Piezoelectric ceramic catalyst, preparation method and application
By carefully selecting and proportioning barium oxide, calcium, titanium, zirconium, cerium, and aluminum raw materials, and combining them with ball milling, sintering, and silver plating polarization processes, a piezoelectric ceramic catalyst was prepared. This solved the problems of unstable catalytic performance and difficult recovery in existing technologies, and achieved the effect of highly efficient degradation of azo dye wastewater.
Patent Information
- Application Number
- CN202410933598.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing piezoelectric catalysts suffer from unstable catalytic performance, easy shedding, and difficulty in recovery when treating azo dye wastewater, making it difficult to effectively degrade complex azo dye wastewater.
Piezoelectric ceramic catalysts are prepared by using barium oxide, calcium oxide, titanium oxide, zirconium oxide, cerium oxide, and aluminum oxide raw materials in specific ratios through ball milling, sintering, and silver plating polarization processes. Combined with light irradiation and ultrasonic treatment, the piezoelectric and photocatalytic properties of the catalysts are improved, and wastewater is treated by activating them with oxidants.
A piezoelectric ceramic catalyst with stable catalytic performance and easy recovery was developed, which improved the degradation efficiency of azo dyes in wastewater, broadened the light absorption range of the catalyst, and enhanced the overall catalytic performance of the catalyst.
Smart Images

Figure CN118892821B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of wastewater treatment technology, specifically relating to a piezoelectric ceramic catalyst, its preparation method, and its application. Background Technology
[0002] Azo dye wastewater mainly originates from the textile printing and dyeing, rubber and leather, and papermaking industries. It contains a large amount of chemically stable azo-bonded organic compounds, accounting for 80% of the total organic dyes. Its complex composition makes treatment extremely difficult. Furthermore, the discharge of azo dye wastewater has a serious impact on water bodies and the ecological environment. The presence of azo dyes not only alters the appearance of water bodies but can also disrupt the balance of aquatic ecosystems, limit photosynthesis in aquatic plants, affect oxygen supply, and pose a threat to aquatic life and human health. Therefore, effective treatment of azo dye wastewater is crucial for protecting the environment and human health.
[0003] Piezoelectric catalysis enhances catalytic performance by utilizing the electric field induced by the piezoelectric potential, through charge energy transfer or the separation of electrons and holes. The piezoelectric effect converts mechanical energy into chemical energy, thereby enhancing catalytic activity. BaTiO3, a classic perovskite piezoelectric material, possesses stable chemical properties and high carrier mobility. Under ultrasonic excitation, electrons and holes separate within the catalyst, forming an internal electric field that generates free radicals, thus redoxing pollutants. Therefore, it holds great potential for the treatment of azo dye wastewater.
[0004] Currently, research on piezoelectric catalytic materials both domestically and internationally is generally at the powder and supported stage, primarily using powdered and supported catalysts to treat organic wastewater. Powdered catalysts possess high catalytic activity and specific surface area, but suffer from problems such as difficult recovery, low stability, and uneven dispersion. While supported catalysts solve the recovery problem, their unstable loading and tendency to detach lead to unstable catalytic performance.
[0005] Therefore, developing a piezoelectric catalyst with stable catalytic performance, high catalytic activity, and easy recovery is crucial for solving the problem of difficult treatment of azo dye wastewater. Summary of the Invention
[0006] The purpose of this invention is to overcome the defects in the prior art and provide a piezoelectric ceramic catalyst capable of photocatalysis, its preparation method and application. It can not only perform piezoelectric catalysis but also photocatalysis, and has high catalytic activity, is easy to recover and has stable catalytic performance, and has broad application prospects in the field of wastewater treatment.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0008] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0009] 70-90 parts of barium oxide, 10-30 parts of calcium oxide, 70-95 parts of titanium oxide, 5-30 parts of zirconium oxide, 0-10 parts of cerium oxide (preferably 0.1-1 parts, more preferably 0.4 parts), and 0-0.5 parts of aluminum oxide (preferably 0.02-0.1 parts, more preferably 0.05 parts).
[0010] A method for preparing the piezoelectric ceramic catalyst includes the following steps:
[0011] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol, and ball mill. After ball milling, dry the raw material, then grind it, sieve it, and obtain raw material powder.
[0012] Step 2, firing: Press the raw material powder into ceramic green bodies, and then fire them at high temperature to obtain ceramic blocks;
[0013] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer. Then, the electrode layer is subjected to high-temperature curing and polarization treatment in sequence to obtain silver-plated piezoelectric ceramic, i.e., piezoelectric ceramic catalyst.
[0014] As a further technical solution, in step 1, zirconium oxide beads, five times the total weight of the raw materials, are added for ball milling; the ball milling time is 1-36 hours (preferably 6-16 hours);
[0015] As a further technical solution, an agate mortar and pestle is used for grinding;
[0016] As a further technical solution, drying is performed using a forced-air drying oven.
[0017] As a further technical solution, the drying temperature is 80-100℃;
[0018] As a further technical solution, a 60-100 mesh sieve is used for sieving.
[0019] As a further technical solution, in step 2, the temperature used for high-temperature firing is 1200-1600℃ (preferably 1200-1500℃), and the firing time is 60-480min (preferably 120-240min).
[0020] As a further technical solution, in step 3, the high-temperature curing temperature is 500-700℃;
[0021] As a further technical solution, in step 3, the polarization adopts an oil bath polarization device, and the parameters of the oil bath polarization device are set as follows: 25-60℃, 1-4KV / mm, and polarization time 20-30min.
[0022] Application of the piezoelectric ceramic catalyst and the piezoelectric ceramic catalyst prepared by the preparation method in wastewater treatment.
[0023] A wastewater treatment method includes the following steps:
[0024] Add the piezoelectric ceramic catalyst described above or the piezoelectric ceramic catalyst prepared by the method described above to the wastewater, carry out a dark reaction for 30 minutes, then add an oxidant, and carry out catalytic degradation under light irradiation at a wavelength of 300-500nm (preferably 330-420nm) and / or ultrasound at 60-180W and 40KHz, thereby degrading the organic pollutants in the wastewater into carbon dioxide and water.
[0025] As a further technical solution, the oxidant is a persulfate oxidant;
[0026] As a further technical solution, the persulfate oxidant is one or more of potassium persulfate (KPS), sodium persulfate (APS), and potassium peroxymonosulfate (PMS).
