A visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst and its preparation method

By loading nano-g-C₃N₄ and Bi₂MoO₆ particles onto the surface of kaolin sheets, a Bi₂MoO₆/g-C₃N₄/kaolin composite material was constructed. This solved the problem of high electron-hole recombination rate of Bi₂MoO₆ photocatalyst under visible light, improved photocatalytic activity and degradation ability, and reduced preparation cost.

CN118892856BActive Publication Date: 2026-11-24NORTH CHINA UNIV OF WATER RESOURCES & ELECTRIC POWER +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410922548.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2026-11-24
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

Existing Bi₂MoO₆ photocatalysts exhibit high electron-hole recombination rates under visible light, limiting their photocatalytic activity. Furthermore, g-C₃N₄/kaolin composite materials show low photocatalytic degradation capabilities under visible light, and their preparation process is cumbersome and costly.

Method used

By loading nano-g-C₃N₄ and Bi₂MoO₆ particles onto the surface of kaolin sheets, a Bi₂MoO₆/g-C₃N₄/kaolin composite material was constructed. Using kaolin as a carrier and melamine as a precursor, a visible light-responsive composite photocatalytic material was prepared by adding bismuth-based narrow bandgap semiconductor Bi₂MoO₆ for modification through a combination of solid-state sintering and solvothermal methods.

Benefits of technology

The specific surface area and reactive sites of the composite material were increased, the visible light photocatalytic degradation performance was enhanced, the problem of high electron-hole recombination rate was solved, the preparation cost was reduced, and the stability and lifespan of the catalyst were improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892856B_ABST
    Figure CN118892856B_ABST
Patent Text Reader

Abstract

This invention relates to the fields of non-metallic mineral materials and environmental engineering technology, specifically to a visible light-responsive Bi₂MoO₆ / g-C₃N₄ / kaolin composite photocatalytic material and its preparation method. The visible light-responsive Bi₂MoO₆ / g-C₃N₄ / kaolin composite photocatalytic material consists of nano-g-C₃N₄ and Bi₂MoO₆ particles loaded on the surface of kaolin sheets. The average particle size of the Bi₂MoO₆ particles is 1–1.5 μm, and the nano-g-C₃N₄ particles are nanosheets with an average size of 2–5 μm. The mass ratio of kaolin to Bi₂MoO₆ in the composite photocatalytic material is [not specified in the original text]. The mass ratio of kaolin to nano-g-C3N4 is 0.4–1.2:1, and the mass ratio of kaolin to nano-g-C3N4 is 3:1.5–2. The preparation method involves using kaolin as a carrier and melamine, Bi(NO3)3·5H2O, and Na2MoO4·2H2O as precursors. Nano-g-C3N4 and Bi2MoO6 are loaded onto the surface of kaolin sheets via solid-state sintering and solvothermal methods. This invention utilizes Bi2MoO6 to modify the g-C3N4 / kaolin composite material, further increasing the specific surface area of ​​the nanocomposite material and adding a large number of reactive sites, which is beneficial to the efficient photocatalytic reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of non-metallic mineral materials and environmental engineering technology, specifically to a visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material and its preparation method. Background Technology

[0002] With the advancement of the national "dual-carbon" strategy, new requirements have been placed on the green transformation of building materials, water pollution control, and air purification. Currently, methods for treating pollutants in water bodies mainly include physical adsorption, chemical methods, biological methods, and photocatalysis. Physical adsorption is simple to operate, highly efficient, and low-cost, but the adsorbent materials often exhibit saturation and selectivity, failing to completely eliminate pollutants and potentially causing secondary pollution. Chemical methods are costly and efficient, but are prone to reacting with other substances, generating secondary pollution. Biological methods require specific environmental conditions and experimental equipment, and have long processing times. In contrast, photocatalysis is simple to operate, highly efficient in degrading organic pollutants, and does not generate secondary pollution, thus meeting the demands of green and efficient technological development. With in-depth research in the field of photocatalysis, the degradation of organic pollutants under visible light has become a research focus. Under sunlight irradiation, the synthesized g-C3N4 / kaolin binary composite material shows good degradation effects on organic pollutants, but its photocatalytic activity in the visible light range remains very low. Bi₂MoO₆, as a narrow-gap semiconductor material, possesses characteristics such as large specific surface area, non-toxicity, chemical stability, low cost, and tunable electronic structure, making it a promising visible-light-responsive photocatalyst. However, its photocatalytic activity is severely limited by its weak built-in electric field and high electron-hole recombination rate.

[0003] Patent application number 202010533764.2 discloses a g-C3N4-Bi2WO6 heterojunction photocatalytic hydrogen production material and its preparation method. Although a Z-type heterojunction is formed in the composite photocatalyst, achieving high-efficiency photocatalytic hydrogen production performance, the preparation process is complicated, the production cost is high, the catalyst only responds under simulated sunlight, and the application range is narrow. Summary of the Invention

[0004] To address the aforementioned issues, this invention proposes a method for synthesizing a g-C3N4 / kaolin composite material using kaolin as a carrier and melamine as a precursor. Furthermore, a heterostructure is constructed by adding bismuth-based narrow-bandgap semiconductor Bi2MoO6, thereby modifying the g-C3N4 / kaolin composite material to prepare a visible-light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material.

