a preset volumetric space velocity to purge the washed medium coal, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the washed medium coal, and then heating it to deoxidize the coalbed methane three times and obtain carbon nanotubes.
[0010] In a possible implementation of an embodiment of the present application, the washed medium coal includes washed medium coal of lignite, or includes washed medium coal of lignite and washed medium coal of long flame coal, the ratio of washed medium coal of lignite and washed medium coal of long flame coal is 1:m, and the value of m is [0-0.3]; the metal oxygen carrier includes Fe 2 O 3 , NiO and K 2 CO 3 , Fe 2 O 3 、NiO、K 2 CO 3 The molar ratio is 1:2:1; the ratio between the second portion and the first portion is 1:10; the initial oxygen content of the coalbed methane is 10%.
[0011] In a possible implementation of an embodiment of one aspect of the present application, washed medium coal is placed in a rotary kiln reactor, methane with a preset volumetric space velocity is introduced to purge the washed medium coal, and then coalbed methane is introduced, and an oxide is mixed evenly with the washed medium coal as a catalyst of a vapor deposition method, and then the temperature is increased to deoxidize the coalbed methane three times, and carbon nanotubes are obtained, including:
[0012] S401, placing the washed medium coal in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the washed medium coal, and then introducing coalbed methane, and mixing the oxide as a catalyst for a vapor phase deposition method with the washed medium coal, and then heating the mixture to deoxidize the coalbed methane three times to obtain a carbon nanotube mixture;
[0013] S402, centrifuging, screening and acid washing the carbon nanotube mixture to obtain pure carbon nanotubes.
[0014] In a possible implementation of an embodiment of one aspect of the present application, it also includes:
[0015] S5, placing the carbon nanotube mixture and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time to deoxygenate the coalbed methane;
[0016] S6, placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volume space velocity to purge the carbon nanotube mixture, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the carbon nanotube mixture, and then heating to purify the carbon nanotube mixture;
[0017] The process of S5-S6 is repeated multiple times to purify the carbon nanotube mixture.
[0018] Another aspect of the present application provides a system for preparing carbon nanotubes after deoxidizing coal bed gas, comprising:
[0019] A selection module is used to select the first portion of washed medium coal, and crush and screen the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range;
[0020] The primary deoxygenation module is used to select a second portion of metal oxygen carriers and put them into the rotary kiln reactor, and introduce coalbed methane with a preset concentration and a preset volume space velocity to perform primary deoxygenation on the coalbed methane by chemical loop combustion, thereby reducing the oxygen content of the coalbed methane to below 3 vol%, and obtaining oxides of the metal oxygen carriers;
[0021] The secondary deoxygenation module is used to place the washed coal and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, raise the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keep the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to less than 1 vol%;
[0022] The preparation module is used to place the washed coal in a rotary kiln reactor, introduce methane with a preset volumetric space velocity to purge the washed coal, and then introduce coalbed methane, and use the oxide as a catalyst for the vapor deposition method to mix evenly with the washed coal and then heat it to deoxidize the coalbed methane three times and obtain carbon nanotubes.
[0023] In a possible implementation of another aspect of the present application, the washed medium coal includes washed medium coal of lignite, or includes washed medium coal of lignite and washed medium coal of long flame coal, the ratio of washed medium coal of lignite and washed medium coal of long flame coal is 1:m, and the value of m is [0-0.3]; the metal oxygen carrier includes Fe 2 O 3 , NiO and K 2 CO 3 , Fe 2 O 3 、NiO、K 2 CO 3 The molar ratio is 1:2:1; the ratio between the second portion and the first portion is 1:10; the initial oxygen content of the coalbed methane is 10%.
[0024] In a possible implementation of another aspect of the present application, the preparation module is used to:
[0025] The washed coal is placed in a rotary kiln reactor, and methane with a preset volumetric space velocity is introduced to purge the washed coal, and then coalbed methane is introduced, and the oxide is mixed evenly with the washed coal as a catalyst for the vapor phase deposition method, and then the temperature is increased to deoxidize the coalbed methane three times to obtain a carbon nanotube mixture
[0026] The carbon nanotube mixture is subjected to centrifugation, sieving and acid washing operations to obtain pure carbon nanotubes.