[0027] As a further technical solution, the concentration of persulfate oxidant in the system is 0.2-6 mmol / L (preferably 0.2-3 mmol / L).
[0028] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0029] 1. This invention selects piezoelectric catalyst raw materials and limits the firing conditions so that they can form perovskite-type piezoelectric catalysts on the one hand and ceramicize them on the other hand, making them easy to recycle.
[0030] 2. In the process of compounding piezoelectric raw materials, the present invention involves doping with cerium oxide and / or alumina, and constructing heterojunctions between raw material powders through ball milling dispersion and solid-state sintering. This not only improves the piezoelectric properties of ceramics, but also enables titanium oxide to still have certain photocatalytic activity after high-temperature firing, broadens the light absorption range of the catalyst, and obtains a piezoelectric ceramic catalyst with a band gap of 1.66 eV.
[0031] 3. After the piezoelectric ceramic is successfully fired, it is silver-plated for polarization, which can form an electrode layer, improve the conductivity and bonding force of the electrode, make the electric field distribution more uniform, and improve the electrical performance.
[0032] 4. The present invention activates the piezoelectric ceramic catalyst by adding an oxidant to the wastewater, which can greatly improve the catalytic performance of the piezoelectric ceramic catalyst.
[0033] In summary, this invention involves the careful selection and proportioning of piezoelectric catalyst raw materials, enabling them to form a perovskite-type piezoelectric catalyst while simultaneously achieving ceramization under specific process conditions, facilitating its recovery. Furthermore, the selection, proportioning, and timing of dopants, along with the use of silver plating polarization and oxidant activation, endow the piezoelectric catalyst with both piezoelectric and photocatalytic properties, significantly improving the wastewater degradation efficiency of the piezoelectric ceramic catalyst. Moreover, the catalytic performance is stable and easily recoverable. All these factors contribute significantly to the catalytic effect of the piezoelectric ceramic catalyst of this invention; each factor interacts with the others and is indispensable. Attached Figure Description
[0034] Figure 1 This is a piezoelectric performance diagram of a piezoelectric ceramic catalyst with different ball milling times in one embodiment of the present invention;
[0035] Figure 2 This is a diagram showing the piezoelectric properties of piezoelectric ceramic catalysts with different Al doping amounts in one embodiment of the present invention;
[0036] Figure 3 This is a graph showing the efficiency of piezoelectric ceramic catalysts for catalytic degradation of methylene blue under different Al doping levels in one embodiment of the present invention.
[0037] Figure 4 This is a diagram showing the physicochemical properties of piezoelectric ceramic catalysts with different cerium doping amounts in one embodiment of the present invention;
[0038] Figure 5 Piezoelectric properties of piezoelectric ceramic catalysts with different cerium doping levels in one embodiment of the present invention;
[0039] Figure 6 The image shows the XRD patterns of piezoelectric ceramic catalysts with different cerium doping levels in one embodiment of the present invention.
[0040] Figure 7 This is a graph showing the efficiency of piezoelectric ceramic catalysts for catalytic degradation of methylene blue under different cerium doping levels in one embodiment of the present invention.
[0041] Figure 8 The DRS spectrum of a piezoelectric ceramic catalyst in one embodiment of the present invention is shown below.
[0042] Figure 9 This is a graph showing the effect of different oxidants on the photocatalytic and piezoelectric catalytic performance of a piezoelectric ceramic catalyst in one embodiment of the present invention;
[0043] Figure 10 This is a graph showing the effect of different amounts of oxidant PMS on the photocatalytic and piezoelectric catalytic performance of the piezoelectric ceramic catalyst in one embodiment of the present invention;
[0044] Figure 11This is a graph showing the effect of the number of cycles on the photocatalytic and piezoelectric catalytic performance of the piezoelectric ceramic catalyst in one embodiment of the present invention;
[0045] exist Figure 3 , 7 In 9-11, a) piezoelectric catalytic performance, b) photocatalytic performance;
[0046] exist Figure 6 In the diagram, a) is a view of the 20-70° range, and b) is a magnified view of the 44.5-46° range. Detailed Implementation
[0047] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0048] Additionally, it should be noted that the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0049] In this invention, barium oxide, calcium oxide, titanium oxide, zirconium oxide, cerium oxide, and aluminum oxide are all of analytical grade (AR) and are sourced from Shandong Xiya Chemical Industry Co., Ltd. or Shanghai Maclean Biochemical Technology Co., Ltd.; the water is laboratory distilled water, and the anhydrous ethanol is of analytical grade (AR).
[0050] Unless otherwise specified, all raw materials used in this invention are commercially available.
[0051] In this invention, a piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0052] Barium oxide 70-90 parts, calcium oxide 10-30 parts, titanium oxide 70-95 parts, zirconium oxide 5-30 parts, cerium oxide 0-10 parts, aluminum oxide 0-0.5 parts.
[0053] Its preparation method includes the following steps:
[0054] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 1-36 hours. After ball milling, dry in a forced-air drying oven at 80-100℃, then grind in an agate mortar and pass through a 60-100 mesh sieve to obtain raw material powder.
[0055] Step 2, firing: Press the raw material powder into ceramic green body using a tablet press, and then fire it at 1200-1600℃ for 60-480 minutes to obtain ceramic block;
[0056] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 25-60℃ and 1-4KV / mm for 20-30 minutes using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0057] The method for treating wastewater using the aforementioned piezoelectric ceramic catalyst includes the following steps:
[0058] The piezoelectric ceramic catalyst was added to the wastewater and subjected to a dark reaction for 30 minutes. Then, 0.2-6 mmol / L persulfate oxidant was added to activate the piezoelectric catalyst. Catalytic degradation was then carried out under light irradiation at a wavelength of 300-500 nm and / or ultrasound at 60-180 W and 40 kHz to degrade the organic pollutants in the wastewater into carbon dioxide and water.
[0059] In this invention, the photocatalytic performance and piezoelectric catalytic performance tests are designed according to the experimental scheme, with 10 experimental groups and 5 parallel samples in each group; the ultraviolet-visible absorption spectroscopy determination is designed according to the experimental scheme, with 5 experimental groups and 1 sample in each group; the piezoelectric performance test is designed according to the experimental scheme, with 3 experimental groups and 5 parallel samples in each group; and the physicochemical performance test is designed according to the experimental scheme, with 3 experimental groups and 5 parallel samples in each group.
