Method for preparing ionic liquid supported resin based on ultrasonic and application thereof
By employing ultrasonic preparation and regeneration techniques, the problems of long synthesis time, high temperature, and unstable performance of ionic liquid-loaded resins have been solved, achieving high adsorption performance and regeneration efficiency, and improving the adsorption capacity and stability of the resin.
Patent Information
- Application Number
- CN202410988416.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Existing methods for synthesizing ionic liquid-supported resins suffer from long synthesis times, high temperatures, and unstable adsorption performance, leading to severe adsorption capacity decay. Furthermore, the regeneration process is complex and cannot restore the initial performance.
An ionic liquid-supported resin was prepared using ultrasound. Through ultrasonic mixing, magnetic stirring, and vacuum drying, combined with ethanol cleaning and gas pressure treatment, a high-efficiency ionic liquid-supported resin was prepared. The resin performance was further improved by utilizing the ultrasonic cavitation effect and activation treatment during the regeneration process.
It significantly shortens the preparation time, lowers the temperature, and improves the adsorption performance and regeneration efficiency of the resin, allowing the adsorption capacity to recover to or exceed the initial level, thus solving the problems existing in traditional methods.
Smart Images

Figure CN118904310B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ionic liquid-supported resin technology, specifically to a method for preparing ionic liquid-supported resin based on ultrasound and its application. Background Technology
[0002] Ionic liquid-supported resins are synthesized by chemical grafting of ionic liquids and polymers. Due to their good cleanliness, high cycling stability, and excellent selectivity, they are considered a promising new type of adsorbent material. Their cleanliness stems from the fact that, compared to traditional liquid-liquid extraction, ionic liquid-supported resins have less environmental impact, avoiding the volatilization of organic solvents and preventing turbidity and emulsification of the solution phase. Their selectivity is due to the ability to prepare ionic liquid-supported resins with different functional groups using various chemical reagents and chemical grafting methods, thus allowing for the design of ionic liquid-supported resins with different selectivities.
[0003] Ionic liquid-supported resins are prepared through chemical grafting, forming strong chemical bonds between the ionic liquid and the resin. This significantly reduces the loss of ionic liquid during adsorption and desorption, ensuring excellent cycling stability. Typically, the adsorption capacity decreases by only about 1% after each cycle, far lower than that of traditional solvent-impregnated resins. Current methods for synthesizing ionic liquid-supported resins utilize three-necked flasks and a constant-temperature magnetic stirrer, requiring synthesis times exceeding 8 hours and temperatures above 90°C. After numerous cycles (generally over 100), the adsorption capacity of the ionic liquid-supported resin decays to less than 80% of its initial value. Regeneration requires repeated preparation of the ionic liquid-supported resin, and the adsorption capacity of the regenerated resin cannot reach the level of the newly prepared resin.
[0004] Therefore, the present invention addresses the above-mentioned problems by preparing ionic liquid-supported resins using ultrasound. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a method for preparing ionic liquid-loaded resins based on ultrasound and its application.
[0006] A method for preparing ionic liquid-supported resin based on ultrasound includes the following steps:
[0007] S1. Chloromethylated polystyrene resin, glycine, and ultrapure water are ultrasonically mixed at 50-95°C for 30-120 minutes with a solid-liquid ratio of 0.2-0.3g:1g:10mL, and magnetic stirring is turned on simultaneously to obtain a mixture.
[0008] The ultrasonic power is 100–500W, and the magnetic stirring speed is 200–300 r / min.
[0009] S2. Filter the mixture obtained in S1 at room temperature to obtain resin. Then wash the resin 3 to 5 times with 10 to 30 mL of anhydrous ethanol. Dry the washed resin in a vacuum drying oven at 60 to 65 °C until constant weight to obtain ion liquid-supported resin.
[0010] Furthermore, the chloromethylated polystyrene resin has a particle size of 100-200 mesh, a crosslinking degree of 0.8-1.2% for divinylbenzene, and a chlorine content of 3.2-3.6 mmol / g.
[0011] Note: The particle size of chloromethylated polystyrene resin is beneficial to improving the resin's adsorption capacity and reactivity. The degree of crosslinking of divinylbenzene determines the mechanical strength and chemical stability of chloromethylated polystyrene resin. Higher chlorine content may increase the resin's hydrophilicity, but it may also increase its corrosivity.