[0005] The technical solution of the present invention is as follows: a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, wherein the composite photocatalytic material is made by loading nano-g-C3N4 and Bi2MoO6 particles on the surface of kaolin sheets, wherein the average particle size of the Bi2MoO6 particles is 1-1.5 μm, the nano-g-C3N4 is a nanosheet, and the average size of the nano-g-C3N4 is 2-5 μm. In the composite photocatalytic material, the mass ratio of kaolin to Bi2MoO6 is 0.4-1.2:1, and the mass ratio of kaolin to nano-g-C3N4 is 3:1.5-2.

[0006] Furthermore, the kaolin is intercalated-exfoliated kaolin.

[0007] The method for preparing the intercalated-exfoliated kaolin is as follows:

[0008] Step A: Mix 3-5g of kaolin and 3-5g of urea, add 30-50mL of deionized water, and centrifuge at 10000-13000rpm for 10-15min at 40-60℃ to form a suspension;

[0009] Step B: After filtering and washing the suspension obtained in step A, dry it at 80°C to obtain a white product;

[0010] Step C: Add 20-40 mL of deionized water to the white product obtained in step B, and sonicate at 50-70°C for 6-10 min. During the sonication process, nitrogen gas is blown into the mixture for 5-6 min to obtain the mixture.

[0011] Step D: After filtering and washing the mixture obtained in step C, dry it at 80°C to obtain intercalated-exfoliated kaolin.

[0012] Explanation: Preparing kaolin into intercalated-exfoliated kaolin can better facilitate the loading of Bi2MoO6 / g-C3N4, thereby improving the composite photocatalytic effect of the product; under the action of ultrasound, the surface of intercalated-exfoliated kaolin becomes more active, and under the synergistic effect of nitrogen blowing, more pores can be formed in the intercalated-exfoliated kaolin, and the surface has more loading points, which is conducive to the subsequent loading of Bi2MoO6 particles and g-C3N4, thereby increasing the loading of intercalated-exfoliated kaolin and enhancing the overall performance of the composite material.

[0013] Furthermore, in step C, the ultrasonic frequency is 30–50 kHz, and the ultrasonic power density is 0.2–0.25 W / cm². 2 ;

[0014] Note: Excessive ultrasonic frequency and power density will break the product into fragments, which is detrimental to catalyst loading.

[0015] A method for preparing a visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material, using kaolin as a support and melamine, Bi(NO3)3·5H2O and Na2MoO4·2H2O as precursors, involves loading nano-g-C3N4 and Bi2MoO6 onto the surface of kaolin sheets via solid-state sintering and solvothermal methods, including the following steps:

[0016] S1. Mix kaolin sheets and melamine in a mass ratio of 3:4 and grind them in a mortar for 30-60 minutes.

[0017] S2. The mixture obtained in step S1 is calcined at a heating rate of 2.5 to 5 °C / min and kept at 525 to 575 °C for 3.9 to 4.1 h. After the holding time is completed, the product is ground to obtain the kaolin-supported g-C3N4 composite photocatalytic material.

[0018] S3. Dissolve 0.8-1.0g Bi(NO3)3·5H2O and 0.23-0.25g Na2MoO4·2H2O in 10-20mL of ethylene glycol respectively, and stir to form solution A and solution B.

[0019] S4. Then add 30-60 mL of anhydrous ethanol to solution A and stir continuously for 20-40 min to obtain solution C. Next, take 0.3-0.9 g of kaolin-supported g-C3N4 composite photocatalyst material from step S2 and add it to solution C. Continue stirring for 20-40 min to obtain solution D. Finally, add solution B to solution D and stir for 20-40 min to mix well.

[0020] S5. Transfer the suspension obtained in step S4 to a high-pressure reactor and maintain the reaction at 150-180°C for 6-12 hours.

[0021] S6. The product obtained in step S5 is filtered and washed with deionized water and anhydrous ethanol 2 to 4 times respectively. The obtained product is dried in an oven at 55 to 65°C for 10 to 12 hours and then ground to obtain the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material.

[0022] Explanation: This invention uses kaolin as a carrier to solve the aggregation problem of pure g-C3N4, thereby improving the adsorption capacity and photocatalytic performance of the composite material. Then, Bi2MoO6 is used to modify the g-C3N4 / kaolin composite material, which further increases the specific surface area of ​​the nanocomposite material and adds a large number of reactive sites, which is beneficial to the efficient photocatalytic reaction.

[0023] Furthermore, in step S4, the amount of kaolin-supported g-C3N4 composite photocatalyst material added is 0.5g;

[0024] Note: The product with the above-mentioned addition amount has better photocatalytic performance.

[0025] Further, in step S6, the Bi2MoO6 / g-C3N4 / kaolin composite material is ground until the specific surface area is 37-49 m². 2 / g, with pore size distribution in the range of 2–20 nm;

[0026] Note: The photocatalytic material with the above parameters performs better.

