Aerogel fireproof coating and preparation method thereof

CN118895077AInactive Publication Date: 2024-11-05HUNAN DEQIAN NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411400775.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides an aerogel fireproof coating and a preparation method thereof, and the aerogel fireproof coating comprises the following raw materials in parts by weight: 5-10 parts of modified aerogel, 5-10 parts of hollow porous micron-sized silicon spheres, 2-4 parts of carbon fibers, 50-55 parts of epoxy resin, 0.5-0.8 part of a defoaming agent and 5-8 parts of an epoxy curing agent. The preparation method comprises the following specific steps: grinding and mixing hollow porous micron-sized silicon balls and carbon fibers, ultrasonically mixing the mixture with modified aerogel, adding the mixture into epoxy resin, carrying out microwave heating and stirring, adding an epoxy curing agent and a defoaming agent, and continuously stirring to obtain the aerogel fireproof coating. According to the aerogel fireproof coating disclosed by the invention, the modified aerogel, the hollow porous micron-sized silicon spheres and the carbon fibers are added into the epoxy resin for synergistic interaction, so that the foaming ratio is increased, and the heat conduction coefficient is reduced, thereby improving the fireproof performance of the coating. Meanwhile, impact resistance, vibration resistance and mechanical damage resistance can be achieved, and long-term durability is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coatings, and in particular to an aerogel fire retardant coating and a preparation method thereof. Background Art

[0002] Cables are the main load-bearing and force-transmitting components of bridges, including main cables, slings and stay cables of suspension bridges, cable-stayed bridges and arch suspension bridges. Their safety and durability are related to the normal use and overall safety of bridges, and cable structures are the lifeline of bridges. Fire is a huge threat to cable safety. When a fire occurs in a tanker truck or a new energy vehicle, the temperature of the jet flame rises quickly and is high, reaching 1400°C in an instant.

[0003] At present, aerogel, a new material with the best thermal insulation performance in the industry, is a research hotspot. Patent CN208594481U provides an aerogel used in the anti-corrosion and thermal insulation of the main cable of a suspension bridge. It is sequentially provided with an aerogel layer, a winding steel wire layer, a primer layer, an intermediate paint layer, and a topcoat layer to reduce the influence of temperature effect on the safety factor of the main cable and extend the service life of the main cable. However, the aerogel layer is designed on the surface of the steel wire of the main cable of the suspension bridge, and then wrapped by the main cable winding wire, which will cause the aerogel to be squeezed and deformed or even damaged by the winding wire. Moreover, it is difficult to form a complete and dense layered protective structure after the aerogel is wrapped on the surface of the main cable steel wire, and its fireproof and even anti-corrosion performance cannot be guaranteed. Patent CN217536672U provides a bridge cable with an aerogel felt anti-corrosion and fireproof structure, with aerogel felt as the main fireproof layer, and from the surface of the cable steel wire from the inside to the outside, it includes a cable steel wire bundle, a winding wire layer, a sealing protective layer, an aerogel felt layer, a wrapping layer, and a surface protective layer. Although the problem of insufficient stability of its fireproof structure under fire has been solved. However, after the inventor prepared samples for testing, the bridge ropes of the aerogel provided by the above patent were burned for 120 minutes (about 805°C on the sample surface), and the temperature inside the sample exceeded 300°C. When the heating temperature of the bridge cable is lower than 300°C, its tensile strength will not be significantly affected by the temperature. After the bridge cable is heated to 550°C, the strength and hardness of the bridge cable will be greatly reduced by 40%. Once the bridge cable fails, it will cause very serious safety accidents and economic losses.

[0004] Therefore, it is necessary to develop an aerogel fireproof layer. When a fire occurs, the aerogel fireproof layer can control the temperature of the cable steel wire to below 170°C within 2 hours, leaving precious time for firefighting and protecting the safety of the bridge. Summary of the invention

[0005] In view of this, the present invention proposes an aerogel fire retardant coating and a preparation method thereof to solve the above problems.

