Super wear-resistant marble tile and preparation method thereof
Patent Information
- Application Number
- CN202410982794.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-05
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic tiles, and in particular relates to a super wear-resistant marble ceramic tile and a preparation method thereof. Background Art
[0002] There are many kinds of tiles used in the building materials industry, such as full-body tiles, glazed tiles, polished tiles, vitrified tiles, antique tiles, mosaics, matte tiles, and wood-grain tiles. The advantages of full-body tiles include high cost performance, easy transportation, easy cleaning, wear resistance and non-slip, while the disadvantages include single design and high technical requirements for preparation; the advantages of glazed tiles include rich colors, high gloss, environmental protection and no radiation, and a wide range of applications. Although the glaze surface of glazed tiles is smooth and beautiful, it is relatively easy to be scratched and worn, and the service life is relatively short. This may lead to more frequent replacements and more waste generation.
[0003] As consumers' requirements for personalized and aesthetic living environments continue to increase, polished glazed tiles, a decorative material with a smooth appearance and various colors, are becoming more and more popular. Marble tiles are a type of glazed tile that imitates marble texture and is currently a popular product among consumers. Marble tiles have always been popular in the market because they can restore the texture of natural marble with high clarity. However, people have found that after 8 to 10 years of laying and use, the glossiness of the surface of fully polished marble tiles has become lower, or there are obvious scratches. The scratch marks on the glaze are very obvious, and they appear in the shape of a "harlequin cat" under the refraction of light, which greatly reduces the aesthetic effect.
[0004] The currently disclosed technical solutions have improved the hardness and wear resistance of the marble porcelain glaze layer or body to a certain extent, mainly by optimizing the formula or introducing some other materials to improve the hardness and wear resistance of the glaze surface. This results in that it cannot fully consider the transparency, making the brick body prone to staining. This is because many glaze materials have many properties of their minerals changed after being ball-milled into glaze slurry. After being substituted into the formula and ball-milled, these materials that can improve the hardness will reduce the transparency of the glaze surface. In order to ensure the super transparency of marble tiles, these materials cannot be introduced too much, which will affect the use effect, so improvements are needed.
[0005] When pursuing the excellent performance of marble tile glaze, we should strive to achieve its multiple optimizations to ensure that it can not only improve its wear resistance, but also resist the scratches and wear of various hard objects in daily use, and maintain a long-lasting beauty; at the same time, the glaze surface must also achieve a high degree of transparency, which can truly restore the delicate texture and color of natural marble. In addition, crack resistance is also an indispensable key element. Through advanced formulas and process treatments, the tile glaze layer has good toughness while enhancing the hardness, effectively resisting the fine cracks caused by temperature changes, improper construction or external impacts, and ensuring the overall stability and service life of the tile. In summary, these comprehensive improvement measures are aimed at giving the marble tile more outstanding physical properties without changing the original noble and elegant temperament, so as to meet the extreme pursuit of modern home decoration for both beauty and practicality. Therefore, the optimization of the wear resistance, transparency and crack resistance of the marble tile glaze is the problem to be solved by the present invention. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art, one of the objects of the present invention is to provide a super wear-resistant marble tile, which can optimize the wear resistance, transparency and crack resistance of the marble tile glaze.
[0007] A super wear-resistant marble tile, comprising a body layer and a glaze layer coated on the body layer, the glaze layer comprising a surface glaze layer and a super wear-resistant polished glaze layer coated on the surface glaze layer, the super wear-resistant polished glaze layer comprising transparent corundum particles, quartz particles and modified basalt fibers.
[0008] Furthermore, the slurry of the green body layer includes 18-20 parts of albite, 16-18 parts of potassium feldspar, 7-9 parts of kaolin, 8-12 parts of quartz sand, 4-6 parts of high-alumina clay, 7-10 parts of corundum powder, 12-15 parts of calcined talc powder and 2-5 parts of zircon sand.
[0009] Furthermore, the slurry of the surface glaze layer includes 12 to 20 parts of potassium feldspar granite, 8 to 10 parts of kaolin, 10 to 12 parts of quartz sand, 1 to 3 parts of modified basalt fiber, 3 to 7 parts of hydroxymethyl cellulose, 5 to 10 parts of zinc oxide, 2 to 8 parts of talc, 8 to 15 parts of zircon sand and 5 to 12 parts of aluminum oxide.