[0027] In a possible implementation of another aspect of the present application, a purification module is further included, which is used to:
[0028] S5, placing the carbon nanotube mixture and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time to deoxygenate the coalbed methane;
[0029] S6, placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volume space velocity to purge the carbon nanotube mixture, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the carbon nanotube mixture, and then heating to purify the carbon nanotube mixture;
[0030] The process of S5-S6 is repeated multiple times to purify the carbon nanotube mixture.
[0031] Another aspect of the present application provides a computer device, including a processor and a memory;
[0032] The processor runs a program corresponding to the executable program code by reading the executable program code stored in the memory, so as to implement the method as described in the above embodiment.
[0033] Another aspect of the present application provides a computer-readable storage medium having a computer program stored thereon, wherein the program implements the method of the above embodiment when executed by a processor.
[0034] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0036] Figure 1 A schematic flow chart of a method for preparing carbon nanotubes by deoxidizing coal-bed methane provided in an embodiment of the present application;
[0037] Figure 2 A schematic flow chart of another method for preparing carbon nanotubes by deoxidizing coal bed gas provided in an embodiment of the present application;
[0038] Figure 3 A schematic diagram of the structure of a system for preparing carbon nanotubes after deoxidizing coalbed methane provided in an embodiment of the present application. DETAILED DESCRIPTION
[0039] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.
[0040] In the process of using coalbed methane to make carbon nanotubes, the oxygen in the coalbed methane may cause some negative effects. For example, the oxidation of carbon nanotubes causes changes in the shape, size and properties of carbon nanotubes, thereby affecting the performance and application of carbon nanotubes. Oxygen may also occupy space during the synthesis of carbon nanotubes, hindering the normal growth of carbon nanotubes. This leads to a decrease in the yield and quality of carbon nanotubes. Oxygen may also react with other gases in the coalbed methane to generate impurities, which may adhere to the surface of the carbon nanotubes and affect their purity and performance. Therefore, in the process of using coalbed methane to make carbon nanotubes, it is necessary to remove the oxygen in the coalbed methane to improve the quality and production capacity of carbon nanotubes.
[0041] The following describes a method for preparing carbon nanotubes after deoxidizing coalbed methane according to an embodiment of the present application with reference to the accompanying drawings.
[0042] Figure 1 A schematic flow chart of a method for preparing carbon nanotubes by deoxidizing coalbed methane provided in an embodiment of the present application.
[0043] The method for preparing carbon nanotubes after deoxidizing coalbed methane in an embodiment of the present application is performed by an apparatus for preparing carbon nanotubes after deoxidizing coalbed methane (hereinafter referred to as the preparation apparatus) provided in an embodiment of the present application to improve the quality, production capacity and safety of the prepared carbon nanotubes.
[0044] like Figure 1 As shown, the method for preparing carbon nanotubes after deoxidizing coal bed gas comprises:
[0045] Step 101, selecting a first portion of washed medium coal, and crushing and screening the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range.
[0046] The washed medium coal may include washed medium coal of lignite, or washed medium coal of lignite and washed medium coal of long flame coal, which is not limited in the present application.
[0047] In the present application, the washed medium coal can be crushed and screened to obtain the washed medium coal containing carbon nanotubes within a preset particle size range.
[0048] Step 102, select a second amount of metal oxygen carrier and put it into the rotary kiln reactor, introduce coalbed methane with a preset concentration and a preset volumetric space velocity, use chemical chain combustion to perform initial deoxygenation on the coalbed methane, reduce the oxygen content of the coalbed methane to below 3 vol%, and obtain the oxide of the metal oxygen carrier.
[0049] Among them, oxygen coal contains methane CH 4 , oxygen O 2 , Nitrogen N 2 . O in coalbed methane 2 The volume concentration is 10%, N 2 The volume concentration is 20%, CH 4 The volume concentration is 70%. The metal oxygen carrier may include one or more metal oxides, such as Fe2O3, NiO and K2CO3, etc., which is not limited in the present application.