[0006] The technical solution of the present invention is achieved in this way: An aerogel fire retardant coating comprises the following raw materials in parts by weight: 5-10 parts of modified aerogel, 5-10 parts of hollow porous micron-sized silicon spheres, 2-4 parts of carbon fibers, 50-55 parts of epoxy resin, 0.5-0.8 parts of defoaming agent, and 5-8 parts of epoxy curing agent; The preparation method of the modified aerogel comprises: first diluting water glass with water, adding dilute sulfuric acid to the dilution solution to adjust the pH to 2-3, stirring evenly, adding tin chloride, ultrasonic stirring, then adding ammonia water until gel is generated, washing the gel, freeze drying, calcining under a mixed atmosphere, and cooling with the furnace to obtain the modified aerogel; The preparation method of the aerogel fire retardant coating comprises the following specific steps: grinding and mixing hollow porous micron-sized silicon balls and carbon fibers, then ultrasonically mixing with modified aerogel, adding into epoxy resin, performing microwave heating and stirring, adding epoxy curing agent and defoaming agent and continuing stirring to obtain the aerogel fire retardant coating.

[0007] Furthermore, the following raw materials are included in parts by weight: 8 parts of modified aerogel, 8 parts of hollow porous micron-sized silicon spheres, 3 parts of carbon fibers, 53 parts of epoxy resin, 0.6 parts of defoaming agent, and 7 parts of epoxy curing agent.

[0008] Further, the mass ratio of water glass to water is 1:5-10; the concentration of dilute sulfuric acid is 0.3-0.5 mol / L; the mass ratio of tin chloride to water glass is 0.05-0.2:1; the ultrasonic stirring is stirred at 200-300 rpm and 40-50° C. for 1-2 h; the concentration of ammonia water is 5-7 wt %; the mixed atmosphere is Ar and NH 2 in a volume ratio of 1-3:1 3 ; The calcination time is 2-4h and the temperature is 450-550℃.

[0009] Furthermore, the preparation method of the hollow porous micron-sized silicon spheres is as follows: aluminum powder and hollow glass microspheres are ground and mixed evenly, calcined in an Ar atmosphere, cooled with the furnace, the calcined mixture is added to acetic acid, stirred evenly, filtered and washed, to obtain hollow porous micron-sized silicon spheres.

[0010] Furthermore, the mass ratio of the aluminum powder to the hollow glass microspheres is 1:6-8; the calcination is performed at 600-800°C for 1-3h; the solid-liquid ratio of the calcined mixture to acetic acid is 1:3-5g / mL; and the concentration of the acetic acid is 0.15-0.2mol / L.

[0011] Furthermore, the epoxy curing agent is any one of triethylenetetramine, diethylenetetramine or tetraethylenetetramine; the defoaming agent is any one of polydimethylsiloxane, GP type defoaming agent and GPE type defoaming agent.

[0012] Furthermore, the ultrasonic mixing is carried out at 100-200 rpm and 20-30° C. for 30-60 min.

[0013] Furthermore, the microwave heating and stirring has a power of 350-450W, a temperature of 60-80°C, and a time of 1-2h.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. The aerogel fire retardant coating of the present invention has the characteristics of high specific surface area, high porosity, low density and low thermal conductivity. It is resistant to impact, vibration and mechanical damage, has long-term durability, and provides fire and corrosion protection. The aerogel fireproof layer hardly increases the load on the cable, does not change the shape of the cable, and does not affect the aerodynamic shape of the cable. The aerogel fireproof layer is very dense, has very good cable wrapping properties, isolates the invasion of corrosive factors, and provides corrosion protection for the cable steel wire. The bonding force is greater than 5MPa. The aerogel fireproof layer has no cracking or falling off after tens of millions of vibration fatigue tests, and the bonding force and fireproof performance are not attenuated. The combustion test under tension state does not affect the fireproof performance.

[0015] 2. The aerogel fire retardant coating of the present invention adds modified aerogel, hollow porous micron-sized silicon spheres and carbon fibers to epoxy resin, synergistically enhancing the effect, increasing the foaming ratio, and reducing the thermal conductivity coefficient, thereby improving the fire retardant performance of the coating. Active metals are used to reduce hollow glass microspheres, and the metal silicon oxide of the hollow glass microspheres after reduction is removed by acid to obtain hollow porous micron-sized silicon spheres with a large number of holes and pores. Inserting carbon fibers into the pores of the hollow porous micron-sized silicon spheres can improve thermal insulation, reduce thermal conductivity, and improve the mechanical properties (strength, toughness and crack resistance) of the coating; the modified aerogel is Sn and N doped into the aerogel, which not only improves the fire retardant performance and thermal stability, but also improves the mechanical strength.

