Semiconductor structure and solution pollution evaluation method

By setting up a dielectric ring sleeve structure with ring sleeves on the semiconductor structure and forming a composite layer for solution pre-impregnation, the problem of evaluating the impact of small-sized particles on the semiconductor process is solved, and the sensitivity evaluation of particles smaller than filter size is achieved. Improves analysis efficiency and accuracy.

CN118899237APending Publication Date: 2024-11-05CSMC TECH FAB2 CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310495195.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art lacks effective methods to evaluate the impact of small-sized particles on semiconductor preparation processes, resulting in the inability to accurately evaluate the impact of particles smaller than the filtered size in deionized water on semiconductor devices.

Method used

Provided is a semiconductor structure, including a dielectric ring ring structure with a plurality of ring rings sleeves on the substrate, the width of the dielectric ring gradually increases from the outside to the inside, and a composite layer is formed on the structure for pre-imulating the target solution. To simulate the process, the composite layer is removed to obtain the number of cone defects, thereby establishing the corresponding relationship between particles and defects.

Benefits of technology

Through this method, the process personnel can accurately obtain the sensitivity of the semiconductor preparation process to particles smaller than the filter size in the target solution, and improve the analysis efficiency and evaluation accuracy of solution contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899237A_ABST
    Figure CN118899237A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor structure and a solution pollution evaluation method. The semiconductor structure comprises a substrate; the at least one lantern ring structure is arranged on the substrate; the lantern ring structure comprises a plurality of medium rings, and the medium rings are sequentially sleeved in a ring-to-ring mode and are arranged at intervals. In the lantern ring structure, the widths of the dielectric rings are gradually increased in the direction from the outermost side of the lantern ring structure to the center of the lantern ring structure, and the width of the dielectric ring on the outermost side is not smaller than the design size of a target device. In this way, the number of defects generated by the particles smaller than the filtering size in the target solution in the semiconductor preparation process can be obtained on the semiconductor structure through a test, and therefore technologists can conveniently obtain the sensitivity of the semiconductor preparation process to the particles smaller than the filtering size in the target solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for evaluating semiconductor structure and solution contamination. Background Art

[0002] The semiconductor integrated circuit industry has experienced exponential growth. As the complexity of semiconductor processes increases, the requirements for process particles are getting higher and higher. Deionized water (DI Water) is widely used in semiconductor processes. The removal of impurities in deionized water generally includes the removal of total organic carbon (TOC) and particles. However, small particles below the filter size range will form agglomerated particles under the action of solvents, and the agglomerated particles are prone to cause device failure. At present, there is no effective evaluation method or structure to evaluate the impact of small particles that cannot be filtered and removed on the semiconductor manufacturing process. Therefore, how to evaluate the impact of small particles on the semiconductor manufacturing process has become an urgent problem to be solved in the industry. Summary of the invention

[0003] Based on this, it is necessary to provide an evaluation method for semiconductor structure and solution contamination to address the above problems.

[0004] In a first aspect, the present application provides a semiconductor structure for evaluating solution contamination. The semiconductor structure comprises:

[0005] substrate;

[0006] At least one ring structure is arranged on the substrate; wherein the ring structure includes a plurality of dielectric rings, each of which is nested in sequence and arranged at intervals from each other; in the ring structure, the width of each of the dielectric rings gradually increases along the direction from the outermost side of the ring structure to the center of the ring structure, and the width of the outermost dielectric ring is not less than the design size of the target device.

[0007] The semiconductor structure provided by the present application is provided with at least one sleeve ring structure on the substrate, the sleeve ring structure includes a plurality of dielectric rings which are nested one inside the other, and the width of each dielectric ring gradually increases from the outside to the inside, and the width of the outermost dielectric ring is not less than the design size of the target device. In this way, the number of defects caused by particles smaller than the filter size in the target solution in the semiconductor manufacturing process can be obtained through experiments on the semiconductor structure, thereby facilitating process personnel to obtain the sensitivity of the semiconductor manufacturing process to particles smaller than the filter size in the target solution.

[0008] In one of the embodiments, the dielectric rings in the sleeve ring structure are sleeved one after another along the same center.

[0009] In one embodiment, the semiconductor structure includes a plurality of collar structures, and the plurality of collar structures are disposed on the substrate at intervals.

[0010] In one embodiment, the width of the outermost dielectric ring of each ring structure gradually increases at a first preset increment.

[0011] In one embodiment, the ratio of the first preset increment to the design size is between 0.05 and 0.3.

