A method for improving low temperature steel inclusions
Patent Information
- Application Number
- CN202411386728.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-30
Smart Images

Figure CN118879979B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving inclusions in steel, in particular to a method for improving inclusions in low-temperature steel. Background Art
[0002] Inclusions will inevitably form during the steel smelting process, and then they can act as modified inclusions after adding different rare earth elements. When producing rare earth steel, adding excessive rare earth elements can easily cause nozzle nodules during the continuous casting process, making it impossible to produce smoothly, thus restricting the high-quality development of rare earth steel. In addition, for specific steel grades, reasonable addition methods and stable yield control can effectively modify inclusions and improve steelmaking quality. Further improve the defects in the performance of specific steel grades, thereby achieving stable and efficient industrial production.
[0003] In order to solve the problem of inclusions deteriorating steel quality, the existing technical method is to appropriately reduce the amount of rare earth added, and after adding trace amounts of high-abundance rare earth elements, the inclusions are fully modified to reduce their harm to the molten steel. The disadvantage is that it is limited to adding trace amounts of rare earth elements, and the actual application effect fluctuates; the addition of trace rare earth elements fails to significantly improve the mechanical properties of the finished steel, and the actual effect is limited.
[0004] The invention patent with publication number CN113416813A, named "A method for controlling the addition of rare earth alloys to rare earth structural steel", proposes to control the rare earth addition method, addition timing, molten steel cleanliness and protective casting in the rare earth structural steel produced by the hot metal desulfurization-converter-LF furnace-continuous casting process to improve the recovery rate of rare earth in steel. This method only considers the rare earth addition process to improve the recovery rate of rare earth, which may not be enough to effectively modify the inclusions in the molten steel.
[0005] The invention patent with publication number CN106521293A, named "A method for improving performance by adding rare earth metals to steel", proposes a method of adding high-purity rare earth alloys to control the formation of inclusions of different sizes, thereby improving the stability of performance. This method does not take into account the price increase of high-purity rare earth alloys and the actual conditions of industrial production, and is not conducive to the industrial production of rare earth steel and the control of inclusion morphology by trace rare earths. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention provides a method for improving inclusions in low-temperature steel, aiming to reduce the size of inclusions in low-temperature steel, refine grains and thus improve the performance of low-temperature steel.
[0007] One of the purposes of the present invention is to provide a method for improving low temperature steel inclusions, comprising the following steps:
[0008] 1) After RH vacuum treatment for 3-5 minutes, add Ce-La rare earth alloy, the amount of Ce-La added is 0.0006-0.0009% based on the total mass of molten steel;
[0009] 2) Re-pressurize the RH vacuum furnace, add Ce-La rare earth alloy again after soft blowing for 5-10 minutes, and the amount of Ce-La added is 0.0004-0.0006% based on the total mass of molten steel;
[0010] 3) The RH vacuum furnace is re-pressurized and soft blowing treatment is continued. Ce-La rare earth alloy is added again 3-5 minutes before tapping. The amount of Ce-La added is 0.0003-0.0005% based on the total mass of molten steel. After the RH treatment is completed, the tapping operation is carried out.
[0011] As a preferred embodiment of the method for improving low-temperature steel inclusions of the present invention, the method further comprises a continuous casting step, during which the superheat of the molten steel is controlled to be 30-40° C. and the casting speed is 1.2-1.4 m / min.
[0012] As a preferred embodiment of the method for improving low-temperature steel inclusions of the present invention, the method also includes a hot rolling step, during which the heating temperature is controlled to be 1200-1250°C, the heating time is 2.5-4h, the rough rolling and final rolling temperatures are ≤1080°C, the finishing rolling start temperature is 980-1050°C, the final rolling temperature is 850-870°C, and the steel plate is rolled to a thickness of 8-12mm and then furnace cooled to 580-600°C for coiling.
[0013] As a preferred embodiment of the method for improving low-temperature steel inclusions of the present invention, the method also includes a quenching step, during which the first quenching heating temperature is controlled to be 860-880°C, the holding time is 1-1.5h, and water cooling, and the second quenching heating temperature is controlled to be 710-730°C, the holding time is 1-1.5h, and water cooling.
[0014] As a preferred embodiment of the method for improving low-temperature steel inclusions of the present invention, the method further comprises a tempering step. During the tempering process, the tempering heating temperature is controlled to be 570-580°C, the holding time is 1.5-2h, and the furnace is cooled.
[0015] As a preferred embodiment of the method for improving low-temperature steel inclusions of the present invention, the low-temperature steel composition includes, by mass, C 0.17-0.19%, Si 0.1-0.2%, Mn 1.35-1.55%, P≤0.01%, S≤0.005%, Ti 0.014-0.02%, and the balance is Fe and unavoidable impurities.