[0027] Furthermore, in step S4, solution C undergoes a mineralization treatment.

[0028] The mineralization process is as follows: A reducing mineralizing agent is prepared according to a mass ratio of solution C to reducing mineralizing agent of 1:0.5–0.8. The reducing mineralizing agent is then added dropwise to a reaction vessel containing solution C, with continuous stirring for 20–40 minutes during the addition process, generating product A. The surface of product A is washed 4–6 times sequentially with deionized water, air, and carbon dioxide, respectively. Finally, the reaction vessel is sealed and placed in a microwave hydrothermal reactor for reaction for 25–30 minutes to obtain the mineralized solution C. The microwave hydrothermal reactor is set to a temperature of 230–250℃ and a power of 100–150W.

[0029] Explanation: Mineralizing the bismuth nitrate solution before reacting it with sodium molybdate enhances its chemical stability. The resulting bismuth oxide exhibits higher chemical stability, facilitating a better reaction with sodium molybdate and resulting in a robust loading on the kaolin surface. Furthermore, the stable loading on the carbon-nitride-containing kaolin surface reduces catalyst loss during the reaction, thus improving catalytic efficiency and catalyst lifetime. In particular, the mineralization process introduces trace amounts of δ-Bi₂O₃ with a cubic fluorite structure and partially vacant oxygen ion positions in its lattice, resulting in very high oxygen ion conductivity. From a chemical bonding perspective, the oxygen ions of δ-Bi₂O₃ in the mineralized bismuth nitrate solution may form hydrogen bonds or other types of chemical bonds with the hydroxyl or oxygen-containing groups in the kaolin, thereby enhancing the bismuth ion loading effect.

[0030] Furthermore, the reducing mineralizer comprises, by mass percentage: 40-45% sodium hydroxide, 5-10% ammonium chloride, 5-7% sodium polyacrylate, and the balance being water;

[0031] Explanation: Sodium polyacrylate can improve the dispersibility of kaolin, thereby facilitating the loading of bismuth molybdate and carbon nitride on the kaolin surface; the addition of ammonium chloride can expand the kaolin, and when applied to molybdate solutions, it can increase the conductivity of the solution, which helps the extraction efficiency of molybdenum, thereby promoting the formation of bismuth molybdate and further improving the loading effect; in addition, ammonium chloride itself can also be used as a chemical swelling agent, generating gas through thermal decomposition to achieve the expansion effect of the material, thereby expanding the kaolin and further promoting the loading effect of bismuth molybdate and carbon nitride on the kaolin surface.

[0032] Furthermore, the filling ratio of the microwave hydrothermal reactor is controlled to be 55-65%;

[0033] Note: At the above filling level, the reactor exhibits good mixing and heat transfer performance, while the reaction pressure is relatively low, which helps maintain the safety and stability of the reaction.

[0034] The beneficial effects of this invention are:

[0035] (1) The material of the present invention utilizes the visible light response and excellent specific surface area characteristics of Bi2MoO6. By modifying the g-C3N4 / kaolin composite material, the specific surface area of ​​the Bi2MoO6 / g-C3N4 / kaolin composite material is increased, so that the composite material has strong visible light photocatalytic degradation performance for pollutants, which solves the problem of high electron-hole recombination rate and low photocatalytic degradation ability of g-C3N4 / kaolin composite material under visible light.

[0036] (2) This invention uses kaolin as a carrier to solve the aggregation problem of pure g-C3N4 and improve the adsorption capacity and photocatalytic performance of the composite material. Then, Bi2MoO6 is used to modify the g-C3N4 / kaolin composite material, which further improves the specific surface area of ​​the nanocomposite material and increases a large number of reactive sites, which is conducive to the efficient photocatalytic reaction. Moreover, the raw materials required are inexpensive, the preparation process is simple, and the reaction conditions are mild, which has great application value in the fields of wastewater treatment and air purification.

[0037] (3) The present invention mineralizes the bismuth nitrate solution before reacting it with sodium molybdate, which helps it to react better with sodium molybdate and thus be firmly loaded on the kaolin surface. At the same time, on the kaolin surface where carbon nitride is present, the stable loading state can reduce the loss of catalyst during the reaction process, thereby improving the catalytic efficiency and catalyst life. Furthermore, the bismuth nitrate solution after mineralization has a cubic fluorite-type structure of δ-Bi2O3, which has some oxygen ion vacancies in its lattice, thus exhibiting very high oxygen ion conductivity. This structure can promote its interaction with the oxygen-containing groups on the kaolin surface. Moreover, from the perspective of chemical bonding, the trace oxygen ions in the δ-Bi2O3 in the mineralized bismuth nitrate solution may also form hydrogen bonds or other types of chemical bonds with the hydroxyl or oxygen-containing groups in the kaolin, thereby enhancing the loading effect of bismuth. Attached Figure Description

[0038] Figure 1 The XRD patterns are of kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin, Bi2MoO6 / kaolin, Bi2MoO6 / g-C3N4 and Bi2MoO6 / g-C3N4 / kaolin with different mass ratios in this invention.