[0010] Furthermore, the slurry of the super wear-resistant glaze layer includes 10-12 parts of potassium feldspar, 18-20 parts of sodium feldspar, 2-3 parts of limestone, 12-14 parts of calcined talc, 18-20 parts of barium carbonate, 5-7 parts of calcined zinc oxide, 8-10 parts of corundum powder, 18-20 parts of frit and 9-11 parts of kaolin.
[0011] Furthermore, the slurry of the super wear-resistant glaze layer also includes transparent corundum particles, quartz particles and modified basalt cellulose. The addition ratio of transparent corundum particles is 18% to 20% of the super wear-resistant glaze slurry, the addition ratio of quartz particles is 18% to 20% of the super wear-resistant glaze slurry, and the addition ratio of modified basalt cellulose is 5% to 10% of the super wear-resistant glaze slurry.
[0012] Furthermore, the particle size of the transparent corundum particles and the quartz particles is 150-250 μm.
[0013] Furthermore, the modified basalt fiber has a length of 5 to 10 mm.
[0014] A second object of the present invention is to provide a method for preparing super wear-resistant marble tiles.
[0015] The second object of the present invention is achieved by adopting the following technical solution:
[0016] The method for preparing the above-mentioned super wear-resistant marble tile comprises the following steps:
[0017] (1) weighing corresponding amounts of raw materials according to the green body composition formula, adding water and a debonding agent, and putting them into a ball mill for ball milling to obtain a green body slurry, and then sieving to remove iron, spray granulation, aging and homogenization, pressing and forming, and drying to obtain a green body for use;
[0018] (2) weighing corresponding amounts of raw materials according to the composition formula of the glaze layer, adding water, and putting them into a ball mill for ball milling to obtain a glaze slurry, which is then deironed and sieved for later use;
[0019] (3) weighing corresponding amounts of raw materials according to the composition formula of the super wear-resistant polishing glaze layer, adding water, and putting them into a ball mill for ball milling to obtain a glaze slurry, and then removing iron, sieving, and then adding the transparent corundum particles, quartz particles and modified basalt cellulose into the slurry, stirring evenly, and setting aside;
[0020] (4) Spread the glaze slurry prepared in step (2) on the body, with the weight controlled at 500-750 g / m 2 After printing, the super wear-resistant polishing glaze slurry is poured on the surface glaze layer, and the weight is controlled at 50-75g / m 2 ;
[0021] (5) The semi-finished product obtained in step (4) is placed in a kiln for sintering at a sintering temperature of 1170 to 1200° C. for a sintering time of 48 to 65 minutes.
[0022] Furthermore, in the step (3), the particle size of the residue after ball milling is controlled to be 0.5 to 1.5 μm.
[0023] Furthermore, in the steps (1), (2), and (3), the proportion of water added is 30% to 35%.
[0024] Furthermore, the amount of the disintegrator added in step (2) is 3% to 7% of the green body slurry.
[0025] Furthermore, the disintegrator is one of sodium tripolyphosphate and sodium hexametaphosphate.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention not only enables the ceramic tile to maintain good mechanical strength through the synergistic effect of various raw materials, but also improves the Mohs hardness grade and rupture modulus of the ceramic tile, that is, improves the wear resistance and crack resistance of the ceramic tile.
[0028] It should be particularly pointed out that the present invention optimizes the wear resistance, transparency and crack resistance of the marble tile glaze by adding transparent corundum particles, quartz particles, modified basalt cellulose and hydroxymethyl cellulose and then through the synergistic effect of each other. DETAILED DESCRIPTION
[0029] Below, in conjunction with specific embodiments, the present invention is further described. It should be noted that, under the premise of no conflict, the embodiments described below or the technical features can be arbitrarily combined to form new embodiments. The specific conditions not specified in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, unless otherwise specified, are conventional products obtained through commercial channels.
[0030] The preparation process of modified basalt cellulose includes the following steps: putting 0.8 kg of silane coupling agent into acetone, stirring for 30 minutes, putting in 2 kg of basalt fiber, ultrasonically dispersing for 35 minutes, filtering, washing the solid with chloroform, and drying to obtain the modified basalt fiber, wherein the weight ratio of the silane coupling agent to acetone is 1:12.
[0031] Example 1
[0032] A super wear-resistant marble tile comprises, from bottom to top, a body layer, a surface glaze layer and a super wear-resistant polishing glaze layer. The particle size of the transparent corundum particles and quartz particles in this embodiment is about 150 μm.
