Preparation method and application of basalt coupled carbon fiber composite bioelectrode
By using a method for preparing a basalt fiber and carbon fiber composite bioelectrode, combined with SiCnw/Ti60 composite material, the problems of high cost and poor conductivity of existing bioelectrode materials have been solved, achieving a highly efficient industrial wastewater treatment effect.
Patent Information
- Application Number
- CN202410972573.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing bioelectrode materials are expensive in microbial fuel cells and cannot be mass-produced on a large scale. In addition, ordinary biological fillers have poor conductivity and cannot effectively improve biodegradation, making it difficult to treat high-concentration, recalcitrant organic wastewater from the chemical industry.
A basalt fiber and carbon fiber composite, combined with SiCnw/Ti60 composite material, is used to form a basalt-coupled carbon fiber composite bioelectrode through etching and braiding, which enhances biocompatibility and mechanical properties.
It significantly improves the biocompatibility and conductivity of the electrodes, enhances the biodegradability of the microbial electrolysis cell, has high degradation efficiency and low cost, and is suitable for industrial wastewater treatment.
Smart Images

Figure CN118908398B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of bioelectrode technology, specifically relating to a method for preparing and applying a basalt-coupled carbon fiber composite bioelectrode. Background Technology
[0002] In the process of treating chemical industry wastewater using biotechnology, the activity of microorganisms and the efficiency of electron transfer are key factors affecting the bio-purification effect. Microbial electrochemical systems (BES), as a new technology, are currently widely used in environmental bioremediation. Their main principle is to utilize microorganisms to degrade organic pollutants while simultaneously converting the chemical energy in the pollutants into electrical energy in situ, representing a novel biotechnology and energy recovery technology. Representative technologies include microbial fuel cells (MFCs) and microbial electrolyzers (MECs).
[0003] The material and selection of the electrode directly affect the degradation efficiency and voltage output of the bioelectrode system (BES) for pollutants. Currently, widely used bioelectrode materials are mostly carbon-based materials (graphite electrodes, carbon cloth, etc.), metallic materials (nickel foam, titanium wire mesh, etc.), conductive polymer materials (glassy carbon), and composite electrodes (polyaniline coating, carbon nanotube composites). Among these, carbon-based materials have been widely used in microbial fuel cells due to their good electrochemical stability, biocompatibility, and structural plasticity. Compared to other electrode materials, carbon-based materials are inexpensive and readily available, but they are still relatively expensive compared to packing materials in conventional biological systems, preventing large-scale mass production and thus limiting the industrial application of BES in wastewater treatment. Furthermore, most ordinary biological packing materials lack good conductivity and cannot be used to construct BES to improve biodegradation; they can only serve to enrich microorganisms and form biofilms. Therefore, the development of novel bioelectrode materials for industrial applications is urgently needed.
[0004] Industrial wastewater contains various recalcitrant organic compounds, which pose a threat to the environment and human health. Wastewater generated during chemical production processes often contains large amounts of recalcitrant organic pollutants with complex compositions, high concentrations, and poor biodegradability, making it difficult for biotechnology to achieve the desired results.
[0005] Therefore, how to improve the preparation method and materials of composite bioelectrodes to further enhance their biocompatibility and mechanical properties, thereby improving their biodegradability of wastewater, has become a technical problem to be solved in this field. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing a basalt-coupled carbon fiber composite bioelectrode, which addresses the technical problem of how to improve the preparation method and materials of the composite bioelectrode to further enhance its biocompatibility and mechanical properties, thereby improving its biodegradation performance for wastewater.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] A method for preparing a basalt-coupled carbon fiber composite bioelectrode includes the following steps:
[0009] (1) Using Soxhlet extraction, basalt fibers are placed in a solvent and the original wetting agent on the surface of the basalt fibers is dissolved by heating and reflux. After Soxhlet extraction, the fibers are removed, washed with water and dried to obtain clean basalt fibers.
[0010] (2) Etching treatment of basalt fiber: an etching solution was prepared by sodium hydroxide, hydrochloric acid and nitric acid. The clean basalt fiber was immersed in the etching solution. Etching increases the specific surface area, surface roughness and adhesion of the fiber. After the reaction is completed, the fiber is taken out, washed with water and dried to obtain basalt fiber filler.
[0011] (3) After cutting the carbon fiber, soak it in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, then put it in acetone overnight and store it before taking it out and drying it.