[0039] Figure 2 SEM images of kaolin, intercalated-exfoliated kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin, and Bi2MoO6 / g-C3N4 / kaolin in this invention;

[0040] Figure 3 TEM images of g-C3N4 / kaolin and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts;

[0041] Figure 4 The N2 adsorption-desorption isotherms and pore size distribution diagrams of kaolin, g-C3N4, Bi2MoO6, and Bi2MoO6 / g-C3N4 / kaolin in this invention are shown.

[0042] Figure 5 The PL spectra of g-C3N4, Bi2MoO6, and Bi2MoO6 / g-C3N4 / kaolin in this invention are shown. Detailed Implementation

[0043] To further illustrate the methods and effects of this invention, the technical solution of this invention will be clearly and completely described below in conjunction with experiments.

[0044] Example 1: A visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material. The composite photocatalyst material is made by loading nano-g-C3N4 and Bi2MoO6 particles onto the surface of kaolin sheets. The average particle size of Bi2MoO6 particles is 1.3 μm, and the nano-g-C3N4 is a nanosheet with an average size of 3.5 μm. The mass ratio of kaolin to Bi2MoO6 in the composite photocatalyst material is 0.8:1, and the mass ratio of kaolin to nano-g-C3N4 is 3:1.8.

[0045] Kaolin is intercalated-exfoliated kaolin.

[0046] The preparation method of intercalated-exfoliated kaolin is as follows:

[0047] Step A: Mix 4g of kaolin and 4g of urea, add 40mL of deionized water, and centrifuge at 11500rpm for 13min at 50℃ to form a suspension;

[0048] Step B: After filtering and washing the suspension obtained in step A, dry it at 80°C to obtain a white product;

[0049] Step C: Add 30 mL of deionized water to the white product obtained in step B, and sonicate at 60 °C for 8 min. During the sonication process, nitrogen gas is blown into the mixture for 5 min to obtain the mixture.

[0050] Step D: After filtering and washing the mixture obtained in step C, dry it at 80°C to obtain intercalated-exfoliated kaolin.

[0051] The ultrasonic frequency in step C is 40 kHz, and the ultrasonic power density is 0.23 W / cm². 2 ;

[0052] A method for preparing a visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material, using kaolin as a support and melamine, Bi(NO3)3·5H2O and Na2MoO4·2H2O as precursors, involves loading nano-g-C3N4 and Bi2MoO6 onto the surface of kaolin sheets via solid-state sintering and solvothermal methods, including the following steps:

[0053] S1. Mix kaolin sheets and melamine in a mass ratio of 3:4 and grind them in a mortar for 45 minutes.

[0054] S2. The mixture obtained in step S1 is calcined at a heating rate of 3.5℃ / min and kept at 550℃ for 4 hours. After the heat preservation is completed, the product is ground to obtain the kaolin-supported g-C3N4 composite photocatalytic material.

[0055] S3. Dissolve 0.9g Bi(NO3)3·5H2O and 0.24g Na2MoO4·2H2O in 15mL of ethylene glycol, and stir to form solution A and solution B.

[0056] S4. Then, add 40 mL of anhydrous ethanol to solution A and stir continuously for 30 min to obtain solution C. Next, add 0.6 g of kaolin-supported g-C3N4 composite photocatalyst material from step S2 to solution C and stir for another 30 min to obtain solution D. Finally, add solution B to solution D and stir for 30 min to mix thoroughly. The amount of kaolin-supported g-C3N4 composite photocatalyst material added is 0.5 g.

[0057] S5. Transfer the suspension obtained in step S4 to a high-pressure reactor and maintain the reaction at 160°C for 8 hours.

[0058] S6. The product obtained in step S5 is filtered and washed three times each with deionized water and anhydrous ethanol. The obtained product is dried in an oven at 60°C for 12 hours. The resulting product is then ground to obtain the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material. The specific surface area of ​​the ground Bi2MoO6 / g-C3N4 / kaolin composite material is 43 m². 2 / g, with pore size distribution in the range of 9-17nm;

[0059] In step S4, solution C is subjected to mineralization treatment.

[0060] The mineralization process is as follows: A reducing mineralizing agent is prepared according to a mass ratio of solution C to reducing mineralizing agent of 1:0.7. The reducing mineralizing agent is then added dropwise to a reaction vessel containing solution C, with continuous stirring for 30 minutes during the addition process, generating product A. This product A is then washed five times each with deionized water, air, and carbon dioxide. Finally, the reaction vessel is sealed and placed in a microwave hydrothermal reactor for 28 minutes to obtain the mineralized solution C. The microwave hydrothermal reactor is set to a temperature of 240℃ and a power of 125W, with a filling ratio of 60%. The microwave hydrothermal reactor is an existing product.

[0061] The reducing mineralizer, by weight percentage, comprises: 43% sodium hydroxide, 8% ammonium chloride, 6% sodium polyacrylate, and the balance being water.