[0012] Furthermore, before proceeding with S1, the chloromethylated polystyrene resin undergoes a pretreatment process, including the following steps:
[0013] The chloromethylated polystyrene resin was soaked in a 95% ethanol solution at a solid-liquid ratio of 1g:1.5-2.5mL for 11-13 hours, then filtered. The filtered chloromethylated polystyrene resin was then rinsed with ultrapure water until no turbidity was produced. The rinsed chloromethylated polystyrene resin was then dried in a vacuum drying oven at 60-65℃ to complete the pretreatment.
[0014] Note: Ethanol can remove grease, dust and other contaminants from the surface of resin, which helps to clean the resin. It can also affect the surface properties of the resin, making it more reactive and facilitating subsequent chemical reactions or processing.
[0015] Furthermore, the soaking is carried out in a container. During the first 1 / 4 to 1 / 3 of the soaking period, the air pressure inside the container is set to 2.5 to 3.5 MPa; during the last 1 / 4 to 1 / 3 of the soaking period, the air pressure inside the container is set to 8 to 10 MPa; and during the remaining soaking period, the air pressure inside the container is set to 0.5 to 1.5 MPa.
[0016] Explanation: Soaking the resin under low pressure helps remove air bubbles from the resin surface, increases the contact area between the resin and a 95% ethanol solution, thereby promoting the penetration of ethanol molecules into the resin interior. This helps clean the resin surface and pores, removing impurities and residues, and creating better conditions for subsequent processing. Further reducing the pressure helps to further clean the resin and promotes the opening of the resin pore structure, improving its permeability. Finally, increasing the pressure can enhance the permeability of the 95% ethanol solution, making it easier for ethanol to enter the resin's microporous structure. This helps to clean the resin more thoroughly and may promote the activation of functional groups inside the resin. In addition, high pressure can also cause changes in the resin's internal microstructure, such as pore size expansion or functional group rearrangement, thereby improving the overall activity of the resin.
[0017] The ionic liquid-supported resin prepared by any of the methods described above is used for the selective adsorption of phosphoric acid.
[0018] Furthermore, the ionic liquid-supported resin after selectively adsorbing phosphoric acid is regenerated.
[0019] Furthermore, the regeneration method is as follows:
[0020] Under ultrasonic power of 250–350 W and temperature of 70–80 °C, ionic liquid-loaded resin that has selectively adsorbed phosphoric acid once or multiple times, glycine, and ultrapure water are mixed at a solid-liquid ratio of 0.4–0.6 g: 1 g: 20 mL. After reacting for 1.5–2.5 h, the mixture is filtered to obtain the resin to be regenerated. The resin to be regenerated is washed 3–5 times with 10–30 mL of anhydrous ethanol. The washed resin is then dried to constant weight in a vacuum drying oven at 60–65 °C to obtain the regenerated ionic liquid-loaded resin.
[0021] Explanation: By utilizing the cavitation effect of ultrasound to expand the active interface sites inside the resin, organic chemical agents can be combined with more active sites in the ionic liquid-loaded resin with severely depleted adsorption capacity, thereby achieving efficient regeneration of the ionic liquid-loaded resin.
[0022] Furthermore, the ionic liquid-supported resin after selectively adsorbing phosphoric acid is first activated. The activation method is as follows:
[0023] First, the ionic liquid-loaded resin after selectively adsorbing phosphoric acid is subjected to moisture curing. The moisture curing temperature is 18-22℃, the air humidity is 65-75%, and the time is 25-35h. After moisture curing, 0.05-0.08% of the resin mass of charge adjustment agent is added and mixed for 10-15min. Then, the air humidity is adjusted to 80-85%, and moisture curing continues for 15-20h. After moisture curing, 0.01-0.02% of the resin mass of charge adjustment agent is added again for 10-15min, and then steam annealing is performed to complete the activation treatment.