[0060] In this invention, the methylene blue degradation rate is calculated using formula (1) as follows:
[0061]
[0062] Among them, c o c represents the initial concentration of methylene blue at the start of the experiment. t The concentration of methylene blue at time t min is given.
[0063] Example 1: Effect of ball milling time on the piezoelectric properties of piezoelectric ceramic catalysts
[0064] I. Experimental Materials:
[0065] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0066] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0 parts cerium oxide, and 0 parts aluminum oxide;
[0067] Its preparation method includes the following steps:
[0068] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 6-24 hours. After ball milling, dry in a forced-air drying oven at 80℃, then grind in an agate mortar and pestle, and pass through a 60-mesh sieve to obtain raw material powder.
[0069] Step 2, Firing: The raw material powder is pressed into ceramic green body using a tablet press, and then fired at 1420℃ for 240 minutes to obtain ceramic block;
[0070] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 40℃ and 2KV / mm for 20min using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0071] In this embodiment, the difference between the experimental groups is that the ball milling time is 6h, 9h, 12h, 15h, 18h, and 24h, respectively.
[0072] II. Detection Indicators and Methods:
[0073] The piezoelectric constant d of the piezoelectric ceramic catalysts prepared in each experimental group was determined. 33 and piezoelectric coefficient K p The results are shown Figure 1 ;
[0074] piezoelectric constant d 33 and piezoelectric coefficient K p The detection methods employed were the quasi-static method and the impedance spectrum method, respectively.
[0075] Figure 1 This is a piezoelectric property diagram for different ball milling times, from... Figure 1 It can be seen that as the ball milling time increases, the sample's d 33 With k p The trend shows an initial increase followed by a decrease. Particularly for the BCZT sample ball-milled for 12 hours, the piezoelectric parameters reached their highest values, specifically dp. 33 =235pC / N, k p=20.61%. The effect of ball milling time on the piezoelectric properties of barium titanate ceramics is a complex process involving changes in the material's microstructure and defect states. The mechanisms of influence are as follows: First, the intense action during ball milling causes lattice distortion and dislocations, generating numerous lattice defects and increasing internal stress, providing more charge carriers and contributing to a larger polarization response under an electric field. Second, lattice distortion and dielectric relaxation reduce domain dynamic barriers, promoting domain migration and thus improving piezoelectric properties. Finally, the ball milling process optimizes the grain shape and size distribution, resulting in finer and more uniform grains, which facilitates uniform grain growth during sintering, playing a crucial role in improving the electrical properties of piezoelectric ceramics.
[0076] Example 2: Effect of different alumina doping amounts on the piezoelectric properties of piezoelectric catalysts
[0077] I. Experimental Materials
[0078] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0079] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0 parts cerium oxide, and 0-0.4 parts aluminum oxide; In this embodiment, the difference between the experimental groups is that the amount of aluminum oxide is 0 parts, 0.05 parts, 0.1 parts, 0.2 parts, 0.4 parts, and 0.8 parts, respectively.
[0080] Its preparation method is consistent with the steps and parameters of Example 2;
[0081] II. Detection Indicators
[0082] The piezoelectric constant d of the piezoelectric ceramic catalysts prepared in each experimental group was determined. 33 and piezoelectric coefficient K p The results are shown Figure 2 ;
[0083] piezoelectric constant d 33 and piezoelectric coefficient K p The detection methods employed were the quasi-static method and the impedance spectrum method, respectively.
[0084] III. Results Analysis
[0085] Figure 2 This is a graph showing the piezoelectric properties of the piezoelectric catalyst with different alumina doping levels. Figure 2 It is understood that, for A1 3+ Doping revealed that trace doping (x = 0.05) significantly improved piezoelectric properties (d). 33 =285pC / N, k p =32.10%). With A1 3+ With increasing content, a decreasing trend in piezoelectric properties was observed. The study results showed that trace amounts of heterovalent Al...3+ Doping with Al can effectively improve the piezoelectric properties of BCZT ceramics. This improvement is mainly achieved through the following two mechanisms: First, Al... 3+ The trace doping of the material induces greater lattice distortion, leading to lattice mismatch and corresponding local strain between the phase structures of each component, promoting increased polarization rotation, and thus enhancing the piezoelectric response. Secondly, the main internal defects in pure BCZT samples are oxygen vacancies and free electrons. A1 3+ When Al is introduced into the perovskite structure as a donor dopant ion, 3 When the + enters the A site, it effectively suppresses the formation of oxygen vacancies, which is beneficial to the enhancement of piezoelectric properties.
[0086] Example 3: Effect of different alumina dosages on the catalytic performance of piezoelectric catalysts
[0087] I. Experimental Materials
[0088] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0089] Barium oxide 85 parts, calcium oxide 15 parts, titanium oxide 95 parts, zirconium oxide 5 parts, cerium oxide 0 parts, aluminum oxide 0-0.4 parts;
[0090] Its preparation method is consistent with the steps and parameters of Example 2;
[0091] In this embodiment, the difference between the experimental groups is that the alumina content is 0 parts (BCZT group), 0.05 parts (BCZT-0.05Al group), 0.1 parts (BCZT-0.1Al group), 0.2 parts (BCZT-0.2Al group), and 0.4 parts (BCZT-0.4Al group).
[0092] II. Detection Indicators
[0093] The photocatalytic and piezoelectric catalytic activities of each group were measured separately. The specific detection methods are as follows, and the results are shown in the figure. Figure 3 .
[0094] 1. Determination of photocatalytic performance: Methylene blue solution was used as simulated wastewater, and the absorbance of the methylene blue solution was measured at 664 nm using a UV spectrophotometer. 1.2 g of the piezoelectric ceramic catalyst prepared in Example 3 was added to methylene blue solutions of pH = 7, 100 mL, and 10 mg / L. After a 30 min dark reaction, the absorbance was measured. After the dark reaction, 2.4 mmol / L PMS oxidant was added to the methylene blue solution, and a photocatalytic experiment was conducted under LED light illumination at wavelengths of 330-420 nm. The changes in absorbance of the methylene blue solution after 30, 60, 90, and 120 min of illumination were recorded. The degradation rate was calculated using formula (1).
