Preparation and application of bismuthyl bromide / phosphotungstic polyacid composite material
Patent Information
- Application Number
- CN202410920328.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
Smart Images

Figure HDA0004936493380000011 
Figure HDA0004936493380000012 
Figure HDA0004936493380000021
Abstract
Description
Technical Field
[0001] The invention relates to the preparation and application of a bismuth oxybromide / phosphotungstic polyacid composite material. Background Art
[0002] Polyoxometalates (POMs), or polyacids for short, are nano-sized electron-rich inorganic metal oxygen-containing clusters composed of pre-transition metals (Mo, W, V, Nb, Ta) coordinated with oxygen atoms. Polyacids have rich structures and diverse compositions, and their composition, structure and charge density can be adjusted by changing the types of heteroatoms. More importantly, polyacids have a similar energy band structure to metal oxide semiconductor photocatalytic materials, especially tungsten-based heteropolyacids have strong redox ability under light excitation, and are suitable for photocatalytic reactions. At the same time, polyacid anions can be compounded with other semiconductor materials by electrostatic adsorption to form polyacid-based composite materials with novel structures and excellent functions.
[0003] Bismuth-based compounds have attracted extensive attention in the fields of photocatalytic water splitting, pollutant photodegradation, and photocatalytic carbon dioxide reduction due to their unique anisotropic structure and good optical properties. Among them, bismuth oxybromide (BiOBr) has a weak Bi-O bond and is easy to form a capture center for photogenerated electrons, which can promote the separation of charge carriers and show good visible light capture and electron transport capabilities. At the same time, for layered BiOBr materials, in their staggered layer structure, the positive [B i2 O2] 2+ An internal electrostatic field can be established between the plate layer and the negative halogen ion plate layer, which can promote the separation and transmission of photogenerated electrons and holes, thereby accelerating the separation of photocarriers and showing good photoelectric properties. In addition, BiOBr can form a nanoflower-like structure with a large specific surface area, stable structure, simple material preparation process, and environmental friendliness. Therefore, through the solvent-thermal preparation method, the first functional composite of BiOBr and phosphotungstic polyacid material is realized, and bismuth oxybromide / phosphotungstic polyacid BiOBr nanoflower-like composite semiconductor photocatalytic material is obtained, which can solve the problem of easy aggregation and dissolution of polyacids, enhance the photocatalytic ability of BiOBr semiconductors, and provide a direction for the preparation and application of polyacid-based BiOBr photocatalytic composite materials. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of poor light absorption, narrow bandgap, easy recombination of photogenerated carriers, etc. caused by easy agglomeration of polyacids in existing polyacid-based composite materials, and to overcome the difficulties of low photocatalytic efficiency and inconvenient application of hydrogen-producing materials.
[0005] The present invention provides a method for preparing phosphotungstic acid: K3[PW 12 O 40 ]·13H2O (abbreviated as PW12 The invention relates to the preparation and application of a bismuth oxybromide / phosphotungstic polyacid composite material, and obtains a three-dimensional nano-flower-like composite photocatalytic material in which the phosphotungstic polyacid is uniformly attached to the surface of BiOBr. The chemical formula of the composite material is BiOBr / nK3[PW 12 O 40 ]·13H2O(abbreviated as BiOBr / nPW 12 , n is the number of PWs to join 12 mass in grams).
[0006] BiOBr / nPW 12 The synthesis of the composite material is completed in the following steps:
[0007] 1. Preparation of phosphotungstic acid: Dissolve Na2WO4·2H2O and Na2HPO4·2H2O in hot water, and add an appropriate amount of HCl aqueous solution dropwise under heating and stirring conditions, then cool the solution and filter it. At room temperature, add a certain amount of KCl to the filtrate, stir until the solution becomes a white suspension, filter it, and wash the white filter residue with dilute hydrochloric acid solution several times. After drying the filter residue, phosphotungstic acid K3[PW 12 O 40 ]·13H2O (PW 12 );
[0008] 2. Preparation of composite materials: Add Bi(NO)3·5H2O to ethylene glycol (EG) and stir until Bi(NO)3·5H2O is completely dissolved. Then add KBr and different amounts of PW 12 After stirring for a while, the mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave and heated. After cooling the autoclave, the sample was centrifuged and washed. Vacuum freeze-dried for 8 hours. 12 O 40 ]·13H2O(abbreviated as BiOBr / nPW 12 , n is the number of PWs to join 12 mass in grams).
[0009] The hot water in step 1 is 150 mL of deionized water with a temperature range of 95° C. to 110° C.