[0012] In one embodiment, the width of the outermost dielectric ring of the collar structure is not greater than 20 times the design size.

[0013] In one embodiment, the dielectric ring is in the shape of a rectangular ring;

[0014] And / or, the material of the dielectric ring includes silicon dioxide.

[0015] In one embodiment, in the collar structure, the distances between any two adjacent dielectric rings are not equal;

[0016] Or, in the sleeve ring structure, the distance between any two adjacent dielectric rings is equal to the designed size.

[0017] In a second aspect, the present application provides a method for evaluating solution contamination, the method comprising:

[0018] Providing a semiconductor structure as described in any embodiment of the first aspect;

[0019] forming a composite layer on the semiconductor structure, and pre-wetting the composite layer with a target solution;

[0020] removing the composite layer;

[0021] The number of cone defects on the semiconductor structure is obtained to obtain a corresponding relationship between particles of a target size in the target solution and the number of cone defects.

[0022] In one embodiment, the step of forming a composite layer on the semiconductor structure and pre-wetting the composite layer with a target solution comprises:

[0023] forming a first material layer on the semiconductor structure;

[0024] A second material layer is formed on the first material layer, and the second material layer is pre-wetted with a target solution.

[0025] In one embodiment, the thickness of the second material layer is not greater than 150 nm;

[0026] And / or, the first material layer is made of polysilicon.

[0027] In one embodiment, the step of providing the semiconductor structure as described in any embodiment of the first aspect includes:

[0028] forming an oxide layer on the substrate;

[0029] A dielectric layer is formed on the oxide layer.

[0030] In one embodiment, in the oxide layer, the number of particles having a particle size not less than 0.2 μm is less than 20, and the number of particles having a particle size greater than or equal to 1 μm is less than 10;

[0031] and / or, in the dielectric layer, the number of particles having a particle size not less than 0.2 μm is less than 20; in the oxide layer, the number of particles having a particle size greater than or equal to 1 μm is less than 10;

[0032] And / or, in the collar structure, the number of particles having a particle size not less than 0.2 μm is less than 20, and the number of particles having a particle size greater than or equal to 1 μm is less than 10.

[0033] The solution contamination evaluation method provided in the present application adopts a semiconductor structure with a collar structure. Specifically, a composite layer is formed on the semiconductor structure, and the composite layer is pre-wetted with a target solution, and finally the composite layer is removed. In this way, cone defects caused by target-sized particles in the target solution can be formed on the semiconductor structure, so that the corresponding relationship between the target-sized particles and the number of cone defects can be obtained, which makes it easier for process personnel to obtain the sensitivity of the semiconductor manufacturing process to particles smaller than the filter size in the target solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments or exemplary embodiments of the present application, the drawings required for use in the description of the embodiments or exemplary embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 A schematic diagram of the cross-sectional structure of a semiconductor structure provided in one embodiment of the present application.

[0036] Figure 2 for Figure 1 A top view of a collar structure in the semiconductor structure is shown.

[0037] Figure 3 for Figure 1Schematic diagram of comparison of multiple ring structures in the semiconductor structure shown.

[0038] Figure 4 A schematic flow chart of a method for evaluating solution contamination provided in one embodiment of the present application.

[0039] Figure 5 for Figure 4 A schematic diagram of a flow chart of S200 in the method shown.

[0040] Figure 6 for Figure 4 A schematic flow chart of S100 in the method shown.

[0041] Figure 7-Figure 16 for Figure 4 A schematic diagram of the cross-sectional structure of a semiconductor structure during the process of the method shown.

[0042] Fig.17 A relationship diagram between the number of cone defects and the UF filter process time provided in an embodiment of the present application.

[0043] Fig.18 A relationship diagram between the number of cone defects and the width of the dielectric ring provided in an embodiment of the present application.

[0044] Reference numerals:

[0045] 10. Semiconductor structure; 11. Substrate; 12. Ring structure; 121. Dielectric ring; 13. Oxide layer; 14. Dielectric layer; 15. Second photoresist layer; 20. Composite layer; 21. First material layer; 22. Second material layer; 31. First photoresist layer; 32. Agglomerated particles; 33. Particle defects; 34. Cone defects. DETAILED DESCRIPTION

[0046] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0048] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present application, the first element, component, region, layer, doping type or part discussed below can be represented as a second element, component, region, layer or part.

[0049] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.

[0050] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts, or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.