[0024] Explanation: Moisture curing helps soften the resin, reduce internal stress, and improve its flexibility and ductility. It also helps restore its ion exchange capacity, preparing it for subsequent charge adjustment. Charge adjustment removes adsorbed impurity ions from the resin and reintroduces desired ions, allowing for effective utilization of the resin's ion exchange sites and improving its selectivity and efficiency. Steam annealing further helps remove residual solvents and impurities from the resin, while promoting internal structural remodeling and improving its thermal stability and mechanical strength. Steam annealing also helps eliminate micropores and defects in the resin, improving its overall performance.
[0025] Furthermore, the charge adjuster comprises, by mass percentage: 10-15% diethanolamine, 1-3% sulfonyloxyketone, and the balance vinyl acetate.
[0026] Explanation: Diethanolamine has good wettability and emulsifying properties, which can effectively regulate the charge distribution of resin. It can help improve the wettability of resin, making it easier for resin to react with other substances, thereby improving the efficiency of charge adjustment; sulfonyloxyketone can participate in the chemical reaction of resin as a catalyst, which can help accelerate the formation of ion exchange sites in resin and improve the ion exchange capacity of resin; vinyl acetate can undergo cross-linking reaction with resin, improving the mechanical strength and heat resistance of resin.
[0027] Furthermore, the relative humidity of the steam annealing is 55-65%, the temperature is 180-200℃, and the time is 10-30 minutes.
[0028] Note: If the relative humidity is too low, the resin may not be able to fully absorb moisture, resulting in poor annealing and affecting the resin's activation level and final performance. If the relative humidity is too high, the resin may absorb too much water, leading to structural changes or even damage, which is also detrimental to resin activation. If the temperature is too low, it may not be enough to activate the chemical bonds in the resin, preventing the resin's performance from being effectively restored. If the temperature is too high, it may cause the resin to decompose or deteriorate, damaging its structure and reducing its performance. If the time is too short, the resin may not be fully activated, while if the time is too long, the resin may be over-annealed, resulting in a decrease in performance.
[0029] Compared with existing methods for preparing ionic liquid-supported resins, the advantages of this invention are:
[0030] (1) Existing technologies synthesize ionic liquid-loaded resins by water bath heating and magnetic stirring, which have the problems of long synthesis time, high reaction temperature, and unstable synthesis effect. The adsorption performance of the product changes significantly with the variation of process parameters, which seriously hinders the industrial application of this process. Therefore, this invention is based on the characteristics of ultrasound, such as relatively low energy consumption, strong mechanical vibration effect, cavitation effect, and thermal effect at the solid-liquid interface. It utilizes the cavitation effect of ultrasound to expand the active interface sites inside the resin, promotes the combination of organic chemical agents with more active sites in the ionic liquid-loaded resin with severely depleted adsorption performance, thereby achieving efficient regeneration of ionic liquid-loaded resin. Compared with traditional flasks and constant temperature magnetic stirring devices, it can significantly shorten the preparation time and reduce the preparation temperature.
[0031] (2) The method for preparing the ionic liquid-supported resin of the present invention involves immersing the resin in ethanol to remove grease, dust, and other contaminants from the resin surface. This helps clean the resin and can affect its surface properties, making it more reactive and facilitating subsequent chemical reactions. Immersing the resin under low pressure helps remove air bubbles from the resin surface, increasing the contact area between the resin and the 95% ethanol solution, thereby promoting the penetration of ethanol molecules into the resin interior. This helps clean the resin surface and pores, removing impurities and residues and creating better conditions for subsequent processing. Further reducing the pressure helps to further clean the resin and promotes the opening of the resin pore structure, improving its permeability. Finally, increasing the pressure can improve the permeability of the 95% ethanol solution, making it easier for ethanol to enter the microporous structure of the resin. This helps to clean the resin more thoroughly and may promote the activation of functional groups inside the resin. In addition, high pressure can also cause changes in the microstructure inside the resin, such as the expansion of pore size or the rearrangement of functional groups, thereby improving the overall activity of the resin.