[0010] The mass ratio of Na2WO4·2H2O to Na2HPO4·2H2O described in step 1 is (0.8-1.2):(1.5-1.7), (unit: gram).
[0011] The appropriate amount of HCl aqueous solution described in step 1 is 0.5-0.7 mol / L, and the volume is 75-85 mL of hydrochloric acid aqueous solution.
[0012] The mass of the certain amount of KCl described in step 1 is 4 to 6 grams.
[0013] The molar concentration of the dilute hydrochloric acid solution described in step 1 is 0.1-0.3 mol / L.
[0014] The volume of ethylene glycol described in step 2 is 75-85 mL.
[0015] The molar ratio of Bi(NO)3·5H2O to KBr in step 2 is (0.8-1.2):(1-1.2) (unit: mol).
[0016] Different amounts of PW as described in step 2 12 , and the mass ratios of Bi(NO)3·5H2O are (0.8~1.2):(0.5~1.5); (0.8~1.2):(1.5~2.5); (0.8~1.2):(2.5~3.5), respectively (unit: g).
[0017] The heating described in step 2 has a heating temperature of 155-165° C. and a heating time of 710-730 minutes.
[0018] Compared with the prior art, the present invention has the following characteristics:
[0019] 1. The present invention is the first to prepare BiOBr / nPW by solvothermal method 12 Composite photocatalyst. BiOBr / nPW 12 The composite photocatalyst is in the shape of nanoflowers. The nanoflower-like structure formed by the cross-lamellar structure increases the specific surface area of the material. The combination of BiOBr nanoflowers and phosphotungstic acid enhances the electron transmission ability of the catalyst and improves the light response rate. The phosphotungstic acid is evenly attached to the surface of the BiOBr nanoflower layer, which improves the light capture ability and effectively promotes the charge separation of the composite material.
[0020] Second, the present invention uses in-situ loading to make the phosphotungstic acid evenly dispersed and stably attached to the surface of the BiOBr nanoflower sheet. This solves the problem that the phosphotungstic acid is easy to dissolve and agglomerate during the catalytic reaction. The present invention is the first example of the application of bismuth oxybromide / phosphotungstic acid composite material in photocatalytic hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope image of BiOBr semiconductor material.
[0022] Figure 2 BiOBr / 0.05PW 12 Scanning electron microscopy images of the composite materials.
[0023] Figure 3 BiOBr / 0.1PW 12 Scanning electron microscopy images of the composite materials.
[0024] Figure 4 BiOBr / 0.15PW 12 Scanning electron microscopy images of the composite materials.
[0025] Figure 5 BiOBr and BiOBr / 0.1PW 12 Infrared spectra of the composite materials.
[0026] Figure 6 BiOBr and BiOBr / 0.1PW 12 XRD patterns of the composite materials.
[0027] Figure 7 BiOBr and BiOBr / 0.1PW 12 The hydrogen production rate of the composite material in a sacrificial agent system (0.35 mol / L Na2S and 0.25 mol / L Na2SO3) and irradiated by a 300W xenon lamp for 6 hours at room temperature and pressure.
[0028] Figure 8 BiOBr and BiOBr / 0.1PW 12 Electrochemical impedance Nyquist plot of the composite material. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0030] Implementation Case 1
[0031] This embodiment is a preparation case of nanoflower-shaped bismuth oxybromide, which is prepared according to the following method:
[0032] Bi(NO)3·5H2O (5mmol) was dissolved in 80mL ethylene glycol solution, and KBr (5mmol) was added. The mixture was stirred for 0.5 hours to fully dissolve the first two raw materials. After stirring the mixed solution for 30 minutes, it was transferred to a 100mL polytetrafluoroethylene-lined autoclave and kept at 160°C for 12 hours. After natural cooling, it was centrifuged, washed with ethanol three times, and freeze-dried in a -50°C vacuum freeze dryer for 12 hours to obtain BiOBr.