[0050] In the present application, the metal oxygen carrier can be placed in a rotary kiln reactor and introduced into the reactor at a preset concentration (e.g., 10%) and a volume space velocity (e.g., 100-500 h -1 ) of coal bed gas. Afterwards, a chemical chain combustion reaction is performed to initially deoxygenate the coal bed gas. The temperature of the metal oxygen carrier chemical chain combustion reaction can be 100-250°C.
[0051] The metal oxygen carrier is oxidized by oxygen in coalbed methane at high temperature (i.e., the oxygen vacancies generated on the surface of the metal oxide can react with O in coalbed methane). 2 The oxygen in the coalbed methane can be effectively removed and the side reaction between methane and oxygen can be reduced. After the initial deoxygenation of the coalbed methane, the oxygen in the coalbed methane can be reduced to less than 3 vol%. This ensures the safety of the use of coalbed methane.
[0052] Step 103, placing the washed coal and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to below 1 vol%.
[0053] In the present application, the washed coal and the coalbed methane after the initial deoxygenation in step 102 are placed in a rotary kiln reactor as raw materials. Thereafter, the rotary kiln reactor is rotated at a speed of 10-100r / min, and the temperature of the rotary kiln reactor is increased to a preset deoxygenation temperature (e.g., 70-120°C) at a preset heating rate (e.g., 3°C / min), and is kept at a constant temperature for a preset time at the preset deoxygenation temperature to reduce the oxygen in the coalbed methane to below 1 vol%, thereby obtaining coalbed methane mainly composed of methane.
[0054] In the present application, the metal oxygen carrier comprises Fe2 O 3 , NiO and K 2 CO 3 When Fe 2 O 3 、NiO、K 2 CO 3 The molar ratio of the washed coal can be 1:2:1. The ratio of the washed coal of lignite and the washed coal of long flame can be 1:m, and the value of m is [0-0.3]. When the initial oxygen content of the coalbed methane is 10%, the ratio of the second portion of the metal oxygen carrier to the first portion of the washed coal (the mass ratio of the metal oxygen carrier to the washed coal) can be 1:10.
[0055] Step 104, placing the washed coal in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the washed coal, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the washed coal and then heating it to deoxidize the coalbed methane three times and obtain carbon nanotubes.
[0056] In the present application, methane with a preset volumetric space velocity can be introduced into the rotary kiln reactor where the washed coal is located to purge the washed coal and remove the residual CO in the washed coal. 2 and CO to improve the quality of washed coal. -1 The secondary deoxidized coal bed gas is introduced into the rotary kiln reactor at a volume space velocity of , and the oxide obtained after the treatment in step 102 is placed into the rotary kiln reactor. Then, the oxide and the washed coal are mixed evenly and heated to prepare carbon nanotubes by a 900°C vapor deposition method.
[0057] During the heating process, the residual oxygen in the coalbed methane etches the amorphous carbon for the third deoxidation, reducing the residual oxygen in the deoxidized coalbed methane to below 0.5%, and the oxides are reduced by the washed coal to form a carbon nanotube catalyst with catalytic activity. Under the action of this catalyst, CH 4 The coal is washed and elongated to obtain a carbon nanotube mixture while being cracked into carbon nanotubes. Afterwards, the carbon nanotube mixture can be centrifuged and / or screened and / or acid-washed to obtain pure carbon nanotubes.
[0058] It is understandable that in the process of preparing carbon nanotubes, the oxides need to be mixed evenly with the washed coal and heated. If the amount of oxides used is large, it is difficult to drive the rotary kiln reactor to rotate, and the energy consumption is large. Therefore, secondary deoxidation of coalbed methane effectively reduces the oxygen content in coalbed methane, thereby reducing the amount of metal oxygen carriers used in the preparation of carbon nanotubes, thereby effectively reducing costs.
[0059] In addition, because washed coal contains ash (the components of ash are sodium oxide and potassium oxide), in the process of preparing carbon nanotubes, washed coal can not only be used to deoxidize coalbed methane, but also act as a catalyst and grow carbon nanotubes, thereby improving the quality and production capacity of carbon nanotubes and reducing costs.