[0051] Embodiments of the application are described herein with reference to cross-sectional views that are schematic diagrams of ideal embodiments (and intermediate structures) of the application, so that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances can be expected. Therefore, embodiments of the application should not be limited to the specific shapes of the zones shown herein, but rather include shape deviations due to, for example, manufacturing techniques. For example, an implanted region shown as a rectangle typically has rounded or curved features and / or an implant concentration gradient at its edges, rather than a binary change from an implanted region to a non-implanted region. Similarly, a buried region formed by implantation may result in some implantation in the region between the buried region and the surface through which the implantation is performed. Therefore, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shape of the region of the device, and do not limit the scope of the application.

[0052] In the first aspect, an embodiment of the present application provides a semiconductor structure for evaluating solution contamination. Here, evaluating solution contamination can be understood as: evaluating the impact of particles smaller than the filter size in the target solution on the semiconductor manufacturing process. It can also be understood as: obtaining the sensitivity of the semiconductor device (or semiconductor device manufacturing process) to particles smaller than the filter size in the target solution. The target solution here can be pure water or impure water, wherein the impure water can be acid in an acid tank or a CMP solution in a CMP machine. The semiconductor devices here can be discrete devices, power devices, MEMS (Micro ElectroMechanical System) devices, IC (Integrated Circuit) devices, and the like.

[0053] Reference Figure 1-Figure 3 As shown, specifically, the semiconductor structure 10 includes a substrate 11 and at least one ring structure 12. The ring structure 12 is arranged on the substrate 11. The ring structure 12 includes a plurality of dielectric rings 121, and each dielectric ring 121 is nested in sequence and arranged at intervals from each other. In the ring structure 12, the width of each dielectric ring 121 gradually increases from the outermost side of the ring structure 12 to the center of the ring structure 12, and the width of the outermost dielectric ring 121 is not less than the design size of the target device. Please refer to Figure 2 , Figure 2 W shown in refractory 3 represents the width of the outermost dielectric ring 121 .

[0054] The semiconductor structure 10 provided in the embodiment of the present application is provided with a sleeve ring structure 12 on a substrate 11, wherein the sleeve ring structure 12 includes a plurality of dielectric rings 121 which are nested one inside the other, and the width of each dielectric ring 121 gradually increases from the outside to the inside, and the width of the outermost dielectric ring 121 is not less than the design size of the target device. In this way, the number of defects generated by particles smaller than the filter size in the target solution in the semiconductor manufacturing process can be obtained through experiments on the semiconductor structure 10, thereby facilitating process personnel to obtain the sensitivity of the semiconductor manufacturing process to particles smaller than the filter size in the target solution.

[0055] In one embodiment, the dielectric rings 121 in the collar structure 12 are nested one after another along the same center. In this way, the collar structure 12 is equivalent to a concentric ring structure. In this way, when manufacturing the collar structure 12, it is easy to control the graphic morphology of the collar structure 12, and it is easier to observe the repeatability and reproducibility of defects.

[0056] Here, "the dielectric rings 121 are nested in sequence along the same center" means that in the same ring structure 12, the dielectric rings 121 are all arranged around the same center, and the dielectric rings 121 are arranged in a radial shape, that is, in two adjacent dielectric rings 121, the outer dielectric ring 121 is nested on the outer side of the inner dielectric ring 121. The target device here can be a discrete device, a power device, a MEMS device, an IC device, etc. The target size can be the minimum design size of the target device, and the minimum design size can be the minimum design line width for example.

[0057] It can be understood that in the embodiment of the present application, the ring structure 12 can also be a non-concentric structure, that is, the centers of at least a part of the dielectric rings 121 do not overlap.

[0058] In one embodiment, referring to Figure 3 As shown, the semiconductor structure 10 includes a plurality of collar structures 12, which are disposed at intervals on the substrate 11. In this way, when the process personnel use the semiconductor structure 10 to evaluate the solution contamination, it is convenient for the process personnel to compare the results presented on different collar structures 12, thereby improving the analysis efficiency or evaluation efficiency of the solution contamination.

[0059] It should be noted that the number of the ring structures 12 in the semiconductor structure 10 may be 3, 6, 8 or more, and the embodiment of the present application does not limit the number of the ring structures 12.

[0060] In one embodiment, the widths of the outermost dielectric rings 121 of each ring structure 12 are not equal, so as to facilitate obtaining the sensitivity of dielectric rings 121 of various sizes to particles smaller than the filtering size.