[0033] Implementation Case 2
[0034] This embodiment provides a bismuth oxybromide / phosphotungstic acid composite material, which is prepared according to the following method:
[0035] (1) Preparation of phosphotungstic acid: 10 g Na2WO4·2H2O and 16 g Na2HPO4·2H2O were dissolved in 150 mL boiling water. Under stirring conditions, 80 mL of 0.6 mol / L concentrated HCl solution was added dropwise. After the HCl solution was added, the solution was heated and stirred for 20 minutes. The solution was cooled, 5 g KCl was added, and the solution was stirred until it became a white suspension. Then, it was filtered and the white residue was washed several times with 0.1 mol / L dilute hydrochloric acid solution. The residue was dried to obtain phosphotungstic acid K3[PW 12 O 40 ]·13H2O (PW 12 );
[0036] (2) Preparation of composite materials: Bi(NO)3·5H2O (5 mmol) was dissolved in 80 mL of ethylene glycol solution, and KBr (5 mmol) was added. The mixture was stirred for 0.5 h to allow the first two raw materials to fully dissolve. Then, 0.1 g of PW 12 After stirring the mixed solution for 30 minutes, it was transferred to a 100 mL polytetrafluoroethylene-lined autoclave and kept at 160°C for 12 hours. After natural cooling, it was centrifuged, washed with ethanol three times, and freeze-dried in a -50°C vacuum freeze dryer for 12 hours to obtain BiOBr / 0.1PW 12 Composite materials.
[0037] Comparative Case 1
[0038] This comparative example provides a bismuth oxybromide / phosphotungstic acid composite material, which is different from Example 2 in that: (2) Preparation of the composite material: Dissolve Bi(NO)3·5H2O (5 mmol) in 80 mL of ethylene glycol solution, add KBr (5 mmol), stir for 0.5 hours to fully dissolve the first two raw materials, add 0.05 g of PW 12 This comparison case can obtain BiOBr / 0.05PW 12 Composite materials.
[0039] Comparative Case 2
[0040] This comparative example provides a bismuth oxybromide / phosphotungstic acid composite material, which is different from Example 2 in that: (2) Preparation of the composite material: Dissolve Bi(NO)3·5H2O (5 mmol) in 80 mL of ethylene glycol solution, add KBr (5 mmol), stir for 0.5 hours to fully dissolve the first two raw materials, add 0.15 g of PW 12 This comparison case can obtain BiOBr / 0.15PW 12 Composite materials.
[0041] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0042] Figure 1 The figure shows a scanning electron microscope image of BiOBr. It is observed that the BiOBr semiconductor material is micrometer-sized, and multiple nanosheets are interspersed and stacked to form a nanoflower cluster structure.
[0043] Figure 2 BiOBr / 0.05PW shown 12 Scanning electron microscopy image of the composite material. It was observed that phosphotungstic acid had little adhesion to the nanoflower-shaped BiOBr and was unevenly attached to the surface of the BiOBr nanoflower.
[0044] Figure 3 BiOBr / 0.1PW shown 12 Scanning electron microscope images of the composite material show that the composite material is micron-sized, phosphotungstic acid is evenly attached to the surface of BiOBr nanosheets, and multiple sheet materials are irregularly combined and accumulated to form a nano-flower cluster structure with raised surfaces.
[0045] Figure 4 BiOBr / 0.15PW shown 12 Scanning electron microscope image of the composite material. It was observed that excess phosphotungstic acid aggregated on the surface of BiOBr, forming a rough bayberry-like structure, the nanoflower-like structure disappeared, the specific surface area was reduced compared to BiOBr, and the performance was greatly reduced.
[0046] Figure 5 Shown are BiOBr and BiOBr / 0.1PW 12 Infrared spectrum of the composite material. As shown in the figure, BiOBr nanomaterials have a wavelength of 700-1400 cm -1 There is almost no infrared characteristic peak in this range, while the infrared characteristic peak of phosphotungstic acid is obvious in this range. The composite material BiOBr / 0.1PW 12 Contains obvious infrared characteristic peaks of phosphotungstic acid.
[0047] Figure 6 Shown are BiOBr and BiOBr / 0.1PW 12 Comparing the XRD pattern of the composite material with the standard PDF card of BiOBr (PDF#09-0393 at the bottom), the BiOBr prepared by solvothermal method has higher purity, and the BiOBr / 0.1PW12 composite material also has obvious BiOBr characteristic peaks.
[0048] Figure 7 Shown are BiOBr and BiOBr / 0.1PW 12 The hydrogen production rate of the composite material under 0.35M Na2S and 0.25M Na2SO3 as sacrificial reagents for 6 hours at room temperature and pressure. 12 The average hydrogen production efficiency of the composite material is 533.68 μmol·g -1·h -1 , much higher than BiOBr monomer and other composite materials, but the addition of excessive phosphotungstic acid, a large amount of phosphotungstic acid surrounds the nanoflowers, reducing the photocatalytic performance. BiOBr / 0.1PW 12 It has good photocatalytic hydrogen production activity. Therefore, the addition of phosphotungstic acid in the present invention improves the photocatalytic efficiency of BiOBr, but the addition of too much phosphotungstic acid will cause the material to agglomerate and affect the catalytic performance. The BiOBr / 0.1PW12 composite material can be used as an efficient photocatalytic water decomposition catalyst.