[0032] (3) In the regeneration of ionic liquid-loaded resin, the present invention first activates the ionic liquid-loaded resin after selectively adsorbing phosphoric acid to improve regeneration efficiency. Moisture curing helps soften the resin, reduce internal stress, and improve its flexibility and ductility. It also helps restore its ion exchange capacity, preparing it for subsequent charge adjustment. Charge adjustment removes impurity ions adsorbed by the resin and reintroduces the required ions, effectively utilizing the ion exchange sites of the resin and improving its selectivity and efficiency. Steam annealing helps further remove residual solvents and impurities from the resin, while promoting internal structural reorganization and improving its thermal stability and mechanical strength. Steam annealing also helps eliminate micropores and defects in the resin, improving its overall performance. Attached Figure Description
[0033] Figure 1 This is a comparison chart of the results of Investigation 1 of the preparation method of the present invention;
[0034] Figure 2 This is a comparison chart of the results of the second investigation into the regeneration method of the present invention;
[0035] Figure 3 This is a comparison chart of the results of the third investigation into the regeneration method of this invention;
[0036] Figure 4 This is a schematic diagram of the apparatus used in the preparation and regeneration method of the present invention. Detailed Implementation
[0037] To further illustrate the methods and effects of this invention, the technical solution of this invention will be clearly and completely described below in conjunction with experiments.
[0038] Example 1: This example describes a method for preparing ionic liquid-supported resin based on ultrasound, including the following steps:
[0039] The chloromethylated polystyrene resin is first pretreated, including the following steps:
[0040] The chloromethylated polystyrene resin was soaked in a 95% ethanol solution at a solid-liquid ratio of 1g:2mL for 12 hours. After soaking, it was filtered and then rinsed with ultrapure water until no turbidity was produced. The rinsed chloromethylated polystyrene resin was then dried in a vacuum drying oven at 62℃. The pretreatment was then completed.
[0041] S1. Chloromethylated polystyrene resin, glycine, and ultrapure water are ultrasonically mixed at 70°C for 75 min with a solid-liquid ratio of 0.25 g: 1 g: 10 mL, and magnetic stirring is turned on simultaneously to obtain a mixture; the chloromethylated polystyrene resin has a particle size of 140-160 mesh, a crosslinking degree of 1% for divinylbenzene, and a chlorine content of 3.4 mmol / g;
[0042] The ultrasonic power is 300W, and the magnetic stirring speed is 250r / min.
[0043] S2. The mixture obtained in S1 is filtered at room temperature (25°C) to obtain resin. The resin is then washed four times with 20 mL of anhydrous ethanol. The washed resin is then dried in a vacuum drying oven at 62°C to obtain ion liquid-supported resin.
[0044] Example 2: The ionic liquid-supported resin prepared by ultrasound in Example 1 was applied to the selective adsorption of phosphoric acid, that is, 4.5 mol / L phosphoric acid was adsorbed by the ionic liquid-supported resin. The liquid-solid ratio of phosphoric acid to ionic liquid-supported resin was 20 mL: 1 g, the oscillation frequency was 120 r / min, the time was 6 h, and the temperature was 25 °C.
[0045] The ionic liquid-supported resin after selective adsorption of phosphoric acid is then regenerated. The regeneration method is as follows:
[0046] Under the conditions of 300W ultrasonic power and 75℃, the ionic liquid-loaded resin that has selectively adsorbed phosphoric acid 100 times, glycine and ultrapure water were mixed at a solid-liquid ratio of 0.5g:1g:20mL. After reacting for 2 hours, the mixture was filtered to obtain the resin to be regenerated. The resin to be regenerated was washed 4 times with 20mL of anhydrous ethanol. The washed resin was then dried in a vacuum drying oven at 62℃ to constant weight to obtain the regenerated ionic liquid-loaded resin.
[0047] An apparatus is provided for the above preparation and regeneration methods, such as... Figure 1 As shown, the device includes an ultrasonic generator 1, a magnetic stirrer 2, a double-layered glass reactor 3, an ultrasonic probe 4, and a constant temperature bath 5. The ultrasonic probe 4 extends into the double-layered glass reactor 3 and is electrically connected to the ultrasonic generator 1. The output end of the magnetic stirrer 2 contacts the bottom of the double-layered glass reactor 3. The double-layered glass reactor 3 has a jacket for circulating water flow on its side wall. The constant temperature bath 5 is connected to the jacket through a water supply pipe. The ultrasonic generator 1, ultrasonic probe 4, magnetic stirrer 2, and constant temperature bath 5 are all existing equipment.