[0061] In one embodiment, the width of the outermost dielectric ring 121 of each ring structure 12 gradually increases. In one example, assuming that the number of ring structures 12 is 4, and the width of the outermost dielectric ring 121 of one ring structure 12 is 90 nm, the widths of the outermost dielectric rings 121 of the other three ring structures 12 may be 100 nm, 130 nm, and 150 nm.

[0062] In one embodiment, the width of the outermost dielectric ring 121 of each ring structure 12 gradually increases at a first preset increment, which is equivalent to the width of the outermost dielectric ring 121 of each ring structure 12 increasing at a fixed "step length".

[0063] It is understandable that when the process personnel obtain the sensitivity of the semiconductor manufacturing process (or semiconductor device) to particles smaller than the filter size in the target solution, it is impossible to evaluate each design size due to process and time constraints. In the embodiment of the present application, since the width of the outermost dielectric ring 121 of each ring structure 12 is uniformly increased, after the process personnel obtain the sensitivity under certain widths, they can more accurately predict the sensitivity within these width ranges based on these data, thereby improving the analysis efficiency.

[0064] In one embodiment, the ratio of the first preset increment to the design size is between 0.05 and 0.3. Exemplarily, the ratio of the first preset increment to the design size can be 0.05, 0.1, 0.15, 0.2, 0.25, 0.28 or 0.3. By making the ratio of the first preset increment to the design size within the above range, the analysis efficiency can be improved while minimizing the analysis error.

[0065] In one embodiment, the width of the outermost dielectric ring 121 of the collar structure 12 is not greater than 20 times the design size. Exemplarily, the multiple may be 20 times, 18 times, 15 times or 10 times.

[0066] Furthermore, when there are multiple ring structures 12, the width of the largest medium ring 121 among all the medium rings 121 of the multiple ring structures 12 is not greater than 20 times the design size. In this way, the number of ring structures 12 can be reduced to the maximum while meeting actual needs and ensuring analysis errors.

[0067] In an example, assuming that the design size is 100 nm, then, among all the dielectric rings 121 of the ring structure 12 , the width of the dielectric ring 121 with the largest width may be 2000 nm, 1900 nm, 1750 nm, 1500 nm or 1000 nm.

[0068] In one embodiment, in each ring structure 12, the width of each dielectric ring 121 increases by a second preset increment along the direction from the outermost side of the ring structure 12 to the center of the ring structure 12. In this way, the width of each dielectric ring 121 increases uniformly. The embodiment of the present application does not limit the value range of the second preset increment.

[0069] In another embodiment, in each ring structure 12, the width of each dielectric ring 121 increases non-uniformly along the direction from the outermost side of the ring structure 12 to the center of the ring structure 12. Exemplarily, the ring structure 12 includes three dielectric rings 121, the width of the outermost dielectric ring 121 is 100 nm, the width of the middle dielectric ring 121 is 150 nm, and the width of the innermost dielectric ring 121 is 180 nm.

[0070] In one embodiment, the dielectric ring 121 is in a rectangular ring shape. By setting the dielectric ring 121 in a rectangular ring shape, the difficulty of preparing the ring structure 12 can be reduced.

[0071] In another embodiment, the shape of the dielectric ring 121 may also be a circular ring, a regular pentagonal ring, a regular hexagonal ring, or a regular octagonal ring.

[0072] In one embodiment, the material of the dielectric ring 121 includes silicon dioxide.

[0073] In one embodiment, the thickness of the dielectric ring 121 is not greater than 2000 nm. For example, the thickness of the dielectric ring 121 may be 300 nm, 500 nm, 1000 nm, 1500 nm, etc.

[0074] In one embodiment, in the ring structure 12, the distances between any two adjacent dielectric rings 121 are not equal. In this way, different process windows can be obtained, making it easier to replicate the immersion characteristics of the target solution after flowing. Figure 1 As shown, L in the figure represents the distance between two adjacent dielectric rings 121.

[0075] In one embodiment, in the ring structure 12 , the distance between any two adjacent dielectric rings 121 is equal.

[0076] In one embodiment, referring to Figure 1 As shown, in the ring structure 12, the distance L between any two adjacent dielectric rings 121 is equal to the designed size.

[0077] It can be understood that the ring structure 12 of the semiconductor structure 10 provided in the embodiment of the present application includes at least the following four structures:

[0078] The first one is that the ring structure 12 is a concentric ring structure, and the distance between any two adjacent dielectric rings 121 in the ring structure 12 is not equal.

[0079] The second type is that the ring structure 12 is a concentric ring structure, and the distance between any two adjacent dielectric rings 121 in the ring structure 12 is equal.