[0033] The method for preparing the super wear-resistant marble tile of this embodiment comprises the following steps:
[0034] (1) Weighing materials for preparing a ligand: 20 parts of albite, 16 parts of potassium feldspar, 9 parts of kaolin, 12 parts of quartz sand, 6 parts of high-alumina clay, 7 parts of corundum powder, 12 parts of calcined talc powder, and 2 parts of zircon sand, adding water and a disintegrator, wherein the water addition ratio is 35%, the disintegrator is sodium tripolyphosphate, and the sodium tripolyphosphate addition ratio is 3%, putting into a ball mill for ball milling to obtain a green body slurry, and then sieving to remove iron, spray granulation, aging and homogenization, pressing and molding, and drying to obtain a green body for standby use;
[0035] (2) Weigh the materials for preparing the glaze slurry: 20 parts of potassium feldspar granite, 10 parts of kaolin, 12 parts of quartz sand, 1 part of modified basalt fiber, 3 parts of hydroxymethyl cellulose, 5 parts of zinc oxide, 2 parts of talc, 15 parts of zircon sand, and 5 parts of aluminum oxide, add water in a ratio of 30%, put into a ball mill for ball milling to obtain the glaze slurry, and then remove iron and sieve for use.
[0036] (3) Weigh the materials for preparing super wear-resistant polishing glaze slurry: 10 parts of potassium feldspar, 18 parts of sodium feldspar, 2 parts of limestone, 12 parts of calcined talc, 19 parts of barium carbonate, 5 parts of calcined zinc oxide, 8 parts of corundum powder, 18 parts of frit and 9 parts of kaolin, add water, the water addition ratio is 30%, put into a ball mill for ball milling to obtain a glaze slurry, and then remove iron, sieve and add transparent corundum particles, quartz particles and modified basalt cellulose, the addition ratio of transparent corundum particles is 20%, the addition ratio of quartz particles is 20%, and the addition ratio of modified basalt cellulose is 8%, stir evenly to obtain a modified high hardness super wear-resistant polishing glaze slurry.
[0037] (4) Preparation of pattern texture: Use a glaze sprayer to evenly pour the glaze slurry obtained in step (2) on the body, and the weight is controlled at 750g / m 2 Then, the marble texture is printed on the glaze surface by screen printing, and the high-hardness and ultra-wear-resistant glaze slurry obtained in step (4) is evenly poured on the pattern, with the weight controlled at 50g / m 2 , semi-finished products are ready for use;
[0038] (5) Firing: The semi-finished product obtained in step (4) is placed in a kiln for sintering at a temperature of 1150° C. The firing cycle can be adjusted according to the length of the kiln and the firing time is controlled within 65 minutes.
[0039] Example 2
[0040] A super wear-resistant marble tile comprises, from bottom to top, a body layer, a surface glaze layer and a super wear-resistant polishing glaze layer. The particle size of the transparent corundum particles and quartz particles in this embodiment is about 180 μm.
[0041] The method for preparing the super wear-resistant marble tile of this embodiment comprises the following steps:
[0042] (1) Weighing materials for preparing a ligand: 18 parts of albite, 14 parts of potassium feldspar, 7 parts of kaolin, 8 parts of quartz sand, 4 parts of high-alumina clay, 10 parts of corundum powder, 15 parts of calcined talc, and 5 parts of zircon sand, adding water and a disintegrator, the water addition ratio is 30%, the disintegrator is sodium hexametaphosphate, the sodium hexametaphosphate addition ratio is 7%, putting into a ball mill for ball milling to obtain a green body slurry, and then sieving to remove iron, spray granulation, aging and homogenization, pressing and molding, drying to obtain a green body for standby use;
[0043] (2) Weigh the materials for preparing the glaze slurry: 15 parts of potassium feldspar granite, 8 parts of kaolin, 10 parts of quartz sand, 3 parts of modified basalt fiber, 5 parts of hydroxymethyl cellulose, 10 parts of zinc oxide, 8 parts of talc, 8 parts of zircon sand, and 12 parts of aluminum oxide, add water at a ratio of 35%, put into a ball mill for ball milling to obtain the glaze slurry, and then remove iron and sieve for use.