[0012] (4) Basalt fiber filler and carbon fiber are braided and connected in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material.
[0013] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling to obtain mixed powder;
[0014] (6) The mixed powder was placed into a graphite mold with a diameter of 1 mm and sintered using a spark plasma activation sintering furnace to complete the coupling of SiCnw and Ti60, and finally obtained the SiCnw / Ti60 composite material.
[0015] (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two titanium wires are twisted continuously to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material to obtain the basalt coupled carbon fiber composite bioelectrode material.
[0016] Furthermore, in the preparation method of the basalt coupled carbon fiber composite bioelectrode, in step (1), the solvent used is one of acetone, isopropanol, cyclohexane, and petroleum ether, the reflux temperature is 40-100℃, and the reflux time is 12-72h.
[0017] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (2), the concentration of sodium hydroxide is 0.5-2 mol / L; the concentration of hydrochloric acid is 0.5-2 mol / L; the concentration of nitric acid is 0.01-0.1 mol / L; the etching time is 10-120 min; and the etching solution temperature is 20-100℃.
[0018] Preferably, the sodium hydroxide concentration is 1 mol / L; the hydrochloric acid concentration is 1 mol / L; the nitric acid concentration is 0.03 mol / L; the etching time is 60 min; and the etching solution temperature is 40 °C.
[0019] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (5), the grinding jar and grinding balls are made of stainless steel, the ball-to-material ratio is 3-5:1, the grinding speed of the ball mill is 300-500 r / min, and the grinding time is 4-6 h.
[0020] Furthermore, in the preparation method of the basalt-coupled carbon fiber composite bioelectrode, in step (6), the sintering temperature is 1000-1200℃, the pressure is 40-60MPa, and the holding time is 5-20min.
[0021] This invention also provides a method for applying a basalt-coupled carbon fiber composite bioelectrode in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor includes the following steps:
[0022] (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell;
[0023] (2) Inoculation of microbial communities: Electroactive microbial communities in the sludge are inoculated onto the anode of the reactor;
[0024] (3) Cultivating biofilm: After inoculation, a stable electroactive biofilm is formed after 7 days of cultivation;
[0025] (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it, and the pH of the wastewater is controlled to be 6-8.
[0026] (5) Operation: Apply an external voltage between the anode and cathode of the microbial electrolysis cell, with a voltage range of 0.02 to 0.4V;
[0027] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0028] Preferably, the sludge inoculated in step (2) is taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge is anaerobically cultured in the laboratory for one week, it is diluted with tap water at a sludge-to-water volume ratio of 1:2, and then 2L of diluted sludge is introduced into the anode of the device; in step (4), the pH of the wastewater is controlled to be 7.
[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. The preparation method of the basalt-coupled carbon fiber composite bioelectrode of the present invention, based on the prior art, involves connecting basalt fiber filler with carbon fiber strands in a braided manner, and tightly connecting the basalt carbon fiber composite material with the SiCnw / Ti60 composite material. Due to the large specific surface area and superior biocompatibility of basalt fiber, the excellent conductivity of carbon fiber, and the good biocompatibility, stable electrochemical performance, and excellent mechanical properties of the SiCnw / Ti60 composite material, the bio-carrying capacity, conductivity, and mechanical properties of the electrode are greatly improved. When applied to a microbial electrolysis cell, microorganisms can quickly attach to the electrode material and form a biofilm. When placed in a conventional biofilter and biological system, the biodegradability can be significantly improved.
[0031] 2. The preparation method of basalt coupled carbon fiber composite bioelectrode is simple, low-cost, and has mild process conditions. The addition of SiCnw / Ti60 composite material and electroactive bacteria can improve the organic matter removal efficiency, providing an efficient solution for industrial wastewater treatment. Attached Figure Description
[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0033] Figure 1 A schematic diagram of the fabrication of the basalt-coupled carbon fiber composite bioelectrode of the present invention;
[0034] Figure 2 Electron micrographs of the material in the microbial electrolysis cell of the present invention before and after microbial biofilm formation;
[0035] Figure 3 An embodiment of the microbial electrolysis cell of the present invention. Detailed Implementation
[0036] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0037] Example 1
[0038] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0039] (1) Using Soxhlet extraction, basalt fibers were placed in acetone and the original wetting agent on the surface of the basalt fibers was dissolved by heating and reflux. The heating and reflux temperature was 40℃ and the heating and reflux time was 12h. After Soxhlet extraction, the fibers were taken out, washed with water and dried to obtain clean basalt fibers.