[0095] 2. Determination of piezoelectric catalytic performance: Methylene blue solution was used as simulated wastewater, and the absorbance of the methylene blue solution was measured at 664 nm using a UV spectrophotometer. 1.2 g of the piezoelectric ceramic catalyst prepared in Example 2 was added to methylene blue solutions of pH = 7, 100 mL, and 10 mg / L, and the absorbance was measured after a 30 min dark reaction. After the dark reaction, 2.4 mmol / L PMS oxidant was added to the methylene blue solution, and a piezoelectric catalytic experiment was conducted under ultrasound at 60-180 W and 40 kHz. The absorbance changes of the methylene blue solution after ultrasound for 30, 60, 90, and 120 min were recorded. The degradation rate was calculated using formula (1).
[0096] III. Results Analysis
[0097] from Figure 3 It is known that in the piezoelectric catalysis experiment, Al₂O₃ as a dopant achieved the highest degradation efficiency, approximately 27%, at a doping concentration of 0.05 parts by weight. This peak efficiency is attributed to the doping optimizing the crystal structure and reducing lattice defects, thereby improving catalytic efficiency. However, with increasing doping concentration, excessive alumina may cause lattice distortion and increase lattice defects. This not only reduces the effective concentration of charge carriers and affects electron transport, but may also alter surface active sites, reducing the thermal and chemical stability of the material, leading to a decrease in catalytic efficiency.
[0098] Regarding photocatalytic efficiency, alumina-doped BCZT ceramics performed worse than undoped ceramics. This may be because doping alters the material's optical properties, reducing light absorption and the generation of photogenerated electron-hole pairs. Furthermore, defects introduced by doping may act as recombination centers, accelerating electron-hole recombination, reducing the separation efficiency of photogenerated charges, and decreasing the number of effective charge carriers. Lattice distortion may affect electron mobility, reducing charge transport efficiency. The reduction in surface active sites decreases catalytic activity, and chemical stability issues may lead to easier degradation of the material under light irradiation.
[0099] In summary, while appropriate alumina doping can optimize the piezoelectric catalytic activity of barium titanate ceramics, excessive doping may negatively impact the photo / electrocatalytic efficiency of the material. To achieve optimal catalytic efficiency, precise control of the doping amount is necessary, taking into account the material's optical properties, charge carrier dynamics, lattice structure stability, and the distribution of surface active sites.
[0100] Example 4: Effect of different cerium oxide doping amounts on the physicochemical properties of piezoelectric ceramic catalysts
[0101] I. Experimental Materials:
[0102] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0103] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0-0.5 parts cerium oxide, and 0.05 parts aluminum oxide;
[0104] Its preparation method includes the following steps:
[0105] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 720 minutes. After ball milling, dry in a forced-air drying oven at 85°C, then grind in an agate mortar and pestle, and pass through a 60-mesh sieve to obtain raw material powder.
[0106] Step 2, Firing: The raw material powder is pressed into ceramic green body using a tablet press, and then fired at 1460℃ for 240 minutes to obtain ceramic block;
[0107] Step 3, Silver Plating Polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 40℃ and 2KV / mm for 20 min using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0108] The difference between the experimental samples in this embodiment is that the doping amount of cerium oxide is 0 parts, 0.2 parts, 0.3 parts, 0.4 parts, and 0.5 parts, respectively;
[0109] II. Detection Indicators and Methods:
[0110] The physicochemical properties (density and packing density) of the piezoelectric ceramic catalysts prepared in each experimental group were tested, and the results are shown in the table below. Figure 4 ;
[0111] Density and packing density were determined using the Archimedes displacement method (GB-T 3810.3-2016);
[0112] III. Results Analysis
[0113] Figure 4 These are physicochemical property diagrams of piezoelectric ceramic catalysts with different cerium oxide doping amounts, derived from... Figure 4 It can be seen that with the increase of cerium oxide doping amount, the density and compactness of the piezoelectric ceramic catalyst show a monotonically increasing trend, reaching a peak at a cerium oxide doping amount of 0.4 parts by weight, and then decreasing. This is because initially, a small amount of cerium oxide enters the lattice and substitutes for (Ti, Zr). 4+The difference in ionic radius promotes charge migration and diffusion, which in turn promotes grain growth and changes the microstructure of piezoelectric ceramic catalysts, thereby improving the density of ceramics. However, the solubility of cerium oxide in crystals is limited. When excessive cerium oxide is incorporated into piezoelectric ceramic catalysts, some dopants precipitate as impurity phases, which inhibits normal grain growth and introduces defects, resulting in a deterioration in the density and performance of piezoelectric ceramic catalysts.
[0114] Example 5: Effect of different cerium oxide doping amounts on the piezoelectric properties of piezoelectric ceramic catalysts
[0115] I. Experimental Materials
[0116] A piezoelectric ceramic catalyst, same as in Example 4;
[0117] II. Detection Indicators
[0118] The piezoelectric constant d of the piezoelectric ceramic catalysts prepared in each experimental group was determined. 33 and piezoelectric coefficient K p The results are shown Figure 5 ;
[0119] piezoelectric constant d 33 and piezoelectric coefficient K p The detection methods employed were the quasi-static method and the impedance spectrum method, respectively.
[0120] Figure 5 This is a graph showing the piezoelectric properties of piezoelectric ceramic catalysts with different weight parts of Ce doping. Figure 3 It is understood that, with Ce 4+ With increasing doping concentration, the piezoelectric properties of the piezoelectric ceramic catalyst gradually increase, and the piezoelectric catalytic activity is enhanced, consistent with the trend of the catalyst's piezoelectric catalytic degradation efficiency of methylene blue. This is because the introduction of cerium dopant ions improves the overall density and grain size uniformity of the sample, reduces the number of grain boundaries, and thus reduces the resistance to domain wall movement.
[0121] Example 6: Effect of different cerium oxide doping amounts on the crystal phase of piezoelectric catalysts
[0122] I. Experimental Materials
[0123] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0124] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0.5 parts cerium oxide, and 0.05 parts aluminum oxide;
[0125] Its preparation method is consistent with the steps and parameters of Example 2;
[0126] In this embodiment, the difference between the experimental groups is that the amount of cerium oxide doped is 0 parts (BCZT group), 0.2 parts (BCZT-0.2Ce group), 0.3 parts (BCZT-0.3Ce group), 0.4 parts (BCZT-0.4Ce group), and 0.5 parts (BCZT-0.5Ce group).