[0044] (3) Weigh the materials for preparing super wear-resistant polishing glaze slurry: 12 parts of potassium feldspar, 20 parts of sodium feldspar, 3 parts of limestone, 14 parts of calcined talc, 20 parts of barium carbonate, 7 parts of calcined zinc oxide, 10 parts of corundum powder, 20 parts of frit and 11 parts of kaolin, add water, the water addition ratio is 35%, put into a ball mill for ball milling to obtain a glaze slurry, and then remove iron, sieve and add transparent corundum particles, quartz particles and modified basalt cellulose, the addition ratio of transparent corundum particles is 18%, the addition ratio of quartz particles is 18%, and the addition ratio of modified basalt cellulose is 10%, stir evenly to obtain a modified high hardness super wear-resistant polishing glaze slurry.
[0045] (4) Use a glaze sprayer to evenly pour the glaze slurry obtained in step (2) on the body, with the weight controlled at 650 g / m 2 Then, the marble texture is printed on the glaze surface by screen printing, and the high-hardness and ultra-wear-resistant glaze slurry obtained in step (4) is evenly poured on the pattern, with the weight controlled at 60g / m 2 , semi-finished products are ready for use;
[0046] (5) The semi-finished product obtained in step (4) is placed in a kiln for sintering at a temperature of 1170° C. The sintering cycle can be adjusted according to the length of the kiln and the sintering time is controlled at 58 minutes.
[0047] Example 3
[0048] A super wear-resistant marble tile comprises, from bottom to top, a body layer, a surface glaze layer and a super wear-resistant polishing glaze layer. The particle size of the transparent corundum particles and quartz particles in this embodiment is about 250 μm.
[0049] The method for preparing the super wear-resistant marble tile of this embodiment comprises the following steps:
[0050] (1) Weighing materials for preparing a ligand: 19 parts of albite, 17 parts of potassium feldspar, 8 parts of kaolin, 10 parts of quartz sand, 5 parts of high-alumina clay, 8 parts of corundum powder, 14 parts of calcined talc, and 4 parts of zircon sand, adding water and a disintegrator, the water addition ratio is 32%, the disintegrator is sodium hexametaphosphate, the sodium hexametaphosphate addition ratio is 5%, putting into a ball mill for ball milling to obtain a green body slurry, and then sieving to remove iron, spray granulation, aging and homogenization, pressing and molding, drying to obtain a green body for standby use;
[0051] (2) Weigh the materials for preparing the glaze slurry: 12 parts of potassium feldspar granite, 9 parts of kaolin, 11 parts of quartz sand, 5 parts of modified basalt fiber, 7 parts of hydroxymethyl cellulose, 8 parts of zinc oxide, 5 parts of talc, 10 parts of zircon sand, and 8 parts of aluminum oxide, add water in a ratio of 32%, put into a ball mill for ball milling to obtain the glaze slurry, and then remove iron and sieve for use.
[0052] (3) Weigh the materials for preparing super wear-resistant polishing glaze slurry: 30 parts of albite, 15 parts of wollastonite, 15 parts of calcite, 15 parts of white jade, 5 parts of zinc oxide, 8 parts of aluminum oxide, 2 parts of nepheline, 5 parts of barium carbonate, and 5 parts of talc, add water, the water addition ratio is 30%, put into a ball mill for ball milling to obtain a glaze slurry, and then remove iron, sieve, and then add transparent corundum particles, quartz particles and modified basalt cellulose, the addition ratio of transparent corundum particles is 19%, the addition ratio of quartz particles is 19%, and the addition ratio of modified basalt cellulose is 5%, stir evenly to obtain a modified high-hardness super wear-resistant polishing glaze slurry.
[0053] (4) Use a glaze sprayer to evenly pour the glaze slurry obtained in step (2) on the body, with the weight controlled at 550 g / m 2 Then, the marble texture is printed on the glaze surface by rubber roller printing, and the high-hardness and ultra-wear-resistant glaze slurry obtained in step (4) is evenly poured on the pattern, and the weight is controlled at 75g / m 2 , semi-finished products are ready for use;
[0054] (5) The semi-finished product obtained in step (4) is placed in a kiln for sintering at a temperature of 1200° C. The sintering cycle can be adjusted according to the length of the kiln and the sintering time is controlled at 48 minutes.
[0055] Comparative Example 1
[0056] A super wear-resistant marble tile is basically the same as Example 1, except that the transparent corundum particles, quartz particles and modified basalt cellulose in step (3) are omitted.
[0057] Comparative Example 2
[0058] A super wear-resistant marble tile is basically the same as Example 1, except that the modified basalt cellulose in steps (2) and (3) is omitted.