[0016] 3. The method for preparing aerogel fire retardant coating of the present invention uses ultrasound and microwave to evenly disperse the raw materials of the coating, prevent agglomeration, and improve the production efficiency of the coating. DETAILED DESCRIPTION

[0017] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0018] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0019] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0020] The defoaming agent used in the following examples and comparative examples is polydimethylsiloxane, and the epoxy curing agent is triethylenetetramine, but they are not limited to this one.

[0021] Example 1 An aerogel fireproof coating comprises the following raw materials in parts by weight: 8 parts of modified aerogel, 8 parts of hollow porous micron-sized silicon balls, 3 parts of carbon fibers, 53 parts of epoxy resin, 0.6 parts of defoaming agent, and 7 parts of epoxy curing agent.

[0022] The preparation method of the aerogel fire retardant coating comprises the following specific steps: (1) Aluminum powder and hollow glass microspheres were ground and mixed evenly in a mass ratio of 1:7, calcined at 700°C for 2 h in an Ar atmosphere, cooled in the furnace, and the calcined mixture was added to 0.18 mol / L acetic acid at a solid-liquid ratio of 1:4 g / mL, stirred evenly, filtered and washed to obtain hollow porous micron-sized silicon spheres; (2) First, dilute the water glass with water (the mass ratio of water glass to water is 1:8), add 0.4 mol / L dilute sulfuric acid to the dilution to adjust the pH to 2.5±0.1, stir evenly, add tin chloride (the mass ratio of tin chloride to water glass is 0.01:1), stir ultrasonically (250 rpm, 45°C) for 1.5 h, then add 6 wt% ammonia water until gel is produced, rinse the gel, freeze-dry, and precipitate in an Ar and NH 3 The mixture was calcined at 500°C for 3 h in a mixed atmosphere and then cooled in the furnace to obtain a modified aerogel. (3) The hollow porous micron-sized silicon spheres and carbon fibers were ground and mixed, and then ultrasonically mixed with the modified aerogel (150 rpm, 25°C) for 45 min, added to the epoxy resin, and heated and stirred by microwave (400 W, 70°C) for 1.5 h. The epoxy curing agent and defoaming agent were added and continued to be stirred to obtain the aerogel fire retardant coating.

[0023] Example 2 An aerogel fireproof coating comprises the following raw materials in parts by weight: 5 parts of modified aerogel, 5 parts of hollow porous micron-sized silicon balls, 2 parts of carbon fibers, 50 parts of epoxy resin, 0.5 parts of defoaming agent, and 5 parts of epoxy curing agent.

[0024] The preparation method of the aerogel fire retardant coating comprises the following specific steps: (1) Aluminum powder and hollow glass microspheres were ground and mixed evenly in a mass ratio of 1:6, calcined at 600°C for 1 h in an Ar atmosphere, cooled in the furnace, and the calcined mixture was added to 0.15 mol / L acetic acid at a solid-liquid ratio of 1:3 g / mL, stirred evenly, filtered and washed to obtain hollow porous micron-sized silicon spheres; (2) First, dilute the water glass with water (the mass ratio of water glass to water is 1:5), add 0.3 mol / L dilute sulfuric acid to the dilution to adjust the pH to 2.1±0.1, stir evenly, add tin chloride (the mass ratio of tin chloride to water glass is 0.05:1), stir ultrasonically (250 rpm, 45°C) for 1.5 h, then add 5 wt% ammonia water until gel is produced, rinse the gel, freeze-dry, and precipitate in an Ar and NH 3 The aerogel was calcined at 450°C for 2 h in a mixed atmosphere and then cooled in the furnace to obtain a modified aerogel. (3) The hollow porous micron-sized silicon spheres and carbon fibers were ground and mixed, and then ultrasonically mixed with the modified aerogel (100 rpm, 20°C) for 30 min, added to the epoxy resin, and heated and stirred by microwave (350 W, 60°C) for 1 h. The epoxy curing agent and defoaming agent were added and continued to be stirred to obtain the aerogel fire retardant coating.