[0016] As a preferred solution of the method for improving low-temperature steel inclusions of the present invention, the rare earth alloy includes Ce-Fe alloy and La-Fe alloy, and the mass ratio of Ce-La in the rare earth alloy is 4-5:5-6.
[0017] As a preferred embodiment of the method for improving low temperature steel inclusions of the present invention, the oxygen activity in the molten steel is controlled to be ≤2.5×10 -6 .
[0018] Based on the thermodynamic and kinetic characteristics of inclusion formation during RH treatment, the present invention creatively finds that by adding an appropriate amount of Ce-La composite rare earth to the RH vacuum furnace in stages, the size of inclusions in steel can be effectively reduced. According to experimental results, the reason for the above effect may be that the segmented addition of rare earth elements can effectively form nucleation points of appropriate content to promote the reduction of inclusion size. In addition, the appropriate Ce-La rare earth content can effectively achieve the modification of inclusions on the one hand, and on the other hand, it can effectively avoid the growth of rare earth inclusions caused by excessive concentration. Based on the system of the present invention, it is more appropriate to divide the addition method of Ce-La composite rare earth alloy into three stages. Among them, the purpose of adding rare earth in the first stage of RH vacuum treatment for 3-5min is to reduce the oxygen activity in the RH vacuum furnace. In this stage, if the amount of rare earth added is less than 0.0006%, the inclusions will be easily aggregated and grown due to insufficient nucleation points of inclusions; when the amount added is higher than 0.0009%, the rare earth inclusions will grow due to excessive rare earth elements. The purpose of adding rare earth alloy in the second stage 5-10 minutes after re-pressing and soft blowing is to ensure that the reaction between the inclusion elements and rare earth in the first stage is sufficient to improve the use effect of the rare earth alloy in the first stage. If the amount of rare earth added is less than 0.0004% in this stage, the modification effect of inclusions is not good, but if it is higher than 0.0006%, the inclusion size will also increase. The purpose of adding rare earth alloy in the third stage 3-5 minutes before steelmaking is to ensure that the rare earth added for the third time can react fully.
[0019] In addition, other parameters involved in the steelmaking and RH treatment processes may be common parameters in the art, and will not be described in detail in the present invention.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention adds a proper amount of rare earth alloy into the RH vacuum furnace in stages, which can increase the use amount of rare earth and improve the shape of inclusions in steel by transforming irregular granular inclusions into ellipsoidal inclusions. On the other hand, it can effectively reduce the size of inclusions, and the particle size of the obtained rare earth inclusions reaches the nanometer level, which can effectively refine the grains. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1Transmission electron microscope image of the low-temperature steel microstructure obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] The technical solution of the present invention will be described in detail below through specific embodiments. It should be noted that the following embodiments are only used to help understand the technical solution and concept of the present invention, and are not just the technical scope that needs to be protected by the present invention. For those skilled in the art, the solutions that can be obtained based on the following embodiments without creative work all fall within the scope that needs to be protected by the present invention.
[0024] Example 1
[0025] A method for improving inclusions in low-temperature steel, wherein the components of the low-temperature steel are, by mass, C 0.18%, Si 0.2%, Mn 1.35%, P 0.005%, S 0.005%, Ti 0.017%, and the balance is Fe and unavoidable impurities, and the method comprises the following steps:
[0026] 1) Adjust the oxygen activity in the molten steel to 2.5×10 -6 , after RH vacuum treatment for 5 min, a rare earth alloy of Ce:La=5:5 was added, and the amount of Ce-La added was 0.0006% based on the total mass of the molten steel;
[0027] 2) Re-pressurize the RH vacuum furnace, add a rare earth alloy of Ce:La=5:5 again after soft blowing for 10 minutes, and the amount of Ce-La added is 0.0004% based on the total mass of the molten steel;
[0028] 3) Re-pressurize the RH vacuum furnace and continue the soft blowing treatment. Add the rare earth alloy of Ce:La=5:5 again 5 minutes before tapping. The amount of Ce-La added is 0.0003% based on the total mass of the molten steel. After the RH treatment is completed, the tapping operation is carried out;
[0029] 4) Continuously casting the above molten steel, controlling the superheat of the molten steel to 40°C and the casting speed to 1.2m / min;
[0030] 5) The solidified steel billet is hot rolled, the heating temperature is controlled to be 1250°C, the heating time is 2.5h, the rough rolling and final rolling temperature is 1080°C, the finishing rolling temperature is 980°C, the final rolling temperature is 850°C, the steel plate is rolled to a thickness of 12mm, and then furnace cooled to 600°C for coiling;
[0031] 6) The steel strip obtained by coiling is quenched, and the first quenching heating temperature is controlled to be 880°C, the holding time is 1.5h, and water cooling, and the secondary quenching heating temperature is controlled to be 730°C, the holding time is 1h, and water cooling;
[0032] 7) Temper the quenched steel strip, control the tempering heating temperature to 580°C, the holding time to 1.5h, and furnace cooling.