[0127] II. Detection Indicators
[0128] The XRD patterns of the piezoelectric ceramic catalysts prepared in each group were scanned separately, and the results are shown in the figure. Figure 6 ;
[0129] III. Results Analysis
[0130] from Figure 6 It can be seen that the introduction of alumina and cerium oxide significantly affects the crystal phase structure of BCZT ceramics during doping. Comparison with standard PDF cards (PDF#86-1569, PDF#74-1960, PDF#74-1960) shows that all samples exhibit a pure perovskite phase, with no secondary impurity phase detected, indicating that the doped alumina and cerium oxide are incorporated into the BCZT ceramics. In the undoped barium titanate sample, the XRD pattern shows a dominant (200) peak, indicating the presence of the prismatic phase of barium titanate ceramics. However, when alumina and cerium oxide are introduced, a splitting of the main peak is observed near 45° in the XRD pattern, with a ratio of approximately 1:2, indicating the coexistence of the prismatic and tetragonal phases. This coexistence may be related to changes in lattice parameters, which affect the symmetry of the lattice, leading to the formation of different crystal phases.
[0131] The co-doping of alumina and cerium oxide significantly affects the lattice stability and ferroelectric properties of barium titanate ceramics. Alumina doping is achieved through Al... 3+ Replace Ba 2+ This causes lattice contraction, thus affecting the ferroelectric properties of the material. Cerium oxide doping replaces Ti. 4+ The presence of oxygen vacancies in the lattice introduces more oxygen vacancies, adjusting the lattice charge balance and improving conductivity. When alumina and cerium oxide are doped simultaneously, these two effects interact, leading to complex changes in lattice parameters. Initially, the doping of alumina and cerium oxide causes lattice parameter contraction, manifested as a shift of diffraction peaks towards higher angles. When the alumina content remains constant, as the cerium oxide doping amount increases, the lattice parameters begin to increase, and the diffraction peaks shift towards lower angles. This may be due to the lattice expansion effect caused by oxygen vacancies.
[0132] Example 7: Effect of different cerium oxide doping amounts on the catalytic performance of piezoelectric catalysts
[0133] I. Experimental Materials
[0134] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0135] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0-0.5 parts cerium oxide, and 0.05 parts aluminum oxide;
[0136] Its preparation method is consistent with the steps and parameters of Example 2;
[0137] In this embodiment, the difference between the experimental groups is that the amount of cerium oxide doped is 0 parts (BCZT group), 0.2 parts (BCZT-0.2Ce group), 0.3 parts (BCZT-0.3Ce group), 0.4 parts (BCZT-0.4Ce group), and 0.5 parts (BCZT-0.5Ce group).
[0138] Another group, Fines, was established. The catalyst in Fines was prepared by grinding the piezoelectric ceramic catalyst prepared in the BCZT group into powder, mixing it with alumina powder and cerium oxide powder, and then setting it aside for later use.
[0139] II. Indicator Testing
[0140] The photocatalytic and piezoelectric catalytic performances of each experimental group and control group were measured separately. The detection methods are described in Example 3, and the results are shown in […]. Figure 7 ;
[0141] III. Results Analysis
[0142] Figure 7 The efficiency of piezoelectric ceramic catalysts for the catalytic degradation of methylene blue under different cerium oxide doping concentrations is shown in the graph (where a represents piezoelectric catalysis and b represents photocatalysis); by... Figure 7 Data analysis revealed that in the Fines control group, the efficiency of catalytic degradation of methylene blue by undoped piezoelectric catalyst powders, when dispersed separately in wastewater as cerium oxide or alumina powders, was significantly lower than that by incorporating cerium oxide into the piezoelectric catalysts (BCZT-0.2Ce, BCZT-0.3Ce, BCZT-0.4Ce, and BCZT-0.5Ce groups). This phenomenon can be attributed to the lack of catalytic performance of alumina and cerium oxide themselves, with their primary function being adsorption. Furthermore, in the Fines control group, cerium oxide failed to effectively bind with the piezoelectric catalyst, thus failing to optimize the microstructure of the piezoelectric catalyst and consequently improve its catalytic efficiency.
[0143] In addition, in the Fines control group, the mixing of piezoelectric catalyst powder with methylene blue caused turbidity in the solution, which not only affected the absorption efficiency of the piezoelectric catalyst for light energy during photocatalysis, but also caused inconvenience to the experimental operation and the separation and recovery of the catalyst after the experiment.
[0144] For the bulk piezoelectric ceramic catalyst of this invention, when doped with alumina, the role of 0.05 parts by weight of alumina in the piezoelectric and photocatalytic processes is: the alumina doping introduces Al into the BCZT lattice. 3+ Ions, replacing Ba 2 + Ions cause lattice contraction. Lattice contraction not only affects the ferroelectric properties of materials, improving their piezoelectric properties, but also enhances the ability of charge carriers to separate, capture, and transfer to the surface of photocatalysts by adjusting the electronic and band structures.
[0145] For the bulk piezoelectric ceramic catalyst of this invention, when doped with cerium oxide, its catalytic degradation efficiency of methylene blue increases with increasing cerium oxide doping concentration. This phenomenon can be attributed to the piezoelectric catalytic mechanism: the localized polarization effect induced by mechanical stress generates charges on the surface of the ferroelectric material, and these charges interact with O2 and OH... - A reaction occurs, forming highly reactive substances that further promote the degradation of methylene blue dye. Methylene blue dye, due to its strong redox capabilities, is reacted with reactive free radicals Ce2. 4+ The introduction of ions improves the overall density and grain size uniformity of the sample, reduces the number of grain boundaries, thereby reducing the hindrance to domain wall movement, improving the free carrier concentration during piezoelectric catalysis, and enhancing the piezoelectric catalytic efficiency. In the photocatalytic process, appropriate CeO2 doping promotes the formation of an n-type heterojunction between the piezoelectric catalyst and CeO2. Because CeO2 has higher valence and conduction band energy levels, electrons in its conduction band tend to migrate to the conduction band of the piezoelectric catalyst, while holes in the valence band of the piezoelectric catalyst migrate to the valence band of CeO2. This interfacial electron transport balance creates a local electric field, enhancing the separation efficiency of photogenerated electron-hole pairs, leading to an increase in the number of carriers on the ceramic surface, and thus improving the photocatalytic activity of the ceramic.