[0060] Furthermore, the metal oxygen carrier is oxidized and reduced during the process of preparing carbon nanotubes and can be reused, thereby improving resource utilization and reducing costs.
[0061] In the present application, a first portion of washed medium coal is selected, and the washed medium coal is crushed and sieved to obtain washed medium coal containing carbon nanotubes in a preset particle size range, and a second portion of metal oxygen carrier is selected and placed in a rotary kiln reactor, and coalbed methane with a preset concentration and a preset volumetric space velocity is introduced to perform primary deoxygenation of the coalbed methane by chemical chain combustion, so that the oxygen content of the coalbed methane is reduced to less than 3 vol%, and the oxide of the metal oxygen carrier is obtained, and then the washed medium coal and coalbed methane are placed as raw materials in a rotary kiln reactor at a preset temperature. , the temperature of the rotary kiln reactor is raised to the preset deoxygenation temperature at a preset heating rate, and the preset deoxygenation temperature is kept constant for a preset time to perform secondary deoxygenation on the coalbed methane, and the oxygen content of the coalbed methane is reduced to below 1 vol%. Then, the washed medium coal is placed in the rotary kiln reactor, and the washed medium coal is purged with methane at a preset volumetric space velocity, and then the coalbed methane is introduced, and the oxide is mixed with the washed medium coal as a catalyst for the vapor phase deposition method and then heated to perform tertiary deoxygenation on the coalbed methane and obtain carbon nanotubes. Thus, after the safety of the use of coalbed methane is ensured by the initial deoxygenation of the coalbed methane, the washed medium coal is used to perform secondary and tertiary deoxygenation on the coalbed methane, avoiding the influence of oxygen on the quality of the preparation of carbon nanotubes. In the process of preparing carbon nanotubes, the washed medium coal plays a catalytic role and grows the tube at the same time. Thus, while improving the quality, production capacity and safety of carbon nanotubes, the cost is reduced.
[0062] Figure 2 A schematic flow chart of a method for preparing carbon nanotubes by deoxidizing coalbed methane provided in an embodiment of the present application.
[0063] like Figure 2 As shown, the method for preparing carbon nanotubes after deoxidizing coal bed gas comprises:
[0064] Step 201, select the first portion of washed medium coal, and crush and screen the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range.
[0065] Step 202, select a second amount of metal oxygen carrier and put it into the rotary kiln reactor, introduce coalbed methane with a preset concentration and a preset volumetric space velocity, use chemical chain combustion to perform initial deoxygenation on the coalbed methane, reduce the oxygen content of the coalbed methane to below 3 vol%, and obtain the oxide of the metal oxygen carrier.
[0066] Step 203, placing the washed coal and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to below 1 vol%.
[0067] In the present application, the specific implementation process of steps 201 to 203 can be found in the detailed description of any embodiment of the present application and will not be repeated here.
[0068] Step 204, placing the washed coal in a rotary kiln reactor, introducing methane with a preset volumetric space velocity to purge the washed coal, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor deposition method with the washed coal, and then heating it to deoxidize the coalbed methane three times to obtain a carbon nanotube mixture.
[0069] In the present application, the carbon nanotube mixture contains not only carbon nanotubes but also impurities such as ash.
[0070] Step 205, placing the carbon nanotube mixture and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time to deoxygenate the coalbed methane.
[0071] Among them, coalbed methane refers to the coal gas layer after initial deoxygenation.
[0072] In the present application, the process of "placing the carbon nanotube mixture and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time" can be referred to the process of "placing the washed coal and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time", which will not be repeated here.
[0073] Step 206, placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the carbon nanotube mixture, then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the carbon nanotube mixture and then heating to purify the carbon nanotube mixture.
[0074] In the present application, the process of "placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the carbon nanotube mixture, then introducing coalbed methane, and mixing the oxide with the carbon nanotube mixture as a catalyst for vapor deposition method and then heating the mixture" can be referred to the process of "placing the washed coal in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the washed coal, then introducing coalbed methane, and mixing the oxide with the washed coal as a catalyst for vapor deposition method and then heating the mixture" in the present application, which will not be repeated here.