[0025] Example 3 An aerogel fireproof coating comprises the following raw materials in parts by weight: 10 parts of modified aerogel, 10 parts of hollow porous micron-sized silicon balls, 4 parts of carbon fibers, 55 parts of epoxy resin, 0.8 parts of defoaming agent, and 8 parts of epoxy curing agent.

[0026] The preparation method of the aerogel fire retardant coating comprises the following specific steps: (1) Aluminum powder and hollow glass microspheres were ground and mixed evenly in a mass ratio of 1:8, calcined under an Ar atmosphere (800°C) for 3 h, cooled in the furnace, and the calcined mixture was added to 0.2 mol / L acetic acid at a solid-liquid ratio of 1:5 g / mL, stirred evenly, filtered and washed to obtain hollow porous micron-sized silicon spheres; (2) First, dilute the water glass with water (the mass ratio of water glass to water is 1:10), add 0.5 mol / L dilute sulfuric acid to the dilution to adjust the pH to 2.9±0.1, stir evenly, add tin chloride (the mass ratio of tin chloride to water glass is 0.2:1), stir ultrasonically (250 rpm, 45°C) for 1.5 h, then add 7 wt% ammonia water until gel is produced, rinse the gel, freeze-dry, and in an Ar and NH 2 O solution with a volume ratio of 3:1 3 calcined at 550°C for 4 h in a mixed atmosphere and cooled in the furnace to obtain a modified aerogel; (3) The hollow porous micron-sized silicon spheres and carbon fibers were ground and mixed, and then ultrasonically mixed with the modified aerogel (200 rpm, 30°C) for 60 min, added to the epoxy resin, and heated and stirred by microwave (450 W, 80°C) for 2 h. The epoxy curing agent and defoaming agent were added and continued to be stirred to obtain the aerogel fire retardant coating.

[0027] Comparative Example 1 The difference from Example 1 is that the amount of raw materials is different, and the rest is consistent with Example 1.

[0028] The aerogel fire retardant coating of this comparative example comprises the following raw materials in parts by weight: 3 parts of modified aerogel, 4 parts of hollow porous micron-sized silicon spheres, 1 part of carbon fiber, 45 parts of epoxy resin, 0.4 parts of defoaming agent, and 4 parts of epoxy curing agent.

[0029] Comparative Example 2 The difference from Example 1 is that SiO 2 The aerogel replaces the modified aerogel, that is, Sn is not doped, and the rest is consistent with Example 1.

[0030] The aerogel fire retardant coating of this comparative example comprises the following raw materials in parts by weight: 8 parts SiO 2 Aerogel, 8 parts of hollow porous micron-sized silicon spheres, 3 parts of carbon fibers, 53 parts of epoxy resin, 0.6 parts of defoaming agent, and 7 parts of epoxy curing agent.

[0031] The step (3) of the preparation process of the fire retardant coating of this comparative example is as follows: grinding and mixing the hollow porous micron-sized silicon spheres and carbon fibers, and then mixing with SiO 2 The aerogel was mixed by ultrasound (150 rpm, 25°C) for 45 min, added to epoxy resin, heated and stirred by microwave (400 W, 70°C) for 1.5 h, and epoxy curing agent and defoaming agent were added and continued to stir to obtain an aerogel fire retardant coating.

[0032] Comparative Example 3 The difference from Example 1 is that hollow glass microspheres are used instead of hollow porous micron-sized silicon spheres, and the rest is the same as Example 1.

[0033] The aerogel fire retardant coating of this comparative example comprises the following raw materials in parts by weight: 8 parts of modified aerogel, 8 parts of hollow glass microspheres, 3 parts of carbon fibers, 53 parts of epoxy resin, 0.6 parts of defoaming agent, and 7 parts of epoxy curing agent.

[0034] The preparation process of the fire retardant coating of this comparative example is specifically as follows: (1) First, dilute water glass with water (the mass ratio of water glass to water is 1:8), add 0.4 mol / L dilute sulfuric acid to the dilution to adjust the pH to 2.5±0.1, stir evenly, add tin chloride (the mass ratio of tin chloride to water glass is 0.01:1), stir ultrasonically (250 rpm, 45°C) for 1.5 h, then add 6 wt% ammonia water until gel is produced, rinse the gel, freeze-dry, and precipitate in an Ar and NH 3 The mixture was calcined at 500°C for 3 h in a mixed atmosphere and then cooled in the furnace to obtain a modified aerogel. (2) The hollow glass microspheres and carbon fibers were ground and mixed, and then ultrasonically mixed with the modified aerogel (150 rpm, 25°C) for 45 min, added to the epoxy resin, and heated and stirred by microwave (400 W, 70°C) for 1.5 h. The epoxy curing agent and defoaming agent were added and continued to be stirred to obtain the aerogel fire retardant coating.