[0033] It has been determined that the average size of inclusions in the low-temperature steel strip obtained in this embodiment is 450 nm, and the impact energy at -40°C reaches 176 J.
[0034] Example 2
[0035] A method for improving inclusions in low-temperature steel, wherein the components of the low-temperature steel are, by mass, C 0.18%, Si 0.2%, Mn 1.35%, P 0.005%, S 0.005%, Ti 0.017%, and the balance is Fe and unavoidable impurities, and the method comprises the following steps:
[0036] 1) Adjust the oxygen activity in the molten steel to 2.5×10 -6 , after RH vacuum treatment for 5 min, a rare earth alloy of Ce:La=5:5 was added, and the amount of Ce-La added was 0.0007% based on the total mass of the molten steel;
[0037] 2) Re-pressurize the RH vacuum furnace, add a rare earth alloy of Ce:La=5:5 again after soft blowing for 10 minutes, and the amount of Ce-La added is 0.0004% based on the total mass of the molten steel;
[0038] 3) Re-pressurize the RH vacuum furnace and continue the soft blowing treatment. Add the rare earth alloy of Ce:La=5:5 again 5 minutes before tapping. The amount of Ce-La added is 0.0004% based on the total mass of the molten steel. After the RH treatment is completed, the tapping operation is carried out;
[0039] 4) Continuously casting the above molten steel, controlling the superheat of the molten steel to 40°C and the casting speed to 1.2m / min;
[0040] 5) The solidified steel billet is hot rolled, the heating temperature is controlled to be 1250°C, the heating time is 2.5h, the rough rolling and final rolling temperature is 1080°C, the finishing rolling temperature is 980°C, the final rolling temperature is 850°C, the steel plate is rolled to a thickness of 12mm, and then furnace cooled to 600°C for coiling;
[0041] 6) The steel strip obtained by coiling is quenched, and the first quenching heating temperature is controlled to be 880°C, the holding time is 1.5h, and water cooling, and the secondary quenching heating temperature is controlled to be 730°C, the holding time is 1h, and water cooling;
[0042] 7) Temper the quenched steel strip, control the tempering heating temperature to 580°C, the holding time to 1.5h, and furnace cooling.
[0043] It has been determined that the average size of inclusions in the low-temperature steel strip obtained in this embodiment is 423 nm, and the impact energy at -40°C reaches 191 J.
[0044] Example 3
[0045] A method for improving inclusions in low-temperature steel, wherein the components of the low-temperature steel are, by mass, C 0.18%, Si 0.2%, Mn 1.35%, P 0.005%, S 0.005%, Ti 0.017%, and the balance is Fe and unavoidable impurities, and the method comprises the following steps:
[0046] 1) Adjust the oxygen activity in the molten steel to 2.5×10 -6 , after RH vacuum treatment for 5 min, a rare earth alloy of Ce:La=5:5 was added, and the amount of Ce-La added was 0.0009% based on the total mass of the molten steel;
[0047] 2) Re-pressurize the RH vacuum furnace, add a rare earth alloy of Ce:La=5:5 again after soft blowing for 10 minutes, and the amount of Ce-La added is 0.0006% based on the total mass of the molten steel;
[0048] 3) Re-pressurize the RH vacuum furnace and continue the soft blowing treatment. Add the rare earth alloy of Ce:La=5:5 again 5 minutes before tapping. The amount of Ce-La added is 0.0005% based on the total mass of the molten steel. After the RH treatment is completed, the tapping operation is carried out;
[0049] 4) Continuously casting the above molten steel, controlling the superheat of the molten steel to 40°C and the casting speed to 1.2 m / min;
[0050] 5) The solidified steel billet is hot rolled, the heating temperature is controlled to be 1250°C, the heating time is 2.5h, the rough rolling and final rolling temperature is 1080°C, the finishing rolling temperature is 980°C, the final rolling temperature is 850°C, the steel plate is rolled to a thickness of 12mm, and then furnace cooled to 600°C for coiling;
[0051] 6) The steel strip obtained by coiling is quenched, and the first quenching heating temperature is controlled to be 880°C, the holding time is 1.5h, and water cooling, and the secondary quenching heating temperature is controlled to be 730°C, the holding time is 1h, and water cooling;
[0052] 7) Temper the quenched steel strip, control the tempering heating temperature to 580°C, the holding time to 1.5h, and furnace cooling.