[0048] Example 3: The difference between this example and Example 1 is that in the preparation method, chloromethylated polystyrene resin is soaked in a 95% ethanol solution at a solid-liquid ratio of 1g:1.5mL, and filtered after soaking for 11 hours.
[0049] Example 4: The difference between this example and Example 1 is that in the preparation method, chloromethylated polystyrene resin is soaked in a 95% ethanol solution at a solid-liquid ratio of 1g:2.5mL for 13 hours and then filtered.
[0050] Example 5: This example differs from Example 1 in that, in the preparation method, the chloromethylated polystyrene resin has a particle size of 100-140 mesh, the degree of crosslinking of divinylbenzene is 0.8%, and the chlorine content is 3.2 mmol / g.
[0051] Example 6: This example differs from Example 1 in that, in the preparation method, the chloromethylated polystyrene resin has a particle size of 160-200 mesh, the degree of crosslinking of divinylbenzene is 1.2%, and the chlorine content is 3.6 mmol / g.
[0052] Example 7: The difference between this example and Example 1 is that in the preparation method, chloromethylated polystyrene resin, glycine and ultrapure water are ultrasonically mixed at 50°C with a solid-liquid ratio of 0.2g:1g:10mL.
[0053] Example 8: The difference between this example and Example 1 is that in the preparation method, chloromethylated polystyrene resin, glycine and ultrapure water are ultrasonically mixed at 95°C with a solid-liquid ratio of 0.3g:1g:10mL.
[0054] Example 9: The difference between this example and Example 1 is that the ultrasonic power is 100W and the ultrasonic mixing time is 30min in the preparation method.
[0055] Example 10: The difference between this example and Example 1 is that the ultrasonic power is 500W and the ultrasonic mixing time is 120min in the preparation method.
[0056] Example 11: The difference between this example and Example 1 is that the magnetic stirring speed is 200 r / min in the preparation method.
[0057] Example 12: The difference between this example and Example 1 is that the magnetic stirring speed is 300 r / min in the preparation method.
[0058] Example 13: This example differs from Example 1 in that, in the preparation method, the resin is rinsed three times with 10 mL of anhydrous ethanol and dried in a vacuum drying oven at 60°C.
[0059] Example 14: The difference between this example and Example 1 is that in the preparation method, the resin is rinsed 5 times with 30 mL of anhydrous ethanol and dried in a vacuum drying oven at 65°C.
[0060] Example 15: The difference between this example and Example 1 is that in the preparation method, the soaking is carried out in a container. During the first 1 / 4 to 1 / 3 of the soaking time, the air pressure inside the container is set to 3 MPa; during the last 1 / 4 to 1 / 3 of the soaking time, the air pressure inside the container is set to 9 MPa; and during the remaining soaking time, the air pressure inside the container is set to 1 MPa.
[0061] Example 16: This example differs from Example 15 in that the air pressure inside the container is set to 2.5 MPa during the first 1 / 4 to 1 / 3 of the soaking period; the air pressure inside the container is set to 8 MPa during the last 1 / 4 to 1 / 3 of the soaking period; and the air pressure inside the container is set to 0.5 MPa during the remaining soaking period.
[0062] Example 17: This example differs from Example 15 in that the air pressure inside the container is set to 3.5 MPa during the first 1 / 4 to 1 / 3 of the soaking period; the air pressure inside the container is set to 10 MPa during the last 1 / 4 to 1 / 3 of the soaking period; and the air pressure inside the container is set to 1.5 MPa during the remaining soaking period.
[0063] Example 18: The difference between this example and Example 2 is that in the regeneration method, the used ionic liquid-loaded resin, glycine and ultrapure water are mixed under the conditions of 250W ultrasonic power and 70°C.
[0064] Example 19: The difference between this example and Example 2 is that in the regeneration method, the used ionic liquid-loaded resin, glycine and ultrapure water are mixed under the conditions of 350W ultrasonic power and 80°C.
[0065] Example 20: The difference between this example and Example 2 is that in the regeneration method, the ionic liquid-loaded resin after selectively adsorbing phosphoric acid once, glycine, and ultrapure water are mixed at a solid-liquid ratio of 0.4g:1g:20mL, reacted for 1.5h, and then filtered.