[0075] In the present application, the process of step 205 to step 206 may be repeated multiple times, so that the content of carbon nanotubes is continuously accumulated, thereby improving the quality of carbon nanotubes.
[0076] Step 207 , centrifuging, screening and acid washing the carbon nanotube mixture to obtain pure carbon nanotubes.
[0077] In the present application, the carbon nanotube mixture can be centrifuged, screened and acid-washed to remove impurities in the carbon nanotube mixture and obtain pure carbon nanotubes. The acid used in the acid-washing process can be 1 mol / L HCL.
[0078] In order to better understand the method of preparing carbon nanotubes after deoxidizing coal bed gas in the present application, the following examples are provided for illustration:
[0079] (1) selecting 100 parts of washed medium coal A with a ratio of lignite to long bituminous coal of 1:0.1, crushing and screening the washed medium coal A to obtain washed medium coal A within a preset particle size range;
[0080] (2) Select 10 parts of Fe 2 O 3 , NiO and K 2 CO 3 The oxygen carrier B with a molar ratio of 1:2:1 was put into the rotary kiln reactor 1 for 200h -1 or 500h -1 The volume space velocity of coalbed methane C (O in coalbed methane C) 2 The volume concentration is 10%, N 2 The volume concentration is 20%, CH 4 The gas C is in contact with oxygen carrier B at a volume concentration of 70%, and the chemical loop combustion is used for the initial deoxidation process. When the chemical loop combustion occurs in the coalbed methane C, the oxygen in the coalbed methane C reacts preferentially with the oxygen carrier B at 150°C or 250°C, and the oxygen vacancies generated on the surface of the metal oxide can react with O 2It occurs rapidly, enabling the coalbed methane C to undergo a deoxygenation reaction first and reducing the occurrence of the side reaction between methane and oxygen. The primary deoxygenation process reduces the oxygen in the coalbed methane from 10 vol% to below 3 vol%, obtaining partially deoxygenated coalbed methane D, coal ash E and oxides of the oxygen carrier B;
[0081] (3) Select the washed coal A in step (1) and the partially deoxygenated coalbed methane D obtained in step (2) as raw materials and heat them for 10000 h. -1 The volume space velocity is placed in the rotary kiln reactor 2 with an initial temperature of 20°C and a rotation speed of 10r / min for secondary deoxygenation reaction, and the temperature is raised to 100°C at a heating rate of 3°C / min and kept at this temperature for a period of time to make the O in the coalbed methane 2 Reduced to below 1 vol%, the deoxygenated coalbed gas F, washed coal G and water vapor H, which are mainly methane, are obtained;
[0082] (4) The washed medium coal G obtained in step (3) is placed in the rotary kiln reactor 2 and introduced at a volume space velocity of 1000 h -1 The methane I is used to purge the residual CO in the rotary kiln reactor 2. 2 After the purge is completed, the gas -1 The deoxygenated coalbed methane F obtained in step (3) is introduced at a volume space velocity of 1.50 g / cm2. The washed medium coal G obtained is used as a raw material. The oxide of the oxygen carrier B in step (2) is put into the reactor. The oxide of the oxygen carrier B is mixed evenly with the washed medium coal G as a catalyst for the vapor deposition method and then heated. During the heating process, the oxide of the oxygen carrier B is reduced by the washed medium coal G to form a carbon nanotube catalyst with catalytic activity. The 900°C vapor deposition method cracks CH 4 Preparation of carbon nanotubes and hydrogen process, using the residual O in deoxygenated coalbed methane F 2 Etching amorphous carbon for the third deoxidation, so that the residual O 2 The carbon nanotubes J (i.e., carbon nanotubes) and CH 4 Cracking to obtain hydrogen K;
[0083] (5) The coal-based carbon nanotubes J obtained in step (4) are used as the raw material to replace the washed coal A in step (3) to repeat the process of step (3) and step (4). The process is repeated 1-3 times to accumulate the carbon nanotube content. Finally, relatively pure coal-based carbon nanotubes N and ash O are obtained by centrifugation, screening and acid washing with 1 mol / L HCL.