[0035] Comparative Example 4 The difference from Example 1 is that carbon fiber is missing, and the missing raw material is allocated to other raw materials in proportion. The rest is the same as Example 1.

[0036] The step (3) of the preparation process of the fire retardant coating of this comparative example is as follows: the hollow porous micron-sized silicon spheres and the modified aerogel are ultrasonically mixed (150 rpm, 25°C) for 45 minutes, added into the epoxy resin, heated and stirred by microwave (400 W, 70°C) for 1.5 hours, and the epoxy curing agent and the defoaming agent are added and stirred continuously to obtain the aerogel fire retardant coating.

[0037] Comparative Example 5 The difference from Example 1 is that ultrasound and microwave treatment are not used in step (3), and the rest is consistent with Example 1.

[0038] The preparation method of the aerogel fire retardant coating of this comparative example comprises the following specific steps: (1) Aluminum powder and hollow glass microspheres were ground and mixed evenly in a mass ratio of 1:7, calcined at 700°C for 2 h in an Ar atmosphere, cooled in the furnace, and the calcined mixture was added to 0.18 mol / L acetic acid at a solid-liquid ratio of 1:4 g / mL, stirred evenly, filtered and washed to obtain hollow porous micron-sized silicon spheres; (2) First, dilute the water glass with water (the mass ratio of water glass to water is 1:8), add 0.4 mol / L dilute sulfuric acid to the dilution to adjust the pH to 2.5±0.1, stir evenly, add tin chloride (the mass ratio of tin chloride to water glass is 0.01:1), stir ultrasonically (250 rpm, 45°C) for 1.5 h, then add 6 wt% ammonia water until gel is produced, rinse the gel, freeze-dry, and precipitate in an Ar and NH 3 The mixture was calcined at 500°C for 3 h in a mixed atmosphere and then cooled in the furnace to obtain a modified aerogel. (3) Grind and mix the hollow porous micron-sized silicon spheres and carbon fibers, stir them with the modified aerogel at 25°C for 45 minutes, add them to the epoxy resin, stir them at 70°C for 1.5 hours, add the epoxy curing agent and defoaming agent and continue stirring to obtain the aerogel fire retardant coating.

[0039] Test Case An aerogel fireproof layer is applied to the outside of the cable wire bundle. Before applying the aerogel fireproof coating, the surface of the substrate should be clean, dry, flat, firm, free of grease, rust and other debris. It can be applied by two-component heating pump spraying, airless spraying or troweling. It can be cured at a temperature greater than 5°C and the construction temperature is 40°C. The surface temperature must always be kept at least 3°C ​​above the dew point and the maximum relative humidity is below 85%.

[0040] The cable samples coated with the aerogel fire retardant coatings of Examples 1-3 and Comparative Examples 1-5 were subjected to fire resistance tests. The test method was based on GB 14907-2018. The test conditions were as follows: the middle of the sample was burned, and the surface and internal temperatures of the sample were tested by a temperature detector. The combustion type was butane gas. The test results are shown in Table 1. Table 1

[0041] As can be seen from Table 1, the fire retardant coatings prepared in Examples 1-3 of the present invention have excellent fire retardant properties and can control the cable steel wire temperature below 150° C. within 2 hours. The fire retardant properties of the coatings in Comparative Examples 1-5 are reduced, and the time for the internal temperature to reach 300° C. is shorter than that in Examples 1-3.

[0042] Table 2 shows the expansion ratio and thermal conductivity of the aerogel fire retardant coatings of Examples 1-3 and Comparative Examples 1-5 when burned for 60 minutes. The higher the expansion ratio of the coating, the thicker the foaming layer, and the better the fireproof and heat-insulating effect. Table 2

[0043] It can be seen from the foaming ratio and thermal conductivity in Table 2 that they correspond to the fire resistance in Table 1. This confirms that the higher the foaming ratio of the coating, the thicker the foaming layer, the lower the thermal conductivity, and the better the fireproof and heat-insulating effect.