[0059] Comparative Example 3
[0060] A super wear-resistant marble tile is basically the same as Example 1, except that the hydroxymethyl cellulose in step (2) is omitted.
[0061] Test Example 1
[0062] The ceramic tiles in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to performance tests (destructive strength, rupture modulus and Mohs hardness grade): the destructive strength of the ceramic tiles was measured in accordance with GB / T3810.4-2006 "Test methods for ceramic tiles - Part 4: Determination of rupture modulus and destructive strength"; the rupture modulus of the ceramic tiles was measured in accordance with GB / T3810.4-2006 "Test methods for ceramic tiles - Part 4: Determination of rupture modulus and destructive strength"; Mohs hardness grade: the ceramic tiles were placed stably on a hard support with the glaze facing upward, and standard minerals with different Mohs values from small to large were selected to scratch the surface of the ceramic tiles in turn, and the ceramic tile surface was scratched evenly and vertically with the edge of the mineral, and the lowest hardness value that could just produce obvious scratches was taken as the test result. The specific data are shown in Table 1.
[0063] Table 1
[0064] Example Destructive strength (N) Mohs hardness grade (grade) Modulus of rupture (MPa) Example 1 1975 5 64.3 Example 2 1978 5 64.8 Example 3 1983 5 65.7 Comparative Example 1 1968 3 47.3 Comparative Example 2 1967 4 41.2 Comparative Example 3 1966 5 43.5
[0065] It can be seen from Table 1 that the ultra-wear-resistant marble tiles of the present invention, through the synergistic effect of various raw materials, can not only maintain good mechanical strength of the tiles, but also improve the Mohs hardness grade and rupture modulus of the tiles, that is, improve the wear resistance and crack resistance of the tiles, wherein the destructive strength is 1975-1983N, the Mohs hardness is level 5, and the rupture modulus is 64.3-65.7MPa.
[0066] Combining Example 1 and Comparative Example 1, it can be seen that the destructive strength of the ceramic tile in Example 1 is 1975N, the Mohs hardness level is 5, and the rupture modulus is 64.3MPa, which is better than Comparative Example 1, indicating that it is more appropriate to add transparent corundum particles, quartz particles and modified basalt cellulose to the raw materials of the ceramic tile, which can not only maintain good mechanical strength of the ceramic tile, but also improve the Mohs hardness level and rupture modulus of the ceramic tile, that is, improve the wear resistance and crack resistance of the ceramic tile.
[0067] Combining Example 1 and Comparative Example 2, it can be seen that the destructive strength of the ceramic tile in Example 1 is 1975N, the Mohs hardness grade is 5, and the rupture modulus is 64.3MPa, which is better than Comparative Example 2, indicating that it is more appropriate to add modified basalt fiber to the raw materials of the ceramic tile, which not only can make the ceramic tile maintain good mechanical strength, but also improve the Mohs hardness grade and rupture modulus of the ceramic tile, that is, improve the wear resistance and crack resistance of the ceramic tile.
[0068] Combining Example 1 and Comparative Example 3, it can be seen that the destructive strength of the ceramic tile in Example 1 is 1975N, the Mohs hardness grade is 5, and the rupture modulus is 64.3MPa, which is better than Comparative Example 3, indicating that hydroxymethyl cellulose is more suitable for the raw materials of the ceramic tile, which can not only maintain good mechanical strength of the ceramic tile, but also improve the rupture modulus of the ceramic tile, that is, improve the wear resistance and crack resistance of the ceramic tile.
[0069] Combining Examples 1 to 3, it can be seen that the destructive strength of the ceramic tile in Example 3 is 1983N, the Mohs hardness grade is 5, and the rupture modulus is 65.7MPa, which is better than other examples, indicating that the addition amount of each component raw material in the formula in Example 3 is more appropriate, which can not only enable the ceramic tile to maintain good mechanical strength, but also improve the crack resistance of the ceramic tile and have a better rupture modulus. In addition, since transparent corundum particles are added to the super wear-resistant glaze layer, the transparency of the marble ceramic tile glaze is improved.
[0070] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A super wear-resistant marble tile, characterized in that: The super wear-resistant marble tile comprises a body layer and a glaze layer coated on the body layer, the glaze layer comprises a surface glaze layer and a super wear-resistant polished glaze layer coated on the surface glaze layer, and the super wear-resistant polished glaze layer comprises transparent corundum particles, quartz particles and modified basalt fibers.