[0084] In order to implement the above embodiment, the embodiment of the present application also proposes a system for preparing carbon nanotubes after deoxidizing coalbed methane. Figure 3A schematic diagram of the structure of a system for preparing carbon nanotubes after deoxidizing coalbed methane provided in an embodiment of the present application.
[0085] like Figure 3 As shown, the system 300 for preparing carbon nanotubes after deoxidizing coal bed gas includes:
[0086] A selection module 310 is used to select the first portion of washed medium coal, and crush and screen the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range;
[0087] The primary deoxygenation module 320 is used to select a second portion of metal oxygen carriers and put them into the rotary kiln reactor, and introduce coalbed methane with a preset concentration and a preset volumetric space velocity to perform primary deoxygenation on the coalbed methane by chemical loop combustion, so as to reduce the oxygen content of the coalbed methane to below 3 vol%, and obtain oxides of the metal oxygen carriers;
[0088] The secondary deoxygenation module 330 is used to place the washed coal and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, raise the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keep the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to less than 1 vol%;
[0089] Preparation module 340 is used to place the washed coal in a rotary kiln reactor, introduce methane with a preset volumetric space velocity to purge the washed coal, and then introduce coalbed methane, and mix the oxide as a catalyst for the vapor deposition method with the washed coal and then heat it to deoxidize the coalbed methane three times and obtain carbon nanotubes.
[0090] In a possible implementation of the embodiment of the present application, the washed medium coal includes lignite washed medium coal, or includes lignite washed medium coal and long flame coal washed medium coal, the ratio of lignite washed medium coal to long flame coal washed medium coal is 1:m, and the value of m is [0-0.3]; the metal oxygen carrier includes Fe 2 O 3 , NiO and K 2 CO 3 , Fe 2 O 3 、NiO、K 2 CO 3 The molar ratio of the second portion is 1:2:1; the ratio between the second portion and the first portion is 1:10; the initial oxygen content of the coalbed methane is 10%.
[0091] In a possible implementation of the embodiment of the present application, the preparation module 340 is used to:
[0092] The washed medium coal is placed in a rotary kiln reactor, and methane with a preset volumetric space velocity is introduced to purge the washed medium coal, and then coalbed methane is introduced, and the oxide is mixed evenly with the washed medium coal as a catalyst for the vapor deposition method, and then the temperature is increased to deoxidize the coalbed methane three times to obtain a carbon nanotube mixture;
[0093] The carbon nanotube mixture is subjected to centrifugation, sieving and acid washing operations to obtain pure carbon nanotubes.
[0094] In a possible implementation of the embodiment of the present application, a purification module is also included, which is used to:
[0095] S5, placing the carbon nanotube mixture and coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time to deoxygenate the coalbed methane;
[0096] S6, placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the carbon nanotube mixture, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the carbon nanotube mixture, and then heating to purify the carbon nanotube mixture;
[0097] The process of S5-S6 is repeated multiple times to purify the carbon nanotube mixture.
[0098] It should be noted that the above explanation of the method embodiment for preparing carbon nanotubes after deoxidizing coalbed methane is also applicable to the system for preparing carbon nanotubes after deoxidizing coalbed methane in this embodiment, so it will not be repeated here.