[0044] The aerogel fire retardant coatings of Examples 1-3 and Comparative Examples 1-5 were tested for other performance indicators, and the technical indicators and test results are shown in Tables 3-4. Table 3

[0045] Table 4

[0046] It can be seen from Table 4 that the fire retardant coatings prepared in Examples 1-3 of the present invention have excellent performance indicators. Most importantly, after the above tests, the thermal insulation efficiency of the aerogel fire retardant coatings of Examples 1-3 is not attenuated.

[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An aerogel fire retardant coating, characterized in that: According to the weight parts, including the following raw materials: 5-10 parts of modified aerogel, 5-10 parts of hollow porous micron-sized silicon spheres, 2-4 parts of carbon fiber, 50-55 parts of epoxy resin, 0.5-0.8 parts of defoaming agent, 5-8 parts of epoxy curing agent; The preparation method of the modified aerogel comprises: first diluting water glass with water, adding dilute sulfuric acid to the dilution solution to adjust the pH to 2-3, stirring evenly, adding tin chloride, ultrasonic stirring, then adding ammonia water until gel is generated, washing the gel, freeze drying, calcining under a mixed atmosphere, and cooling with the furnace to obtain the modified aerogel; The preparation method of the aerogel fire retardant coating comprises the following specific steps: grinding and mixing hollow porous micron-sized silicon balls and carbon fibers, then ultrasonically mixing with modified aerogel, adding into epoxy resin, performing microwave heating and stirring, adding epoxy curing agent and defoaming agent and continuing stirring to obtain the aerogel fire retardant coating.

2. An aerogel fire retardant coating according to claim 1, characterized in that: The following raw materials are included in parts by weight: 8 parts of modified aerogel, 8 parts of hollow porous micron-sized silicon spheres, 3 parts of carbon fibers, 53 parts of epoxy resin, 0.6 parts of defoaming agent, and 7 parts of epoxy curing agent.

3. An aerogel fire retardant coating according to claim 1, characterized in that: The mass ratio of water glass to water is 1:5-10; the concentration of dilute sulfuric acid is 0.3-0.5 mol / L; the mass ratio of tin chloride to water glass is 0.05-0.2:1; the ultrasonic stirring is stirred at 200-300 rpm and 40-50°C for 1-2h; the concentration of ammonia water is 5-7wt%; the mixed atmosphere is Ar and NH3 in a volume ratio of 1-3:1; the calcination time is 2-4h and the temperature is 450-550°C.

4. An aerogel fire retardant coating according to claim 1, characterized in that: The preparation method of the hollow porous micron-sized silicon spheres comprises the following steps: grinding and mixing aluminum powder and hollow glass microspheres uniformly, calcining in an Ar atmosphere, cooling with the furnace, adding the calcined mixture into acetic acid, stirring uniformly, filtering and washing, and obtaining hollow porous micron-sized silicon spheres.

5. An aerogel fire retardant coating as claimed in claim 4, characterized in that: The mass ratio of the aluminum powder to the hollow glass microspheres is 1:6-8; the calcination is carried out at 600-800° C. for 1-3 hours; the solid-liquid ratio of the calcined mixture to acetic acid is 1:3-5 g / mL; and the concentration of the acetic acid is 0.15-0.2 mol / L.

6. An aerogel fire retardant coating according to claim 1, characterized in that: The epoxy curing agent is any one of triethylenetetramine, diethylenetetramine or tetraethylenetetramine; the defoaming agent is any one of polydimethylsiloxane, GP type defoaming agent and GPE type defoaming agent.

7. An aerogel fire retardant coating according to claim 1, characterized in that: The ultrasonic mixing is carried out at 100-200 rpm and 20-30° C. for 30-60 min.

8. The aerogel fire retardant coating according to claim 1, characterized in that: The microwave heating and stirring has a power of 350-450 W, a temperature of 60-80° C., and a time of 1-2 h.

Citation Information

Cited By

  • Outdoor intumescent fire retardant coating for steel structure and preparation method of outdoor intumescent fire retardant coating