[0146] However, it is worth noting that when Ce 4+ When the doping amount is too high, Ce has limited solubility in perovskite solid solutions. 4+ It may segregate towards grain boundaries, hindering grain growth, reducing surface energy, and slowing down particle aggregation. Furthermore, Ce... 4+ It may replace the original Ba 2+ and Ca 2+ This leads to an increase in oxygen vacancies and defective dipoles, which may in turn reduce the catalytic activity (piezoelectric and photocatalytic) of the material.
[0147] Example 8: Determination of UV absorption spectrum and geobaric width of piezoelectric ceramic catalysts
[0148] I. Experimental Materials
[0149] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0150] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0.4 parts cerium oxide, and 0.05 parts aluminum oxide;
[0151] Its preparation method includes the following steps:
[0152] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 360 minutes. After ball milling, dry in a forced-air drying oven at 80°C, then grind in an agate mortar and pestle, and pass through a 60-mesh sieve to obtain raw material powder.
[0153] Step 2, Firing: The raw material powder is pressed into ceramic green body using a tablet press, and then fired at 1400℃ for 180 minutes to obtain ceramic block;
[0154] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 40℃ and 2KV / mm for 20min using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0155] The prepared piezoelectric ceramic catalyst was ground through a 200-mesh sieve and then dried at 100°C for later use.
[0156] II. Detection Indicators:
[0157] 1. Ultraviolet-Visible Absorption Spectroscopy: The ultraviolet-visible absorption spectrum of the sample was measured using a solid-state ultraviolet-visible-infrared analyzer; and its band gap was calculated; the results are shown in […]. Figure 8 ;
[0158] III. Results Analysis:
[0159] The absorption characteristics of the samples were studied and their band gaps were calculated using UV-vis diffuse reflectance spectroscopy (DRS). The DRS spectra of the prepared piezoelectric ceramic catalysts were analyzed. Figure 8 The band gap (Eg) of each sample is quantified using the Tauc plot formula (2), as follows:
[0160]
[0161] Where α is the absorbance index, h is Planck's constant, v is the frequency (nm), A is a constant, and E is a constant. g denoted as the semiconductor bandgap (eV). The exponent n is related to the semiconductor type: direct bandgap semiconductors: n = 1 / 2; indirect bandgap semiconductors: n = 2.
[0162] like Figure 8As shown, the piezoelectric ceramic catalyst sample prepared in Example 2 has a band gap of 1.66 eV and exhibits strong responses to both ultraviolet and visible light, with its light absorption range broadened to approximately 700 nm. This change in color, from pale yellow to brownish-red, indicates that the barium calcium zirconate titanate (BCZT) ceramic surface doped with cerium oxide and alumina forms more reactive sites, thereby enhancing light absorption intensity and improving the material's light absorption performance in the visible light region. Clearly, the addition of dopants not only acts as electron acceptors or donors, increasing the generation of photogenerated electron-hole pairs and the number of surface charge carriers, but also reduces electron-hole recombination, thus effectively improving the degradation rate of methylene blue.
[0163] Example 9: Effects of different oxidants and dosages on the photocatalytic and piezoelectric catalytic performance of piezoelectric ceramic catalysts I. Experimental materials:
[0164] A piezoelectric ceramic catalyst comprises the following raw materials in parts by weight:
[0165] 85 parts barium oxide, 15 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0.4 parts cerium oxide, and 0.05 parts aluminum oxide;
[0166] Its preparation method includes the following steps:
[0167] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 360 minutes. After ball milling, dry in a forced-air drying oven at 80°C, then grind in an agate mortar and pestle, and pass through a 60-mesh sieve to obtain raw material powder.
[0168] Step 2, Firing: The raw material powder is pressed into ceramic green body using a tablet press, and then fired at 1400℃ for 180 minutes to obtain ceramic block;
[0169] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 40℃ and 2KV / m for 20min using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0170] II. Experimental Methods:
[0171] 1. The effects of different oxidants on the photocatalytic and piezoelectric catalytic performance of piezoelectric ceramic catalysts are shown in the figure. Figure 9 (a. piezoelectric catalytic performance, b. photocatalytic performance);
[0172] 1) Determination of photocatalytic performance: Methylene blue solution was used as simulated wastewater, and the absorbance of the methylene blue solution was measured at 664 nm using a UV spectrophotometer. 1.2 g of the piezoelectric ceramic catalyst prepared in Example 2 was added to methylene blue solutions of pH = 7, 100 mL, and 10 mg / L, respectively. After a 30 min dark reaction, the absorbance was measured. After the dark reaction, 1.2 mmol / L of oxidant (APS oxidant, PMS oxidant, and KPS oxidant, respectively) was added to the methylene blue solution, and a photocatalytic experiment was conducted under LED light illumination at wavelengths of 330-420 nm. The changes in absorbance of the methylene blue solution after 30, 60, 90, and 120 min of illumination were recorded. A control group without added oxidant, i.e., the 0 mmol / L oxidant group, was also set up; its degradation rate was calculated using formula (1).
[0173] 2) Determination of piezoelectric catalytic performance: Methylene blue solution was used as simulated wastewater, and the absorbance of the methylene blue solution was measured at 664 nm using a UV spectrophotometer. 1.2 g of the piezoelectric ceramic catalyst prepared in Example 2 was added to methylene blue solutions of pH = 7, 100 mL, and 10 mg / L, respectively. After a 30 min dark reaction, the absorbance was measured. After the dark reaction, 1.2 mmol / L of oxidant (APS oxidant, PMS oxidant, and KPS oxidant, respectively) was added to the methylene blue solution, and a piezoelectric catalytic experiment was performed under ultrasound at 60-180 W and 40 kHz. The absorbance changes of the methylene blue solution after ultrasound for 30, 60, 90, and 120 min were recorded. A control group without added oxidant, i.e., the 0 mmol / L oxidant group, was also set up; its degradation rate was calculated using formula (1).
[0174] 2. The effect of different amounts of oxidant PMS on the photocatalytic and piezoelectric catalytic performance of the piezoelectric ceramic catalyst is shown in the figure. Figure 10 (a. piezoelectric catalytic performance, b. photocatalytic performance);
[0175] The determination of photocatalytic performance and piezoelectric catalytic performance were the same as above, except that the oxidant was PMS, and the amounts used in each group were 0 mmol / L, 0.6 mmol / L, 1.2 mmol / L, 1.8 mmol / L, and 2.4 mmol / L, respectively.