2. The super wear-resistant marble tile according to claim 1, characterized in that: The slurry of the green body layer includes 18-20 parts of albite, 16-18 parts of potassium feldspar, 7-9 parts of kaolin, 8-12 parts of quartz sand, 4-6 parts of high-alumina clay, 7-10 parts of corundum powder, 12-15 parts of calcined talc powder and 2-5 parts of zircon sand.
3. The super wear-resistant marble tile according to claim 1, characterized in that: The slurry of the surface glaze layer includes 12-20 parts of potassium feldspar granite, 8-10 parts of kaolin, 10-12 parts of quartz sand, 1-3 parts of modified basalt fiber, 3-7 parts of hydroxymethyl cellulose, 5-10 parts of zinc oxide, 2-8 parts of talc, 8-15 parts of zircon sand and 5-12 parts of aluminum oxide.
4. The super wear-resistant marble tile according to claim 1, characterized in that: The slurry of the super wear-resistant glaze layer includes 10-12 parts of potassium feldspar, 18-20 parts of sodium feldspar, 2-3 parts of limestone, 12-14 parts of calcined talc, 18-20 parts of barium carbonate, 5-7 parts of calcined zinc oxide, 8-10 parts of corundum powder, 18-20 parts of frit and 9-11 parts of kaolin.
5. The super wear-resistant marble tile according to claim 4, characterized in that: The slurry of the super wear-resistant glaze layer also includes transparent corundum particles, quartz particles and modified basalt cellulose. The addition ratio of transparent corundum particles is 18% to 20% of the super wear-resistant glaze slurry, the addition ratio of quartz particles is 18% to 20% of the super wear-resistant glaze slurry, and the addition ratio of modified basalt cellulose is 5% to 10% of the super wear-resistant glaze slurry.
6. The super wear-resistant marble tile according to claim 5, characterized in that: The particle size of the transparent corundum particles and the quartz particles is 150-250 μm.
7. The method for preparing super wear-resistant marble tiles according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) weighing corresponding amounts of raw materials according to the green body composition formula, adding water and a debonding agent, and putting them into a ball mill for ball milling to obtain a green body slurry, and then sieving to remove iron, spray granulation, aging and homogenization, pressing and forming, and drying to obtain a green body for use; (2) weighing corresponding amounts of raw materials according to the composition formula of the glaze layer, adding water, and putting them into a ball mill for ball milling to obtain a glaze slurry, which is then deironed and sieved for later use; (3) weighing corresponding amounts of raw materials according to the composition formula of the super wear-resistant polishing glaze layer, adding water, and putting them into a ball mill for ball milling to obtain a glaze slurry, and then removing iron, sieving, and then adding the transparent corundum particles, quartz particles and modified basalt cellulose into the slurry, stirring evenly, and setting aside; (4) Spread the glaze slurry prepared in step (2) on the body, with the weight controlled at 500-750 g / m 2 After printing, the super wear-resistant polishing glaze slurry is poured on the surface glaze layer, and the weight is controlled at 50-75g / m 2 ; (5) The semi-finished product obtained in step (4) is placed in a kiln for sintering at a sintering temperature of 1170 to 1200° C. for a sintering time of 48 to 65 minutes.
8. The method for preparing super wear-resistant marble tiles according to claim 7, characterized in that: In the step (3), the particle size of the residue after ball milling is controlled to be 0.5 to 1.5 μm.
9. The method for preparing super wear-resistant marble tiles according to claim 7, characterized in that: In the steps (1), (2) and (3), the addition ratio of water is 30% to 35%.
10. The method for preparing super wear-resistant marble tiles according to claim 7, characterized in that: The amount of the disintegrating agent added in step (2) is 3% to 7% of the green body slurry.
Citation Information
Patent Citations
Efficient building ventilation equipment
CN219674412U
Automatic visual detection and laser rejection equipment for chips
CN219785648U
Wear-resistant domestic ceramic product and preparation method thereof
CN111574055A
High-wear-resistance marble-imitated ceramic tile and preparation method thereof
CN112592063A
Wear-resistant glaze material as well as preparation method and application thereof
CN113105266A
Cited By
Anti-fouling porcelain glaze and preparation method thereof
CN120136433A
Jade ceramic tile with soft fat effect and preparation method of jade ceramic tile
CN120607414A