[0099] In the present application, a first portion of washed medium coal is selected, and the washed medium coal is crushed and sieved to obtain washed medium coal containing carbon nanotubes in a preset particle size range, and a second portion of metal oxygen carrier is selected and placed in a rotary kiln reactor, and coalbed methane with a preset concentration and a preset volumetric space velocity is introduced to perform primary deoxygenation of the coalbed methane by chemical chain combustion, so that the oxygen content of the coalbed methane is reduced to less than 3 vol%, and the oxide of the metal oxygen carrier is obtained, and then the washed medium coal and coalbed methane are placed as raw materials in a rotary kiln reactor at a preset temperature. , the temperature of the rotary kiln reactor is raised to the preset deoxygenation temperature at a preset heating rate, and the preset deoxygenation temperature is kept constant for a preset time to perform secondary deoxygenation on the coalbed methane, and the oxygen content of the coalbed methane is reduced to below 1 vol%. Then, the washed medium coal is placed in the rotary kiln reactor, and the washed medium coal is purged with methane at a preset volumetric space velocity, and then the coalbed methane is introduced, and the oxide is mixed with the washed medium coal as a catalyst for the vapor phase deposition method and then heated to perform tertiary deoxygenation on the coalbed methane and obtain carbon nanotubes. Thus, after the safety of the use of coalbed methane is ensured by the initial deoxygenation of the coalbed methane, the washed medium coal is used to perform secondary and tertiary deoxygenation on the coalbed methane, avoiding the influence of oxygen on the quality of the preparation of carbon nanotubes. In the process of preparing carbon nanotubes, the washed medium coal plays a catalytic role and grows the tube at the same time. Thus, while improving the quality, production capacity and safety of carbon nanotubes, the cost is reduced.
[0100] In order to implement the above embodiment, the embodiment of the present application also proposes a computer device, including a processor and a memory;
[0101] The processor runs a program corresponding to the executable program code by reading the executable program code stored in the memory, so as to implement the method for preparing carbon nanotubes after deoxidizing coalbed methane as described in the above embodiment.
[0102] In order to implement the above embodiments, the embodiments of the present application also propose a computer-readable storage medium on which a computer program is stored. When the program is executed by a processor, the method for preparing carbon nanotubes after deoxidizing coalbed methane as described in the above embodiments is implemented.
[0103] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A method for preparing carbon nanotubes by deoxidizing coal bed gas, characterized in that: include: S1, selecting a first portion of washed medium coal, and crushing and screening the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range; S2, selecting a second portion of metal oxygen carriers and placing them into a rotary kiln reactor, introducing coalbed methane with a preset concentration and a preset volumetric space velocity, so as to perform primary deoxygenation on the coalbed methane by a chemical looping combustion method, reduce the oxygen content of the coalbed methane to below 3 vol%, and obtain the oxide of the metal oxygen carrier; S3, placing the washed coal and the coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to less than 1 vol%; S4, placing the washed coal in a rotary kiln reactor, introducing methane with a preset volumetric space velocity to purge the washed coal, and then introducing the coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the washed coal, and then heating the mixture to deoxidize the coalbed methane three times and obtain carbon nanotubes.
2. The method according to claim 1, characterized in that The washed medium coal includes washed medium coal of lignite, or includes washed medium coal of lignite and washed medium coal of long flame coal, the ratio of the washed medium coal of lignite and the washed medium coal of long flame coal is 1:m, and the value of m is [0-0.3]; the metal oxygen carrier includes Fe2O3, NiO and K2CO3, and the molar ratio of Fe2O3, NiO and K2CO3 is 1:2:1; the ratio between the second portion and the first portion is 1:10; the initial oxygen content of the coalbed methane is 10%.
3. The method according to claim 1, characterized in that The washed coal is placed in a rotary kiln reactor, methane with a preset volume space velocity is introduced to purge the washed coal, and then the coalbed methane is introduced, and the oxide is used as a catalyst for the vapor phase deposition method and mixed evenly with the washed coal, and then the temperature is increased to deoxidize the coalbed methane three times and obtain carbon nanotubes, including: S401, placing the washed coal in a rotary kiln reactor, introducing methane at a preset volumetric space velocity to purge the washed coal, and then introducing the coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the washed coal, and then heating the mixture to deoxidize the coalbed methane three times to obtain a carbon nanotube mixture; S402, centrifuging, screening and acid washing the carbon nanotube mixture to obtain pure carbon nanotubes.
4. The method according to claim 3, characterized in that Also includes: S5, placing the carbon nanotube mixture and the coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time to deoxygenate the coalbed methane; S6, placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volume space velocity to purge the carbon nanotube mixture, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the carbon nanotube mixture, and then heating to purify the carbon nanotube mixture; The process of S5 to S6 is repeated multiple times to purify the carbon nanotube mixture.