[0080] The third type is that the ring structure 12 is a non-concentric structure, and the distances between any two adjacent dielectric rings 121 in the ring structure 12 are not equal.

[0081] The fourth type: the ring structure 12 is a non-concentric structure, and the distance between any two adjacent dielectric rings 121 in the ring structure 12 is equal.

[0082] Among them, the first structure is convenient for controlling the graphic morphology of the ring structure 12 on the one hand, and it is easier to observe the repeatability and reproducibility of defects on the other hand. On the other hand, different process windows can be obtained, making it easier to replicate the immersion characteristics after the target solution flows.

[0083] It should be noted that, assuming that the process personnel need to obtain the sensitivity of a semiconductor device with a minimum design size of 100 nm to particles smaller than the filtration size in the target solution, then in the actual operation process, the semiconductor structure 10 can specifically be the following two structures.

[0084] First, the largest ring structure 12 and the smallest ring structure 12 are defined. In the semiconductor structure 10, the ring structure 12 with the largest width of the outermost dielectric ring 121 is the largest ring structure 12. In the semiconductor structure 10, the ring structure 12 with the smallest width of the outermost dielectric ring 121 is the smallest ring structure 12.

[0085] The first type: the width of the outermost dielectric ring 121 of the largest ring structure 12 is 150nm, and the width of the outermost dielectric ring 121 of the smallest ring structure 12 is 50nm. The widths of the outermost dielectric rings 121 of the other ring structures 12 are between 50-150nm, and increase in sequence based on 50nm by a third preset increment. The range of the third preset increment can be 10-30nm. The advantage of the first structure is that the sensitivity of the device near the minimum design size can be obtained more accurately.

[0086] The second type: the width of the outermost dielectric ring 121 of the largest ring structure 12 is 2000nm, and the width of the outermost dielectric ring 121 of the smallest ring structure 12 is 100nm. The widths of the outermost dielectric rings 121 of the other ring structures 12 are between 100-2000nm, and increase in sequence based on 100nm with a fourth preset increment. The range of the fourth preset increment can be 5-30nm. The advantage of the second structure is that the sensitivity of the device under various conventional design dimensions can be obtained more comprehensively.

[0087] Second, refer to Figure 4 , and in combination with 7-16, the embodiment of the present application provides a method for evaluating solution contamination, the method for evaluating solution contamination comprising:

[0088] S100: Provide a semiconductor structure 10 as described in any embodiment of the first aspect.

[0089] S200: forming a composite layer 20 on the semiconductor structure 10, and pre-wetting the composite layer 20 with a target solution. In this step, pre-wetting the composite layer 20 with a target solution has at least the following effects: on the one hand, it can simulate the process of using a target solution to treat (e.g., clean) a semiconductor device in a semiconductor manufacturing process, so that target-sized particles of the target solution exist on the composite layer 20, which is convenient for obtaining the number of cone defects 34 on the semiconductor structure 10; on the other hand, it is convenient for subsequent processes to treat the composite layer 20.

[0090] Here, it should be noted that the target size particles refer to particles in the target solution that are smaller than the filtration size.

[0091] S300: removing the composite layer 20. It should be noted that the composite layer 20 can be removed by a dry process or a wet process. In one example, during the process of removing the composite layer 20, a target solution is also used, and target-sized particles of the target solution are also left on the composite layer 20.

[0092] S400: Obtain the number of pyramidal defects 34 on the semiconductor structure 10 to obtain a corresponding relationship between target size particles in the target solution and the number of pyramidal defects 34. Specifically, the number of pyramidal defects 34 on the semiconductor structure 10 can be obtained by a defect scanning machine.

[0093] The solution contamination evaluation method provided in the embodiment of the present application adopts a semiconductor structure 10 having a collar structure 12. Specifically, a composite layer 20 is formed on the semiconductor structure 10, and the composite layer 20 is pre-wetted with a target solution, and finally the composite layer 20 is removed. In this way, a cone defect 34 caused by target-sized particles in the target solution can be formed on the semiconductor structure 10, so that the corresponding relationship between the number of target-sized particles and the cone defect 34 can be obtained, which makes it easier for process personnel to obtain the sensitivity of the semiconductor manufacturing process to particles smaller than the filter size in the target solution.

[0094] In one embodiment, referring to Figure 5 , and combined with Fig.12 and Fig.13 As shown, S200: forming a composite layer 20 on the semiconductor structure 10, and pre-wetting the composite layer 20 with a target solution includes:

[0095] S210: forming a first material layer 21 on the semiconductor structure 10. For example, the first material layer 21 may be formed on the semiconductor structure 10 by chemical vapor deposition, physical vapor deposition or molecular beam epitaxy.