[0053] It has been determined that the average size of inclusions in the low-temperature steel strip obtained in this embodiment is 441 nm, and the impact energy at -40°C reaches 184 J.
[0054] Comparative Example 1
[0055] A method for improving inclusions in low-temperature steel, wherein the components of the low-temperature steel are, by mass, C 0.18%, Si 0.2%, Mn 1.35%, P 0.005%, S 0.005%, Ti 0.017%, and the balance is Fe and unavoidable impurities, and the method comprises the following steps:
[0056] 1) Adjust the oxygen activity in the molten steel to 2.5×10 -6 , after RH vacuum treatment for 5 minutes, add Ce:La=5:5 rare earth alloy, based on the total mass of molten steel, the amount of Ce-La added is 0.0013%, re-pressurize the RH vacuum furnace, soft blow for 10 minutes, and perform steel tapping after the RH treatment is completed;
[0057] 2) Continuously casting the above molten steel, controlling the superheat of the molten steel to 40°C and the casting speed to 1.2 m / min;
[0058] 3) The solidified steel billet is hot rolled, the heating temperature is controlled to be 1250°C, the heating time is 2.5h, the rough rolling and final rolling temperature is 1080°C, the finishing rolling temperature is 980°C, the final rolling temperature is 850°C, the steel plate is rolled to a thickness of 12mm, and then furnace cooled to 600°C for coiling;
[0059] 4) The steel strip obtained by coiling is quenched, and the first quenching heating temperature is controlled to be 880°C, the holding time is 1.5h, and water cooling, and the secondary quenching heating temperature is controlled to be 730°C, the holding time is 1h, and water cooling;
[0060] 5) Temper the quenched steel strip, control the tempering heating temperature to 580°C, the holding time to 1.5h, and furnace cooling.
[0061] It has been determined that the average size of inclusions in the low-temperature steel strip obtained in this embodiment is 3.8 μm, and the impact energy at -40°C reaches 147 J.
Claims
1. A method for improving low temperature steel inclusions, characterized in that: The steps include: 1) After RH vacuum treatment for 3-5 minutes, add Ce-La rare earth alloy, the amount of Ce-La added is 0.0006-0.0009% based on the total mass of molten steel; 2) Re-pressurize the RH vacuum furnace, add Ce-La rare earth alloy again after soft blowing for 5-10 minutes, and the amount of Ce-La added is 0.0004-0.0006% based on the total mass of molten steel; 3) Re-pressurize the RH vacuum furnace and continue the soft blowing treatment. Add Ce-La rare earth alloy again 3-5 minutes before tapping. The amount of Ce-La added is 0.0003-0.0005% based on the total mass of molten steel. After the RH treatment is completed, the tapping operation is carried out; The low temperature steel composition includes, by mass, C 0.17-0.19%, Si 0.1-0.2%, Mn 1.35-1.55%, P≤0.01%, S≤0.005%, Ti 0.014-0.02%, and the balance is Fe and unavoidable impurities.
2. The method according to claim 1, characterized in that The method also includes a continuous casting step, during which the superheat of the molten steel is controlled to be 30-40° C. and the casting speed is controlled to be 1.2-1.4 m / min.
3. The method according to claim 2, characterized in that The method also includes a hot rolling step, during which the heating temperature is controlled to be 1200-1250°C, the heating time is 2.5-4h, the rough rolling and final rolling temperatures are ≤1080°C, the finishing rolling start temperature is 980-1050°C, the final rolling temperature is 850-870°C, and the steel plate is rolled to a thickness of 8-12mm and then furnace cooled to 580-600°C for coiling.
4. The method according to claim 3, characterized in that The method also includes a quenching step, during which the first quenching heating temperature is controlled to be 860-880°C, the holding time is 1-1.5 hours, and water cooling is performed, and the second quenching heating temperature is controlled to be 710-730°C, the holding time is 1-1.5 hours, and water cooling is performed.
5. The method according to claim 4, characterized in that The method further comprises a tempering step, during which the tempering heating temperature is controlled to be 570-580° C., the heat preservation time is 1.5-2 hours, and the furnace is cooled.
6. The method according to any one of claims 1 to 5, characterized in that: The rare earth alloy comprises a Ce-Fe alloy and a La-Fe alloy, and the mass ratio of Ce-La in the rare earth alloy is 4-5:5-6.
7. The method according to any one of claims 1 to 5, characterized in that: Before RH treatment, the oxygen activity in the molten steel should be controlled to be ≤2.5×10 -6 .