[0062] Example 2: Unlike Example 1, the preparation method of intercalated-exfoliated kaolin is as follows:

[0063] Step A: Mix 3g of kaolin and 3g of urea, add 30mL of deionized water, and centrifuge at 10000rpm for 10min at 40℃ to form a suspension;

[0064] Step B: After filtering and washing the suspension obtained in step A, dry it at 80°C to obtain a white product;

[0065] Step C: Add 20 mL of deionized water to the white product obtained in step B, and sonicate at 50 °C for 10 min. During the sonication process, nitrogen gas is blown into the mixture for 5 min to obtain the mixture.

[0066] Step D: After filtering and washing the mixture obtained in step C, dry it at 80°C to obtain intercalated-exfoliated kaolin.

[0067] The ultrasonic frequency in step C is 30 kHz, and the ultrasonic power density is 0.2 W / cm². 2 .

[0068] Example 3: Unlike Example 1, the preparation method of intercalated-exfoliated kaolin is as follows:

[0069] Step A: Mix 5g of kaolin and 5g of urea, add 50mL of deionized water, and centrifuge at 13000rpm for 15min at 60℃ to form a suspension;

[0070] Step B: After filtering and washing the suspension obtained in step A, dry it at 80°C to obtain a white product;

[0071] Step C: Add 40 mL of deionized water to the white product obtained in step B, and sonicate at 70 °C for 6 min. During the sonication process, nitrogen gas is blown into the mixture for 6 min to obtain the mixture.

[0072] Step D: After filtering and washing the mixture obtained in step C, dry it at 80°C to obtain intercalated-exfoliated kaolin.

[0073] The ultrasonic frequency in step C is 50 kHz, and the ultrasonic power density is 0.25 W / cm². 2 .

[0074] Example 4: Unlike Example 1,

[0075] S1. Mix kaolin sheets and melamine in a mass ratio of 3:4 and grind them in a mortar for 30 minutes.

[0076] S2. The mixture obtained in step S1 is calcined at a heating rate of 2.5℃ / min and kept at 550℃ for 4.1h. After the holding time is completed, the obtained product is ground to obtain the kaolin-supported g-C3N4 composite photocatalytic material.

[0077] S3. Dissolve 0.8g Bi(NO3)3·5H2O and 0.23g Na2MoO4·2H2O in 10mL of ethylene glycol, and stir to form solution A and solution B.

[0078] S4. Then, add 30 mL of anhydrous ethanol to solution A and stir continuously for 20 min to obtain solution C. Next, add 0.3 g of kaolin-supported g-C3N4 composite photocatalyst material from step S2 to solution C and stir for another 20 min to obtain solution D. Finally, add solution B to solution D and stir for 20 min to mix thoroughly. The amount of kaolin-supported g-C3N4 composite photocatalyst material added is 0.3 g.

[0079] S5. Transfer the suspension obtained in step S4 to a high-pressure reactor and maintain the reaction at 150°C for 6 hours.

[0080] S6. The product obtained in step S5 is filtered and washed twice with deionized water and anhydrous ethanol, respectively. The obtained product is dried in an oven at 60°C for 12 hours. The resulting product is then ground to obtain the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material. The specific surface area of ​​the ground Bi2MoO6 / g-C3N4 / kaolin composite material is 37 m². 2 / g, with pore size distribution in the range of 2-8nm.

[0081] Example 5: Unlike Example 1,

[0082] S1. Mix kaolin sheets and melamine in a mass ratio of 3:4 and grind them in a mortar for 60 minutes.

[0083] S2. The mixture obtained in step S1 is calcined at a heating rate of 5℃ / min and kept at 550℃ for 4h. After the heat preservation is completed, the obtained product is ground to obtain the kaolin-supported g-C3N4 composite photocatalytic material.

[0084] S3. Dissolve 1.0gBi(NO3)3·5H2O and 0.25gNa2MoO4·2H2O in 20mL of ethylene glycol, and stir to form solution A and solution B.

[0085] S4. Then, add 50 mL of anhydrous ethanol to solution A and stir continuously for 40 min to obtain solution C. Next, add 0.9 g of kaolin-supported g-C3N4 composite photocatalyst material from step S2 to solution C and stir for another 40 min to obtain solution D. Finally, add solution B to solution D and stir for 40 min to mix thoroughly. The amount of kaolin-supported g-C3N4 composite photocatalyst material added is 0.7 g.

[0086] S5. Transfer the suspension obtained in step S4 to a high-pressure reactor and maintain the reaction at 170°C for 10 hours.

[0087] S6. The product obtained in step S5 is filtered and washed four times each with deionized water and anhydrous ethanol. The obtained product is dried in an oven at 60°C for 12 hours. The resulting product is then ground to obtain the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material. The specific surface area of ​​the ground Bi2MoO6 / g-C3N4 / kaolin composite material is 49 m². 2 / g, with pore size distribution in the range of 15-20nm.