[0049] Figure 8 Shown are BiOBr and BiOBr / 0.1PW 12 Electrochemical AC impedance Nyquist plot of the composite material. As shown in the figure, the composite material does not show an obvious semicircular structure in the high frequency region. The intersection of the curve and the x-axis is taken as the impedance of the composite material, representing the electronic conductivity of the material. The higher the slope of the curve, the better the electronic conductivity. As shown in the figure, BiOBr / 0.1PW 12 The composite material has stronger electron conduction ability, stronger separation effect of photogenerated electrons and photogenerated holes, and lower recombination rate.
[0050] In summary, the bismuth oxybromide / phosphotungstic acid composite material synthesized by the present invention has a main morphology of nanoflowers, and the addition of phosphotungstic acid enhances the material's light capture ability, electron transport ability, and photocatalytic water decomposition hydrogen production efficiency. Bismuth oxybromide loaded phosphotungstic acid flower-like materials have great application potential in photocatalytic water decomposition.
Claims
1. A preparation process of a bismuth oxybromide / phosphotungstic polyacid composite material, characterized in that: (1) Preparation of phosphotungstic acid: Na2WO4·2H2O and Na2HPO4·2H2O were dissolved in hot water, and an appropriate amount of HCl aqueous solution was added dropwise under heating and stirring conditions. The solution was then cooled and filtered. A certain amount of KCl was added to the filtrate at room temperature, and the solution was stirred until it became a white suspension, then filtered, and the white residue was washed several times with dilute hydrochloric acid solution. The residue was dried to obtain phosphotungstic acid K3[PW 12 O 40 ]·13H2O (PW 12 ); (2) Preparation of composite materials: Bi(NO)3·5H2O was added to ethylene glycol (EG) and stirred until Bi(NO)3·5H2O was completely dissolved. KBr and different amounts of PW were then added. 12 After stirring for a while, the mixed solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave and heated. After the autoclave cooled, the sample was centrifuged and washed. Vacuum freeze-dried for 8 hours. 12 O 40 ]·13H2O(abbreviated as BiOBr / nPW 12 , n is the number of PWs to join 12 mass in grams).
2. According to step (1) of claim 1, the mass ratio of Na2WO4·2H2O to Na2HPO4·2H2O is (0.8-1.2):(1.5-1.7), (unit: gram).
3. The hot water according to step (1) of claim 1 is 150 mL of deionized water with a temperature range of 95° C. to 110° C.
4. According to claim 1, the appropriate amount of HCl aqueous solution in step (1) is 0.5-0.7 mol / L HCl aqueous solution (total solution volume is 75-85 mL).
5. According to claim 1, the mass of the certain amount of KCl in step (1) is 4 to 6 grams; the molar concentration of the dilute hydrochloric acid solution is 0.1 to 0.3 mol / L.
6. According to claim 1, the volume of EG described in step (2) is 75-85 mL; the molar ratio of Bi(NO)3·5H2O to KBr is (0.8-1.2):(1-1.2).
7. The different amounts of PW according to step (2) of claim 1. 12 , and the mass ratios of Bi(NO)3·5H2O are (0.8~1.2):(0.5~1.5); (0.8~1.2):(1.5~2.5); (0.8~1.2):(2.5~3.5), respectively (unit: g).
8. According to the heating in step (2) of claim 1, the heating temperature is 155-165° C. and the heating time is 710-730 minutes.
9. The bismuth oxybromide / phosphotungstic polyacid composite material prepared by the preparation method of the composite material according to claims 1 to 8 is used for photocatalytic water decomposition to produce hydrogen at room temperature and pressure.
Citation Information
Patent Citations
BiOBr composite photo-catalytic material of three-dimensional flower-shaped structure modified by cuprous sulfide quantum dots
CN104226338A
Preparation method and application of bismuthyl bromide photocatalyst
CN107321369A
Preparation method of carbon nitride-polyacid charge transfer salt photocatalytic material
CN111250141A
Preparation method and catalytic application of carbon-coated potassium phosphotungstate-titanium dioxide composite material
CN111822049A
Oxygen vacancy-rich WO3 / BiOBr nanoflower photocatalyst as well as preparation method and application thereof