[0066] Example 21: The difference between this example and Example 2 is that in the regeneration method, the ionic liquid-loaded resin after selectively adsorbing phosphoric acid 100 times, glycine, and ultrapure water are mixed at a solid-liquid ratio of 0.6g:1g:20mL, reacted for 2.5h, and then filtered.
[0067] Example 22: The difference between this example and Example 2 is that in the regeneration method, after rinsing the resin to be regenerated three times with 10 mL of anhydrous ethanol, the rinsed resin is dried to constant weight in a vacuum drying oven at 60°C.
[0068] Example 23: The difference between this example and Example 2 is that in the regeneration method, the resin to be regenerated is rinsed 5 times with 30 mL of anhydrous ethanol, and then the rinsed resin is dried in a vacuum drying oven at 65°C until constant weight.
[0069] Example 24: This example differs from Example 2 in that, in the regeneration method, the ionic liquid-supported resin after selectively adsorbing phosphoric acid is first activated. The activation method is as follows:
[0070] First, the used ionic liquid-loaded resin is subjected to moisture curing at a temperature of 20°C, an air humidity of 70%, and a time of 30 hours. After moisture curing, 0.065% of the resin mass of charge adjuster (K2483 charge adjuster) is added and mixed for 12 minutes. Then, the air humidity is adjusted to 82%, and moisture curing continues for 18 hours. After moisture curing, 0.015% of the resin mass of charge adjuster is added again and mixed for 12 minutes. Then, steam annealing is performed at a relative humidity of 60%, a temperature of 190°C, and a time of 20 minutes. The activation treatment is then complete.
[0071] Example 25: This example differs from Example 24 in that the moisture curing temperature is 18°C, the air humidity is 65%, and the time is 25 hours.
[0072] Example 26: This example differs from Example 24 in that the moisture curing temperature is 22°C, the air humidity is 75%, and the time is 35 hours.
[0073] Example 27: The difference between this example and Example 24 is that after moisture curing, a charge adjuster accounting for 0.05% of the resin mass is added and mixed for 10 minutes.
[0074] Example 28: The difference between this example and Example 24 is that after moisture curing, a charge adjuster accounting for 0.08% of the resin mass is added and mixed for 15 minutes.
[0075] Example 29: The difference between this example and Example 24 is that the air humidity is adjusted to 80% and the curing is continued for 20 hours.
[0076] Example 30: The difference between this example and Example 24 is that the air humidity is adjusted to 85% and the curing is continued for 20 hours.
[0077] Example 31: The difference between this example and Example 24 is that a charge adjuster of 0.01% of the resin mass is added for 10 minutes after moisture curing.
[0078] Example 32: The difference between this example and Example 24 is that a charge adjuster of 0.02% of the resin mass is added for 15 minutes after moisture curing.
[0079] Example 33: This example differs from Example 24 in that the relative humidity of the steam annealing is 55%, the temperature is 180°C, and the time is 10 minutes.
[0080] Example 34: This example differs from Example 24 in that the relative humidity of the steam annealing is 65%, the temperature is 200°C, and the time is 30 minutes.
[0081] Example 35: This example differs from Example 1 in that the charge adjuster, by mass percentage, comprises: 12.5% diethanolamine, 2% sulfonyloxyketone, and the balance vinyl acetate.
[0082] Example 36: This example differs from Example 35 in that the charge adjuster, by mass percentage, comprises: 10% diethanolamine, 1% sulfonyloxyketone, and the balance vinyl acetate.
[0083] Example 37: This example differs from Example 35 in that the charge adjuster, by mass percentage, comprises: 15% diethanolamine, 3% sulfonyloxyketone, and the balance vinyl acetate.
[0084] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and aims to illustrate the practical application effect of the present invention.
[0085] 1. Ionic liquid-supported resins were prepared and regenerated using conventional methods. Adsorption was compared with that of ionic liquid-supported resins prepared and regenerated using this method under the same conditions, and the adsorption capacity was calculated. The results are as follows:
[0086] Depend on Figure 1 As shown, the ionic liquid-supported resin prepared in Example 1 selectively adsorbed phosphoric acid once using the application method of Example 2, with an adsorption capacity of 312 mg / g. In contrast, the control example 1 was prepared using conventional synthesis with optimal conditions of 105°C and 8 hours, and the maximum adsorption capacity of the prepared ionic liquid-supported resin was 260 mg / g. This demonstrates that the ultrasonically prepared ionic liquid-supported resin significantly shortened the preparation time, reduced the preparation temperature, and effectively increased the adsorption performance of the resin.