[0088] Example 6: Unlike Example 1, the mineralization method is as follows: A reducing mineralizing agent is prepared according to a mass ratio of solution C to reducing mineralizing agent of 1:0.5. The reducing mineralizing agent is then added dropwise to a reaction vessel containing solution C, with continuous stirring for 20 minutes during the addition process, generating product A. This product A is washed four times sequentially with deionized water, air, and carbon dioxide. Finally, the reaction vessel is sealed and placed in a microwave hydrothermal reactor for 25 minutes to obtain the mineralized solution C. The microwave hydrothermal reaction temperature is set to 230℃, and the power is 100W. The filling ratio of the microwave hydrothermal reactor is controlled at 55%.

[0089] The reducing mineralizer, by weight percentage, comprises: 40% sodium hydroxide, 5% ammonium chloride, 5% sodium polyacrylate, and the balance being water.

[0090] Example 7: Unlike Example 1, the mineralization method is as follows: A reducing mineralizing agent is prepared according to a mass ratio of solution C to reducing mineralizing agent of 1:0.8. The reducing mineralizing agent is then added dropwise to a reaction vessel containing solution C, with continuous stirring for 40 minutes during the addition process, generating product A. This product A is washed six times sequentially with deionized water, air, and carbon dioxide. Finally, the reaction vessel is sealed and placed in a microwave hydrothermal reactor for 30 minutes to obtain the mineralized solution C. The microwave hydrothermal reactor is set to a temperature of 250°C and a power of 150W, with a filling ratio of 65%.

[0091] The reducing mineralizer, by weight percentage, comprises: 45% sodium hydroxide, 10% ammonium chloride, 7% sodium polyacrylate, and the balance being water.

[0092] Experimental example: XRD test

[0093] XRD analysis was performed on kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin, Bi2MoO6 / kaolin, Bi2MoO6 / g-C3N4, and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts with different mass ratios. Figure 1 As shown, the characteristic diffraction peaks of Bi2MoO6 can be clearly seen in the XRD pattern of the Bi2MoO6 / g-C3N4 / kaolin ternary composite material, proving that the ternary composite photocatalyst was successfully prepared.

[0094] SEM test

[0095] SEM analysis was performed on kaolin, intercalated-exfoliated kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin, and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 2 As shown in (a) and (b), pure kaolinite exhibits a book-like accumulation pattern, while the number of kaolinite aggregates after intercalation-exfoliation is significantly reduced, and the number of thin kaolinite flakes increases. Figure 2 As shown in (c), the morphology of pure g-C3N4 exhibits a lamellar stacked structure with relatively large particle sizes. Figure 2 As shown in (d), the morphology of pure Bi₂MoO₆ is that of microspheres or flower-like structures with a diameter of 1–1.5 μm, and the aggregates are composed of nanospheres and nanosheets. Figure 2 As shown in (e), in the g-C3N4 / kaolin composite material, the aggregation phenomenon of g-C3N4 can be significantly improved, and the g-C3N4 nanoparticles can be well dispersed on the kaolin sheets. Figure 2 As shown in (f), the Bi2MoO6 / g-C3N4 / kaolin composite material exhibits a particle packing morphology with many Bi2MoO6 fragments loaded on its surface.

[0096] TEM test

[0097] TEM analysis was performed on the g-C3N4 / kaolin and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 3 As shown in (a), in the g-C3N4 / kaolin binary composite material, kaolin and g-C3N4 are tightly bonded, which increases the specific surface area of ​​the material and provides more active sites for photocatalytic reactions. Figure 3 As shown in (b), in the Bi2MoO6 / g-C3N4 / kaolin ternary composite material, kaolin, g-C3N4 nanosheets and Bi2MoO6 nanosheets form a heterojunction structure through coupling, which further confirms the formation of the ternary composite material structure.

[0098] BET test

[0099] BET analysis was performed on kaolin, g-C3N4, Bi2MoO6, and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 4As shown in (a) and (b), compared with pure g-C3N4 and kaolin, the Bi2MoO6 / g-C3N4 / kaolin composite material has an increased number of mesopores with a pore size distribution in the range of 2-20 nm, which is beneficial to promoting the adsorption and diffusion of target reactants.

[0100] PL test

[0101] PL analysis was performed on g-C3N4, Bi2MoO6, and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 5 As shown, the fluorescence intensity of the Bi2MoO6 / g-C3N4 / kaolin composite material is low, indicating that the introduction of kaolin and the formation of the Bi2MoO6 / g-C3N4 heterojunction can effectively improve the separation efficiency of electron-hole pairs.

[0102] The performance and parameters of the final products in Examples 1 to 7 were tested and calculated according to the methods described below, and the results are listed in Table 1.