[0096] In one example, after the first material layer 21 is formed, the first material layer 21 may be pre-wetted with a target solution.

[0097] S220: forming a second material layer 22 on the first material layer 21, and pre-wetting the second material layer 22 with a target solution. For example, the second material layer 22 may be formed on the semiconductor structure 10 by chemical vapor deposition, physical vapor deposition, or molecular beam epitaxy. It should be noted that the second material layer 22 may absorb photons to reduce interference effects.

[0098] In one example, the thickness of the second material layer 22 is not greater than 150 nm. Exemplarily, the thickness of the second material layer 22 may be 30 nm, 50 nm, 60 nm, 80 nm, 110 nm, 130 nm, or 150 nm. By making the thickness of the second material layer 22 within the above range, the second material layer 22 can better reduce the interference effect.

[0099] In one example, the second material layer 22 may be an anti-reflection layer.

[0100] In one embodiment, the material of the first material layer 21 includes polysilicon. Exemplarily, the material of the first material layer 21 can be doped polysilicon or undoped polysilicon.

[0101] In one embodiment, referring to Figure 6 , and combined with Figure 7-Figure 11As shown, S100: the step of providing the semiconductor structure 10 as described in any embodiment of the first aspect includes:

[0102] S110: Provide a substrate 11. The material of the substrate 11 can be single crystal silicon, polycrystalline silicon, amorphous silicon, germanium silicon compound, silicon-on-insulator (SOI) or low temperature polysilicon (LTPS), or other materials known to those skilled in the art.

[0103] S120 : forming a barrier layer on the substrate 11 .

[0104] In one embodiment, S120: forming a barrier layer on the substrate 11, specifically includes:

[0105] S121: forming an oxide layer 13 on the substrate 11. For example, the oxide layer 13 may be formed on the substrate 11 by chemical vapor deposition, physical vapor deposition or molecular beam epitaxy.

[0106] S122: forming a dielectric layer 14 on the oxide layer 13. Exemplarily, the dielectric layer 14 can be formed on the substrate 11 by chemical vapor deposition, physical vapor deposition or molecular beam epitaxy. In the embodiment of the present application, the material of the dielectric layer 14 includes silicon nitride. In the embodiment of the present application, the barrier layer includes the oxide layer 13 and the dielectric layer 14.

[0107] After forming the dielectric layer 14, the following steps are then performed:

[0108] S130 : patterning the barrier layer to expose a portion of the substrate 11 .

[0109] S140: forming a collar structure 12 on the exposed surface of the substrate 11. In the embodiment of the present application, the collar structure 12 is made of silicon dioxide. Specifically, the collar structure 12 can be formed by wet oxygen, dry oxygen or high temperature oxidation process.

[0110] In one embodiment, S130: the step of patterning the barrier layer to expose a portion of the substrate 11 specifically includes:

[0111] S131: forming a second photoresist layer 15 on the blocking layer.

[0112] S132: exposing and developing the second photoresist layer 15.

[0113] S133: The barrier layer is processed by dry etching to expose a portion of the substrate 11.

[0114] In one embodiment, in the oxide layer 13 , the number of particles with a particle size not less than 0.2 μm is less than 20, and the number of particles with a particle size greater than or equal to 1 μm is less than 10.

[0115] In one embodiment, in the dielectric layer 14 , the number of particles with a particle size not less than 0.2 μm is less than 20. In the oxide layer 13 , the number of particles with a particle size greater than or equal to 1 μm is less than 10.

[0116] In one embodiment, in the collar structure 12 , the number of particles having a particle size not less than 0.2 μm is less than 20, and the number of particles having a particle size greater than or equal to 1 μm is less than 10.

[0117] Based on the description of the above embodiments, more specific embodiments are proposed below for detailed description.

[0118] Embodiment 1

[0119] Please refer to Figure 3 as well as Figure 7-Figure 16 As shown, a method for evaluating solution contamination includes:

[0120] S1: providing a substrate 11. The material of the substrate 11 is silicon.

[0121] S2: forming an oxide layer 13 on the substrate 11. The oxide layer 13 is grown by dry oxygen method of N2 and O2 to 110+ / -5 angstroms. The particles of the oxide layer 13 meet the following requirements: in the oxide layer 13, the number of particles with a particle size not less than 0.2 μm is less than 20, and the number of particles with a particle size greater than or equal to 1 μm is less than 10.