[0087] Depend on Figure 2 As shown, the ionic liquid-supported resin prepared in Example 1 selectively adsorbed phosphoric acid 100 times using the application method of Example 2, and the adsorption capacity significantly decreased to 208 mg / g. Example 2 is the ionic liquid-supported resin regenerated by ultrasonic enhancement. The adsorption capacity of the regenerated ionic liquid-supported resin reached 285 mg / g, which is higher than that of the newly prepared ionic liquid-supported resin under conventional conditions. However, the conventional method of regeneration, i.e., Control Example 2, requires a reaction at 105°C for 8 hours, and the adsorption capacity of the regenerated ionic liquid-supported resin is only 229 mg / g, which is only 88% of that of the conventionally synthesized new resin.
[0088] Therefore, ultrasonic regeneration of ionic liquid-loaded resin can significantly reduce regeneration time and temperature, and can restore the adsorption capacity of the resin after selective adsorption of phosphoric acid to the initial level, or even exceed the initial value.
[0089] 2. To investigate the effect of parameters for ultrasonic preparation of ionic liquid-supported resin on its adsorption capacity.
[0090] Depend on Figure 1 Comparing Examples 1 to 14, it can be seen that excessively small or large soaking parameters, excessively small or large parameters of chloromethylated polystyrene resin, excessively small or large mixing temperature, excessively small or large ultrasonic parameters, excessively small or large stirring speed, and excessively small or large drying parameters will all reduce the adsorption capacity of the ionic liquid-loaded resin. Therefore, the parameters in Example 1 are more effective.
[0091] Comparing Examples 1 and 15-17, it can be seen that linking the soaking time with the pressure during soaking can significantly increase the adsorption capacity of the ionic liquid-loaded resin. However, too small or too large a pressure change will also reduce the improvement rate. Therefore, the parameters of Example 15 are relatively better.
[0092] 3. Investigate the effect of parameters of ultrasonically regenerated ionic liquid-supported resin on its adsorption capacity.
[0093] Depend on Figure 2 Comparing Examples 2 and 18-23, it can be seen that excessively small or large ultrasonic parameters, excessively small or large mixing parameters, and excessively small or large drying parameters will reduce the adsorption capacity of the ionic liquid-loaded resin. Therefore, the parameters in Example 2 are more effective.
[0094] 4. Investigate the effect of activation treatment parameters on the adsorption capacity during ultrasonic regeneration.
[0095] The difference between Comparative Example 3 and Example 24 is that the parameters for the two moisture curing processes remain unchanged;
[0096] The difference between Comparative Example 4 and Example 24 is that the amount of charge adjuster added remains the same in both cases;
[0097] The difference between Comparative Example 5 and Example 24 is that steam annealing is not performed.
[0098] Depend on Figure 3 The results show that Examples 24-34 significantly increased the adsorption capacity of the ionic liquid-supported resin compared to Example 2. However, Control Examples 3 and 4 lacked the regular changes between the two times, and Control Example 5 lacked steam annealing, which reduced the improvement rate of Examples 24-34. Therefore, the regular changes and the scheme effects of Examples 24-34 are better.
[0099] Comparing Examples 24-37, it can be seen that excessively small or large parameters during the two moisture curing cycles, excessively small or large amounts of charge modifier added during the two cycles, and excessively small or large parameters during steam annealing all reduce the adsorption capacity of the ionic liquid-supported resin. Therefore, in summary, the parameters of Example 24 are relatively better. Examples 35-37 provide charge modifiers that are more suitable for this method, which further improve the adsorption capacity of the ionic liquid-supported resin compared to Example 24. However, excessively small or large proportions of vinyl acetate can also reduce the improvement rate. Therefore, in summary, Example 35 is relatively better.