[0103] Photocatalytic Degradation Performance of Tetracycline Wastewater: Tetracycline is widely used and consumed in large quantities, making it one of the major antibiotic pollutants. Therefore, tetracycline was selected as the target liquid-phase pollutant to test the degradation performance of the sample on antibiotic wastewater. Under specific conditions, the lower the absorbance of tetracycline, the better the photocatalytic degradation performance of the composite material. In this specific embodiment, the concentration of the tetracycline solution used was 30 mg / L. Each time, 50 mL of tetracycline solution was mixed with 0.04 g of product and ultrasonically dispersed for 5 min. After a dark reaction of 1 h, a 500 W xenon lamp was turned on for photocatalytic reaction. Samples were taken periodically, with 3 mL of solution extracted each time. The catalyst was filtered out using a 0.22 μm filter membrane, and the absorbance C of the tetracycline solution at a wavelength of 355 nm was accurately measured using an ultraviolet spectrophotometer. The removal rate of the tetracycline solution was then calculated using the formula: Removal rate = (C0 - C) / ... t ) / C0×100%, where C0 is the absorbance value of the initial tetracycline solution, C t This is the absorbance value of the tetracycline solution when the reaction is complete.

[0104] Determination of Adsorption-Photocatalytic Degradation Performance of Formaldehyde Gas: Formaldehyde is a volatile organic pollutant widely present in the air, which greatly reduces indoor air quality and causes irreversible damage to human health. Therefore, formaldehyde is used as the target gaseous pollutant to further evaluate the visible light photocatalytic performance of the material. The formaldehyde reaction device mainly consists of a 0.125L reaction chamber, a light source, a heating device, a fan, an injection port, a sampling pump, a formaldehyde detector, and a CO2 detector. The light source consists of three 8W LED lamps. The lifting platform is located directly below the light source. A glass dish coated with the sample is placed on the lifting platform, and the distance between the sample and the light source is adjusted to 15cm. The heating device and the fan mainly facilitate the dispersion and uniformity of formaldehyde. In this specific embodiment, the initial concentration of formaldehyde gas used is approximately 1.54ppm. 750mg of catalyst is evenly coated onto the glass dish, dried, and then placed in the reaction chamber. After 60 minutes of dark adsorption, the lamps are turned on to initiate the photocatalytic reaction process. Formaldehyde and CO2 concentrations are measured in real time using formaldehyde and CO2 detectors, and data is recorded periodically. The formaldehyde removal rate is then calculated using the formula: Removal Rate = (C0 - C...) t Ct = (C0) / C0 × 100%, where C0 is the initial formaldehyde concentration (ppm) and Ct is the formaldehyde concentration (ppm) when the reaction is complete.

[0105] Table 1. Performance and parameters of kaolin, g-C3N4, Bi2MoO6, and the final products of Examples 1-7 and Comparative Examples 1-3.

[0106]

[0107] The difference between Comparative Example 1 and Example 1 is that nitrogen blowing is not performed during the preparation of intercalated-exfoliated kaolin.

[0108] The difference between Comparative Example 2 and Example 1 is that solution C is not mineralized.

[0109] The difference between Comparative Example 3 and Example 1 is that the reducing mineralizer does not contain ammonium chloride.

[0110] Conclusion: Table 1 shows that the catalytic performance of the composite photocatalyst material obtained without nitrogen blowing in Control Example 1 is slightly reduced. Under the combined effects of nitrogen blowing and ultrasonic treatment, the surface of kaolin becomes more active and porous, which is beneficial for the loading of Bi2MoO6 particles and g-C3N4, thus improving the loading of intercalated-exfoliated kaolin and enhancing the overall performance of the composite material. Furthermore, nitrogen blowing and ultrasonic treatment may help improve the interfacial bonding ability of intercalated-exfoliated kaolin, promoting the interfacial bonding energy between Bi2MoO6 particles, g-C3N4, and kaolin. A good interfacial bond can reduce the internal resistance between materials and improve charge transport efficiency, thereby enhancing the photocatalytic performance of the composite material. In Comparative Example 2, the lack of mineralization treatment of the bismuth nitrate solution affects the catalytic performance of the composite photocatalytic material. This is because the present invention mineralizes the bismuth nitrate solution before reacting it with sodium molybdate, which helps it react better with sodium molybdate and thus firmly load it onto the kaolin surface. Simultaneously, on the kaolin surface containing carbon nitride, a stable loading state can reduce catalyst loss during the reaction process, thereby improving catalytic efficiency and catalyst lifetime. Furthermore, the mineralized bismuth nitrate solution contains a small amount of δ-Bi₂O₃ with a cubic fluorite mineral structure. Its lattice has some oxygen ion vacancies, thus exhibiting very high oxygen ion conductivity. This structure can promote its interaction with oxygen-containing groups on the kaolin surface, thereby improving the composite photocatalytic effect. Moreover, the composite material prepared in this application has strong visible light photocatalytic degradation performance for pollutants, solving the problem of high electron-hole recombination rate and low photocatalytic degradation ability of the g-C₃N₄ / kaolin composite material under visible light. Comparative Example 3 does not contain chlorine. Ammonium chloride can weaken the catalytic performance of composite photocatalytic materials. This is mainly because the addition of ammonium chloride can expand kaolinite. When applied to molybdate solutions, it can increase the conductivity of the solution, which helps to improve the extraction efficiency of molybdenum and thus promotes the formation of bismuth molybdate, thereby improving the loading effect. In addition, ammonium chloride itself can also be used as a chemical swelling agent. It can expand the material by generating gas through thermal decomposition, thereby expanding kaolinite and further promoting the loading effect of bismuth molybdate and carbon nitride on the surface of kaolinite. Therefore, this application has significant progress compared with the prior art.