[0122] S3: forming a dielectric layer 14 on the oxide layer 13. The dielectric layer 14 of 1535+ / -50 angstroms is obtained by a diffusion process for 10 hours. The dielectric layer 14 is made of silicon nitride. The particles of the dielectric layer 14 meet the following requirements: in the dielectric layer 14, the number of particles with a particle size of not less than 0.2 μm is less than 20, and the number of particles with a particle size of greater than or equal to 1 μm is less than 10.

[0123] S4: forming a second photoresist layer 15 on the dielectric layer 14, and exposing and developing the second photoresist layer 15. The second photoresist layer 15 is coated with a thickness of 6000 angstroms by a coating process.

[0124] S5: Patterning the oxide layer 13 and the dielectric layer 14 to expose a portion of the substrate 11. Specifically, a dry etching process is used. The etching process is shown in Table 1.

[0125] Table 1 Dry etching process

[0126]

[0127] S6: Form a collar structure 12 on the exposed surface of the substrate 11. Specifically, silicon dioxide with a thickness of 3000 - 5000 angstroms is grown using a wet process to form the collar structure 12.

[0128] S7: Remove the oxide layer 13 and the dielectric layer 14. Specifically, at a temperature of 165 °C, treat with 85% H3PO4 for 40 minutes.

[0129] After step S7, the semiconductor structure 10 as shown in Fig.11 is obtained. The width of the dielectric ring 121 closer to the center of the collar structure 12 is larger. As shown in the figure, W1 < W2 < W3. Further, in the embodiment of the present application, a semiconductor structure 10 including 27 widths is fabricated, and the widths of the respective dielectric rings 121 are as shown in Figure 3 .

[0130] Further, referring to Figure 12-16 shown, the following steps are then carried out:

[0131] S8: Form a first material layer 21 on the semiconductor structure 10. Specifically, the first material layer 21 is formed on the semiconductor structure 10 using a chemical vapor deposition process, and the material of the first material layer 21 is polysilicon.

[0132] S9: Form a second material layer 22 on the first material layer 21 and pre - wet the second material layer 22 with a target solution. Specifically, the second material layer 22 is formed on the semiconductor structure 10 using chemical vapor deposition. The thickness of the second material layer 22 is 600 angstroms. In the embodiment of the present application, the target solution is pure water.

[0133] S10: Form a first photoresist layer 31 on the second material layer 22.

[0134] S11: Expose and develop the first photoresist layer 31.

[0135] S12: Treat the first material layer 21 and the second material layer 22 using dry etching. Here, Figure 14-16 is a schematic diagram of the first material layer 21 and the second material layer 22 during the dry etching process. As can be seen from Fig.14 , agglomerated particles 32 that are not filtered in pure water remain on the surface of the second material layer 22. In addition, in the figure, D represents the remaining film thickness of the second material layer 22. It can be seen that the smaller the width of the dielectric ring 121, the thinner the remaining film thickness, that is: D1 < D2 < D3. It can be understood that after photolithography and development, the surface is rinsed with the target solution (pure water), and particles are likely to remain on the second material layer 22. These particles are likely to adhere to organic materials such as the second material layer 22 and appear during development.

[0136] It should be noted here that when the target solution is not pure water, after dry etching, "pure water" is required to clean the surface. The "pure water" is pure water that has been evaluated to achieve the target cleanliness to avoid introducing particles during cleaning, which may affect the evaluation (or analysis) results.

[0137] exist Fig.15 In the figure, the particle defect 33 is what is left in the etching of the first material layer 21 after the second material layer 22 is etched. The step of etching the second material layer 22 includes hydrogen bromide, oxygen and argon. The thinner the film thickness of the second material layer 22 is, the earlier it contacts the surface of the first material layer 21. Under the action of the van der Waals force, it is more difficult to be removed. Due to the blocking effect of the particle defect 33, a cone defect 34 is formed on the dielectric ring 121.

[0138] S13: Obtain the number of cone defects 34 on the semiconductor structure 10 to obtain a corresponding relationship between the number of target-sized particles and the number of cone defects 34 in the target solution.

[0139] Specifically, the present embodiment combines the life of the UF filter to perform correlation analysis. It can be understood that the service life of the UF filter is related to the target size particles in the target solution (pure water). Fig.17 As shown, the hollow circles in the figure represent the data obtained by the embodiment of the present application, and the solid circles represent the data obtained by the related art. It can be seen from the figure that the longer the UF filter is used, the more cone defects 34 there are. At the same time, by comparison, it can be seen that the linear slope of the data obtained by the embodiment of the present application is more sensitive than the test results of the related art.