Claims
1. A method for regenerating an ionic liquid-supported resin after selective adsorption of phosphoric acid, characterized in that, A method for preparing ionic liquid-supported resin includes the following steps: S1. Chloromethylated polystyrene resin, glycine, and ultrapure water are ultrasonically mixed at 50-95℃ for 30-120 minutes with a solid-liquid ratio of 0.2-0.3g:1g:10mL, and magnetic stirring is turned on simultaneously to obtain a mixture. The ultrasonic power is 100~500W, and the magnetic stirring speed is 200~300r / min; S2. Filter the mixture obtained in S1 at room temperature to obtain resin. Then wash the resin with 10-30 mL of anhydrous ethanol 3-5 times. Dry the washed resin in a vacuum drying oven at 60-65℃ to constant weight to obtain ion liquid-loaded resin. The ionic liquid-supported resin is used for selective adsorption of phosphoric acid, and the ionic liquid-supported resin after selective adsorption of phosphoric acid is regenerated. The regeneration method is as follows: The ionic liquid-supported resin that selectively adsorbs phosphoric acid is first activated. The activation method is as follows: The ionic liquid-loaded resin after selectively adsorbing phosphoric acid is subjected to moisture curing at a temperature of 18-22°C, an air humidity of 65-75%, and a time of 25-35 hours. After moisture curing, 0.05-0.08% (by weight of the resin) of charge modifier is added and mixed for 10-15 minutes. The air humidity is then adjusted to 80-85%, and moisture curing continues for 15-20 hours. After moisture curing, 0.01-0.02% (by weight of the resin) of charge modifier is added again and mixed for 10-15 minutes. Then, steam annealing is performed to complete the activation treatment. The charge modifier, by weight percentage, includes: 10-15% diethanolamine, 1-3% sulfonyloxyketone, and the balance being vinyl acetate. Then, under ultrasonic power of 250~350W and temperature of 70~80℃, the ionic liquid-supported resin after selective adsorption of phosphoric acid, glycine and ultrapure water are mixed at a solid-liquid ratio of 0.4~0.6g:1g:20mL. After reacting for 1.5~2.5h, the mixture is filtered to obtain the resin to be regenerated. The resin to be regenerated is washed 3~5 times with 10~30mL of anhydrous ethanol. The washed resin is then dried in a vacuum drying oven at 60~65℃ to constant weight to obtain the regenerated ionic liquid-supported resin.
2. The regeneration method as described in claim 1, characterized in that, The chloromethylated polystyrene resin has a particle size of 100-200 mesh, a crosslinking degree of 0.8-1.2% for divinylbenzene, and a chlorine content of 3.2-3.6 mmol / g.
3. The regeneration method as described in claim 1, characterized in that, Before proceeding with S1, the chloromethylated polystyrene resin undergoes a pretreatment process, including the following steps: The chloromethylated polystyrene resin was soaked in a 95% ethanol solution at a solid-liquid ratio of 1g:1.5~2.5mL for 11~13h, then filtered. The filtered chloromethylated polystyrene resin was then rinsed with ultrapure water until no turbidity was produced. The rinsed chloromethylated polystyrene resin was then dried in a vacuum drying oven at 60~65℃ to complete the pretreatment.
4. The regeneration method as described in claim 3, characterized in that, The soaking is carried out in a container. During the first 1 / 4 to 1 / 3 of the soaking period, the air pressure inside the container is set to 2.5 to 3.5 MPa; during the last 1 / 4 to 1 / 3 of the soaking period, the air pressure inside the container is set to 8 to 10 MPa; and during the remaining soaking period, the air pressure inside the container is set to 0.5 to 1.5 MPa.
5. The regeneration method as described in claim 1, characterized in that, The steam annealing process involves a relative humidity of 55-65%, a temperature of 180-200℃, and a time of 10-30 minutes.
Citation Information
Patent Citations
Method and device for rapidly producing ion liquid by promoting synthesis reaction with ultrasonic wave
CN102372676A
Heavy metal ion adsorbent for grafting glycine to chloromethylated polystyrene, preparation method and application thereof
CN104209102A
Supported alkyl imidazole ionic liquid adsorbing material as well as preparation method and application thereof
CN117680096A
Method for regenerating porous phosphorus adsorbent
KR101464195B1