Claims

1. A visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, characterized in that, The composite photocatalytic material is made by loading nano-g-C3N4 and Bi2MoO6 particles onto the surface of kaolin sheets. The average particle size of the Bi2MoO6 particles is 1~1.5µm, and the nano-g-C3N4 particles are nanosheets with an average size of 2~5µm. The mass ratio of kaolin to Bi2MoO6 in the composite photocatalytic material is 0.4~1.2:1, and the mass ratio of kaolin to nano-g-C3N4 is 3:1.5~2. The kaolin is intercalated-exfoliated kaolin. The method for preparing the intercalated-exfoliated kaolin is as follows: Step A: Mix 3-5g of kaolin and 3-5g of urea, add 30-50mL of deionized water, and centrifuge at 10000-13000rpm for 10-15min at 40-60℃ to form a suspension; Step B: After filtering and washing the suspension obtained in step A, dry it at 80°C to obtain a white product; Step C: Add 20-40 mL of deionized water to the white product obtained in step B, and sonicate at 50-70°C for 6-10 min. During the sonication process, nitrogen gas is blown into the mixture for 5-6 min to obtain the mixture. Step D: After filtering and washing the mixture obtained in step C, dry it at 80°C to obtain intercalated-exfoliated kaolin. The preparation method of the visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material is as follows: using kaolin as a carrier, and melamine, Bi(NO3)3•5H2O and Na2MoO4•2H2O as precursors, nano-g-C3N4 and Bi2MoO6 are loaded onto the surface of kaolin sheets by solid-state sintering and solvothermal methods, including the following steps: S1. Mix kaolin sheets and melamine in a mass ratio of 3:4 and grind them in a mortar for 30-60 minutes. S2. The mixture obtained in step S1 is calcined at a heating rate of 2.5~5℃ / min and kept at 525~575℃ for 3.9-4.1h. After the holding time is completed, the product is ground to obtain the kaolin-supported g-C3N4 composite photocatalytic material. S3. Dissolve 0.8~1.0g Bi(NO3)3•5H2O and 0.23~0.25g Na2MoO4•2H2O in 10~20mL of ethylene glycol respectively, and stir to form solution A and solution B. S4. Then add 30-60 mL of anhydrous ethanol to solution A and stir continuously for 20-40 min to obtain solution C. Mineralize solution C. Then take 0.3-0.9 g of kaolin-supported g-C3N4 composite photocatalyst material from step S2 and add it to the mineralized solution C. Continue stirring for 20-40 min to obtain solution D. Finally, add solution B to solution D and stir for 20-40 min to mix well. The mineralization process is as follows: A reducing mineralizing agent is prepared according to a mass ratio of solution C to reducing mineralizing agent of 1:0.5~0.

8. The reducing mineralizing agent is then added dropwise to a reaction vessel containing solution C, with continuous stirring for 20~40 minutes during the addition process, generating product A. The surface of product A is washed 4~6 times sequentially with deionized water, air, and carbon dioxide, respectively. Finally, the reaction vessel is sealed and placed in a microwave hydrothermal reactor for reaction for 25~30 minutes to obtain the mineralized solution C. The microwave hydrothermal reactor is set to a temperature of 230~250℃ and a power of 100~150W. The reducing mineralizer comprises, by mass percentage: 40-45% sodium hydroxide, 5-10% ammonium chloride, 5-7% sodium polyacrylate, and the balance being water; S5. Transfer the suspension obtained in step S4 to a high-pressure reactor and maintain the reaction at 150~180℃ for 6~12h. S6. Filter the product obtained in step S5 and wash it with deionized water and anhydrous ethanol 2 to 4 times in sequence. Dry the obtained product in an oven at 55-65℃ for 10 to 12 hours. After grinding, the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material is obtained.

2. The visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material as described in claim 1, characterized in that, The ultrasonic frequency in step C is 30~50kHz, and the ultrasonic power density is 0.2~0.25W / cm². 2 .

3. The visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material as described in claim 1, characterized in that, In step S4, the amount of kaolin-supported g-C3N4 composite photocatalyst material added is 0.5g.

4. The visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material as described in claim 1, characterized in that, In step S6, the Bi2MoO6 / g-C3N4 / kaolin composite material is ground until its specific surface area is 37~49 m². 2 / g, with pore size distribution in the range of 2~20nm.

5. The visible light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalyst material as described in claim 1, characterized in that, The filling ratio of the microwave hydrothermal reactor is controlled to be 55-65%.

Citation Information

Patent Citations

  • G-C3N4-Bi2WO6 heterojunction photocatalytic hydrogen production material and preparation method thereof

    CN111659441A

  • Preparation method of ultrafine silane surface grafted kaolinite powder body

    CN103864084A

  • Method for preparing bismuth sulfide / montmorillonite composite material by hydrothermal method

    CN104891514A

  • Preparation method and application of bismuth molybdate / graphite-phase carbon nitride composite catalyst

    CN106076389A