[0140] Specifically, Fig.18 It shows the relationship between the thickness of the second material layer 22, the number of cone defects 34 and the thickness of the dielectric ring 121. As can be seen from the figure, the thicker the second material layer 22 is, the thinner the dielectric ring 121 is, and the higher the sensitivity to the cone defect 34 is. Further, the result shows that the evaluation method provided in the embodiment of the present application can well characterize the influence of particles smaller than the filtration size in the target solution on the process after the agglomerated particles 32 are formed.

[0141] It should be understood that, in the embodiments of the present application, although the various steps in the flowchart of the accompanying drawings are displayed in sequence according to the indication of the arrows, these steps are not necessarily executed in sequence in the order indicated by the arrows. Unless there is a clear description in this article, the execution of these steps is not strictly limited in order, and these steps can be executed in other orders. Moreover, at least a portion of the steps in the accompanying drawings may include multiple steps or multiple stages, and these steps or stages are not necessarily executed at the same time, but can be executed at different times, and the execution order of these steps or stages is not necessarily to be carried out in sequence, but can be executed in turn or alternately with other steps or at least a portion of the steps or stages in other steps.

[0142] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0143] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A semiconductor structure for evaluating solution contamination, It is characterized in that include: substrate; At least one ring structure is arranged on the substrate; wherein the ring structure includes a plurality of dielectric rings, each of which is nested in sequence and arranged at intervals from each other; in the ring structure, the width of each of the dielectric rings gradually increases along the direction from the outermost side of the ring structure to the center of the ring structure, and the width of the outermost dielectric ring is not less than the design size of the target device.

2. The semiconductor structure according to claim 1, It is characterized in that The dielectric rings in the sleeve ring structure are sleeved one after another in sequence along the same center.

3. The semiconductor structure according to claim 1, It is characterized in that The semiconductor structure includes a plurality of collar structures, and the plurality of collar structures are arranged on the substrate at intervals.

4. The semiconductor structure according to claim 3, It is characterized in that The width of the outermost dielectric ring of each of the ring structures gradually increases at a first preset increment.

5. The semiconductor structure according to claim 4, It is characterized in that The ratio of the first preset increment to the design size is between 0.05 and 0.

3.

6. The semiconductor structure according to any one of claims 1 to 5, It is characterized in that The width of the outermost dielectric ring of the collar structure is not greater than 20 times the designed size.

7. The semiconductor structure according to any one of claims 1 to 5, It is characterized in that The dielectric ring is in the shape of a rectangular ring; And / or, the material of the dielectric ring includes silicon dioxide.

8. The semiconductor structure according to any one of claims 1 to 5, It is characterized in that In the sleeve ring structure, the distance between any two adjacent dielectric rings is not equal; Or, in the sleeve ring structure, the distance between any two adjacent dielectric rings is equal to the designed size.

9. A method for evaluating solution contamination, It is characterized in that include: Providing a semiconductor structure as claimed in any one of claims 1 to 8; forming a composite layer on the semiconductor structure, and pre-wetting the composite layer with a target solution; removing the composite layer; The number of cone defects on the semiconductor structure is obtained to obtain a corresponding relationship between particles of a target size in the target solution and the number of cone defects.

10. The method for evaluating solution contamination according to claim 9, It is characterized in that The step of forming a composite layer on the semiconductor structure and pre-wetting the composite layer with a target solution comprises: forming a first material layer on the semiconductor structure; A second material layer is formed on the first material layer, and the second material layer is pre-wetted with a target solution.

11. The method for evaluating solution contamination according to claim 10, It is characterized in that The thickness of the second material layer is not greater than 150 nm; And / or, the first material layer is made of polysilicon.

12. The method for evaluating solution contamination according to claim 9, It is characterized in that The step of providing a semiconductor structure as claimed in any one of claims 1 to 8 comprises: forming an oxide layer on the substrate; A dielectric layer is formed on the oxide layer.

13. The method for evaluating solution contamination according to claim 12, It is characterized in that In the oxide layer, the number of particles having a particle size of not less than 0.2 μm is less than 20, and the number of particles having a particle size of 1 μm or more is less than 10; In the oxide layer, the number of particles with a particle size greater than or equal to 1 μm is less than 10; And / or, in the collar structure, the number of particles having a particle size not less than 0.2 μm is less than 20, and the number of particles having a particle size greater than or equal to 1 μm is less than 10.