[0176] III. Results Analysis
[0177] Depend on Figure 9-10 It can be seen that different oxidants can improve the degradation efficiency, with the highest degradation rate observed when PMS is used to activate the piezoelectric ceramic catalyst. Higher PMS dosage leads to higher degradation rates. When APS or KPS oxidants are used to activate the piezoelectric ceramic catalyst, they not only generate strong oxidizing agents (·SO4-) but also promote the generation of ·OH. During the catalytic reaction, the ceramic is stimulated by ultrasound or light, generating h...+ With e - h + It reacts with H2O to produce ·OH, and e reacts with O2 at oxygen vacancies (OVs) to produce ·O2. - Simultaneously, under the action of ultrasound or photoactivation, S2O8 in APS and KPS... 2- It can be converted into SO4, which has strong oxidizing properties. - Among them, S208 in piezoelectric catalysis 2 - It can accept electrons from the anode to promote the formation of SO4-. In photocatalysis, methylene blue dye, as a photosensitive dye, reacts under light with a positive charge, reacting with negatively charged S2O8-. 2- Easy to access, SO4 is effectively generated through the injection of photogenerated electrons into APS and KPS. - The generated SO4 - It reacts with OH- to produce ·OH and SO4. 2- These factors work together to promote the degradation process of organic pollutants. Finally, the catalytic reaction produces highly oxidizing SO42-. - ·OH and ·O2 - The catalytic degradation of methylene blue-simulated wastewater was rapidly oxidized. Compared to APS and KPS oxidants, PMS oxidant simultaneously generates ·SO4- and ·OH upon activation, accelerating ·OH formation and increasing the amount of ·OH generated compared to APS and KPS. Therefore, PMS oxidant significantly improves the catalytic reaction efficiency compared to APS and KPS oxidants.
[0178] Example 10
[0179] 1. A piezoelectric ceramic catalyst, same as in Example 9;
[0180] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0181] The photocatalysis process includes: adding 1.2 g of piezoelectric ceramic catalyst to 100 mL of methylene blue simulated wastewater at pH = 7 and 10 mg / L, performing a dark reaction for 30 min, then adding 1.2 mmol / L of KPS oxidant, and performing photocatalytic degradation for 120 min under light irradiation at a wavelength of 330-420 nm; and detecting and calculating the photocatalytic degradation rate.
[0182] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 1.2mmol / L of KPS oxidant, and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; detecting and calculating the piezoelectric catalytic degradation rate.
[0183] In this embodiment, the photocatalytic degradation rate of simulated methylene blue wastewater at pH=7, 100 mL, and 10 mg / L was 75.60%, and the piezoelectric catalytic degradation rate was 76.41%.
[0184] Example 11
[0185] 1. A piezoelectric ceramic catalyst, same as in Example 9;
[0186] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0187] The photocatalysis process includes: adding 1.2 g of the piezoelectric ceramic catalyst prepared in Example 9 to 100 mL of methylene blue simulated wastewater at pH = 7 and 10 mg / L, performing a dark reaction for 30 min, then adding 1.2 mmol / L of PMS oxidant, and performing photocatalytic degradation for 120 min under light irradiation at a wavelength of 330-420 nm; n; detecting and calculating the photocatalytic degradation rate;
[0188] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 1.2mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0189] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100mL, and 10mg / L was 87.54%, and the piezoelectric catalytic degradation rate was 86.62%.
[0190] Example 12
[0191] 1. A piezoelectric ceramic catalyst, same as in Example 9;
[0192] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0193] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0194] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0195] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100 mL, and 10 mg / L was 92.76%, and the piezoelectric catalytic degradation rate was 91.19%.
[0196] Example 13: Effect of recycling on the catalytic performance of piezoelectric ceramic catalysts
[0197] I. Experimental Materials
[0198] A piezoelectric ceramic catalyst, same as in Example 9.
[0199] II. Detection Indicators
[0200] The piezoelectric ceramic catalyst prepared above was used for photocatalytic and piezoelectric degradation of MB dye. After the first degradation experiment was completed, the catalyst was recovered, and the next degradation experiment was conducted. The cycle was repeated 5 times, and the photocatalytic and piezoelectric catalytic efficiencies at different catalytic times were measured in each cycle. The results are shown in […]. Figure 11 .
[0201] III. Results and Analysis
[0202] from Figure 11 It can be seen that after repeated degradation by BCZT-0.4Ce ceramic, the efficiency of MB dye degradation initially slowed down and then stabilized. In the initial degradation experiment, the degradation efficiency of both catalytic reactions was close to 90%. However, in the fifth repeated experiment, the degradation efficiency of piezoelectric catalysis decreased to 79.82%, and the photocatalytic efficiency also decreased to 69.04%. The experimental results show that despite repeated catalytic experiments, BCZT-0.4Ce ceramic still exhibits relatively good performance in MB degradation and demonstrates reliable reusability.
[0203] Example 14
[0204] 1. A piezoelectric ceramic catalyst, comprising the following raw materials in parts by weight:
[0205] 80 parts barium oxide, 20 parts calcium oxide, 95 parts titanium oxide, 5 parts zirconium oxide, 0.4 parts cerium oxide, and 0.05 parts aluminum oxide;
[0206] Its preparation method includes the following steps: same as in Example 9.
[0207] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0208] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0209] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0210] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100 mL, and 10 mg / L was 78.19%, and the piezoelectric catalytic degradation rate was 76.78%.
[0211] Example 15
[0212] 1. A piezoelectric ceramic catalyst, comprising the following raw materials in parts by weight:
[0213] 85 parts barium oxide, 15 parts calcium oxide, 75 parts titanium oxide, 25 parts zirconium oxide, 0.4 parts cerium oxide, and 0.05 parts aluminum oxide;
[0214] Its preparation method includes the following steps: same as in Example 9.
[0215] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0216] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0217] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0218] In this embodiment, the photocatalytic degradation rate of simulated methylene blue wastewater at pH=7, 100 mL, and 10 mg / L was 73.42%, and the piezoelectric catalytic degradation rate was 78.19%.
[0219] Example 16
[0220] 1. A piezoelectric ceramic catalyst, comprising the following raw materials in parts by weight:
[0221] 70 parts barium oxide, 30 parts calcium oxide, 90 parts titanium oxide, 10 parts zirconium oxide, 0.3 parts cerium oxide, and 0.4 parts aluminum oxide;
[0222] Its preparation method includes the following steps: same as in Example 9.