5. A system for preparing carbon nanotubes after deoxidizing coal bed gas, characterized in that: include: A selection module is used to select a first portion of washed medium coal, and crush and screen the washed medium coal to obtain washed medium coal containing carbon nanotubes within a preset particle size range; A primary deoxygenation module is used to select a second portion of metal oxygen carriers and put them into a rotary kiln reactor, and introduce coalbed methane with a preset concentration and a preset volumetric space velocity to perform primary deoxygenation on the coalbed methane by a chemical loop combustion method, thereby reducing the oxygen content of the coalbed methane to below 3 vol%, and obtaining oxides of the metal oxygen carriers; A secondary deoxygenation module is used to place the washed coal and the coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, raise the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keep the temperature at the preset deoxygenation temperature for a preset time to perform secondary deoxygenation on the coalbed methane and reduce the oxygen content of the coalbed methane to less than 1 vol%; The preparation module is used to place the washed coal in a rotary kiln reactor, introduce methane with a preset volumetric space velocity to purge the washed coal, and then introduce the coalbed methane, and mix the oxide as a catalyst for the vapor deposition method with the washed coal and then heat it to deoxidize the coalbed methane three times and obtain carbon nanotubes.
6. The system according to claim 5, characterized in that The washed medium coal includes washed medium coal of lignite, or includes washed medium coal of lignite and washed medium coal of long flame coal, the ratio of the washed medium coal of lignite and the washed medium coal of long flame coal is 1:m, and the value of m is [0-0.3]; the metal oxygen carrier includes Fe2O3, NiO and K2CO3, and the molar ratio of Fe2O3, NiO and K2CO3 is 1:2:1; the ratio between the second portion and the first portion is 1:10; the initial oxygen content of the coalbed methane is 10%.
7. The system according to claim 5, characterized in that The preparation module is used for: The washed coal is placed in a rotary kiln reactor, methane with a preset volumetric space velocity is introduced to purge the washed coal, and then the coalbed methane is introduced, and the oxide is mixed evenly with the washed coal as a catalyst for the vapor deposition method, and then the temperature is increased to deoxidize the coalbed methane three times to obtain a carbon nanotube mixture; The carbon nanotube mixture is centrifuged, screened and acid-washed to obtain pure carbon nanotubes.
8. The system according to claim 7, characterized in that Also includes a purification module for: S5, placing the carbon nanotube mixture and the coalbed methane as raw materials in a rotary kiln reactor at a preset temperature, heating the temperature of the rotary kiln reactor to a preset deoxygenation temperature at a preset heating rate, and keeping the temperature at the preset deoxygenation temperature for a period of time to deoxygenate the coalbed methane; S6, placing the carbon nanotube mixture in a rotary kiln reactor, introducing methane at a preset volume space velocity to purge the carbon nanotube mixture, and then introducing coalbed methane, and mixing the oxide as a catalyst for the vapor phase deposition method with the carbon nanotube mixture, and then heating to purify the carbon nanotube mixture; The process of S5 to S6 is repeated multiple times to purify the carbon nanotube mixture.
9. A computer device, characterized in that: including a processor and a memory; The processor runs a program corresponding to the executable program code by reading the executable program code stored in the memory, so as to implement the method according to any one of claims 1 to 4.
10. A computer-readable storage medium having a computer program stored thereon, characterized in that: When the program is executed by a processor, the method according to any one of claims 1 to 4 is implemented.
Citation Information
Patent Citations
Coal-based carbon nanotube for deoxidizing low-concentration coalbed methane and preparation and purification method thereof
CN110713179A
Method for preparing multi-walled carbon nanotubes by deoxidizing coalbed methane
CN110921653A
Deoxidation method and deoxidation system for low-concentration coal bed gas
CN114907892A
Comprehensive utilization method of coal bed gas and middling coal
CN118240600A
Process for catalytic deoxygenation of coal mine methane
US20120003132A1
Cited By
Carbon nanotube based on combustion flame heat source and coal bed gas concerted catalysis and controllable growth method and application thereof
CN120817595A
Carbon nanotubes based on combustion flame heat source and coal bed gas synergistic catalysis and controllable growth method and application thereof
CN120817595B