[0223] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0224] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0225] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0226] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100mL, and 10mg / L was 82.14%, and the piezoelectric catalytic degradation rate was 75.06%.
[0227] Example 17
[0228] 1. A piezoelectric ceramic catalyst, comprising the following raw materials in parts by weight:
[0229] 80 parts barium oxide, 20 parts calcium oxide, 90 parts titanium oxide, 10 parts zirconium oxide, 0.1 parts cerium oxide, and 0.05 parts aluminum oxide;
[0230] Its preparation method includes the following steps: same as in Example 9.
[0231] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0232] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0233] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0234] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100mL, and 10mg / L was 79.94%, and the piezoelectric catalytic degradation rate was 73.98%.
[0235] Example 18
[0236] 1. A piezoelectric ceramic catalyst, comprising the following raw materials in parts by weight: same as in Example 9;
[0237] Its preparation method includes the following steps:
[0238] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 120 minutes. After ball milling, dry in a forced-air drying oven at 80°C, then grind in an agate mortar and pestle, and pass through a 60-mesh sieve to obtain raw material powder.
[0239] Step 2, Firing: The raw material powder is pressed into ceramic green body using a tablet press, and then fired at 1300℃ for 60 minutes to obtain ceramic block;
[0240] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 30℃ and 2KV / mm for 20min using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0241] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0242] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0243] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0244] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100mL, and 10mg / L was 65.89%, and the piezoelectric catalytic degradation rate was 64.65%.
[0245] Example 19
[0246] 1. A piezoelectric ceramic catalyst, comprising the following raw materials in parts by weight: Same as in Example 1
[0247] Its preparation method includes the following steps:
[0248] Step 1, ball milling: Weigh each raw material according to the proportion, then place each raw material in a ball mill jar, add an equal weight of anhydrous ethanol and 5 times the mass of zirconium oxide beads, and ball mill for 30 hours. After ball milling, dry in a forced-air drying oven at 80℃, then grind in an agate mortar and pestle, and pass through a 60-mesh sieve to obtain raw material powder.
[0249] Step 2, Firing: The raw material powder is pressed into ceramic green body using a tablet press, and then fired at 1500℃ for 360 minutes to obtain ceramic block;
[0250] Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer, and then the electrode layer is cured at 500-700℃. Subsequently, it is polarized at 40℃ and 3KV / mm for 25 minutes using an oil bath polarization device to obtain the piezoelectric ceramic catalyst.
[0251] 2. A wastewater treatment method comprising photocatalysis and piezoelectric catalysis, wherein,
[0252] The photocatalysis process includes: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7 and 10mg / L, performing a dark reaction for 30min, then adding 2.4mmol / L of PMS oxidant, and performing photocatalytic degradation for 120min under light irradiation at a wavelength of 330-420nm; and detecting and calculating the photocatalytic degradation rate.
[0253] The piezoelectric catalyst comprises: adding 1.2g of the piezoelectric ceramic catalyst prepared in Example 9 to 100mL of methylene blue simulated wastewater at pH=7, and performing a dark reaction for 30min; then adding 2.4mmol / L of PMS oxidant; and performing piezoelectric catalytic degradation for 120min under ultrasonic conditions of 60-180W and 40kHz; and detecting and calculating the piezoelectric catalytic degradation rate.
[0254] In this embodiment, the photocatalytic degradation rate of methylene blue simulated wastewater at pH=7, 100mL, and 10mg / L was 69.15%, and the piezoelectric catalytic degradation rate was 67.42%.
[0255] The embodiments described above are merely preferred embodiments of the present invention, and not an exhaustive list of all possible implementations of the present invention. Any obvious modifications made by those skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.
Claims
1. A wastewater treatment method, characterized in that, Includes the following steps: A piezoelectric ceramic catalyst was added to the wastewater, and a dark reaction was carried out for 30 min. Then an oxidant was added, and catalytic degradation was carried out under light irradiation of 300-500 nm wavelength and / or ultrasound of 60-180 W and 40 KHz to degrade the organic pollutants in the wastewater into carbon dioxide and water. The oxidant used is a persulfate oxidant; In the system, the concentration of persulfate oxidant is 0.2-6 mmol / L; The piezoelectric ceramic catalyst comprises the following raw materials in parts by weight: Barium oxide 70-90 parts, calcium oxide 10-30 parts, titanium oxide 70-95 parts, zirconium oxide 5-30 parts, cerium oxide 0.4 parts, aluminum oxide 0.05 parts.
2. The wastewater treatment method according to claim 1, characterized in that, The piezoelectric ceramic catalyst includes the following steps: Step 1, ball milling: Weigh each raw material according to the proportion, then place them in a ball mill jar, add anhydrous ethanol, and ball mill them. After ball milling, dry them, then grind them, and sieve them to obtain raw material powder. Step 2, firing: Press the raw material powder into ceramic green bodies, and then fire them at high temperature to obtain ceramic blocks; Step 3, Silver plating polarization: A layer of silver metal is printed on the surface of the fired ceramic block as an electrode layer. Then, the electrode layer is subjected to high-temperature curing and polarization treatment in sequence to obtain silver-plated piezoelectric ceramic, i.e., piezoelectric ceramic catalyst.
3. The wastewater treatment method according to claim 2, characterized in that, In step 1, add zirconium oxide beads at a ratio of 5 times the total weight of the raw materials and ball mill; the ball milling time is 1-36 h.
4. The wastewater treatment method according to claim 2, characterized in that, The grinding process uses an agate mortar and pestle; Drying is performed using a forced-air drying oven. Drying temperature is 80-100 o C; The sieving process uses a 60-100 mesh sieve.
5. A wastewater treatment method according to claim 2, characterized in that, In step 2, the high-temperature firing temperature is 1200-1600℃. o C, firing time is 60-480 min.
6. The wastewater treatment method according to claim 2, characterized in that, In step 3, the high-temperature curing temperature is 500-700°C. o C.
7. A wastewater treatment method according to claim 2, characterized in that, In step 3, the polarization is performed using an oil bath polarization device, and the parameters of the oil bath polarization device are set to 25-60. o C, 1-4 KV / mm, polarization time 20-30 min.
Citation Information
Patent Citations
Ceramic powder, piezoelectric ceramic, piezoelectric element, and electronic equipment
US20150255703A1