[0040] (2) Etching treatment of basalt fiber: an etching solution was prepared by using 0.5 mol / L sodium hydroxide, 0.5 mol / L hydrochloric acid and 0.01 mol / L nitric acid. The clean basalt fiber was immersed in the etching solution for 10 min. The etching solution temperature was 20℃. After the reaction was completed, the fiber was taken out, washed with water and dried to obtain basalt fiber filler.
[0041] (3) After cutting the carbon fiber, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, then placed in acetone overnight for storage, and then dried. The carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods.
[0042] (4) Basalt fiber filler and carbon fiber are connected by strands in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material. The porosity of basalt fiber provides attachment points for biomolecules, while the conductivity of carbon fiber provides an electron transfer channel for electrochemical degradation.
[0043] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling. The ball-to-material ratio is 3:1, the ball mill speed is 300 r / min, and the ball milling time is 4 h to obtain mixed powder. Titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. One-dimensional nanomaterial silicon carbide nanowires (SiCnw) not only inherit the excellent properties of high strength and low thermal expansion coefficient of SiC, but also have better mechanical properties, such as higher strength and better toughness, due to its unique nanoscale effect.
[0044] (6) The mixed powder is placed in a graphite mold with a diameter of 1 mm and sintered in a spark plasma sintering furnace. The sintering temperature is 1000℃, the pressure is 40MPa, and the holding time is 5min to complete the coupling of SiCnw and Ti60 and obtain SiCnw / Ti60 composite material.
[0045] (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two SiCnw / Ti60 composite materials are twisted continuously to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally the basalt coupled carbon fiber composite bioelectrode material is obtained. The prepared basalt coupled carbon fiber composite bioelectrode material is named MBFNW1.
[0046] The above-mentioned MBFNW1 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor includes the following steps:
[0047] (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell;
[0048] (2) Inoculation of microbial community: The electroactive microbial community in the sludge is inoculated into the anode of the reactor. The sludge used for inoculation is taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge is anaerobically cultured for one week, it is diluted with tap water at a sludge-to-water volume ratio of 1:2. 2L of diluted sludge is then introduced into the anode of the device.
[0049] (3) Cultivating biofilm: After inoculating sludge, a stable electroactive biofilm is formed after 7 days of cultivation;
[0050] (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it, and the pH of the wastewater is controlled to be 6.
[0051] (5) Operation: Apply an external voltage of 0.02V between the anode and cathode of the microbial electrolysis cell;
[0052] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0053] Example 2
[0054] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0055] (1) Using Soxhlet extraction, basalt fibers were placed in acetone and the original wetting agent on the surface of the basalt fibers was dissolved by heating and reflux. The heating and reflux temperature was 50℃ and the heating and reflux time was 24h. After Soxhlet extraction, the fibers were taken out, washed with water and dried to obtain clean basalt fibers.
[0056] (2) Etching treatment of basalt fiber: an etching solution was prepared by using 1 mol / L sodium hydroxide, 1 mol / L hydrochloric acid and 0.02 mol / L nitric acid. The clean basalt fiber was immersed in the etching solution for 30 min. The etching solution temperature was 30℃. After the reaction was completed, the fiber was taken out, washed with water and dried to obtain basalt fiber filler.
[0057] (3) After cutting the carbon fiber, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, then placed in acetone overnight for storage, and then dried. The carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods.
[0058] (4) Basalt fiber filler and carbon fiber are connected by strands in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material. The porosity of basalt fiber provides attachment points for biomolecules, while the conductivity of carbon fiber provides an electron transfer channel for electrochemical degradation.
[0059] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling. The ball-to-material ratio is 3:1, the ball mill speed is 300 r / min, and the ball milling time is 4 h to obtain mixed powder. Titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. One-dimensional nanomaterial silicon carbide nanowires (SiCnw) not only inherit the excellent properties of high strength and low thermal expansion coefficient of SiC, but also have better mechanical properties, such as higher strength and better toughness, due to its unique nanoscale effect.
[0060] (6) The mixed powder was placed in a graphite mold with a diameter of 1 mm and sintered in a spark plasma sintering furnace. The sintering temperature was 1100℃, the pressure was 45MPa, and the holding time was 10min to complete the coupling of SiCnw and Ti60 and obtain SiCnw / Ti60 composite material.
[0061] (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two SiCnw / Ti60 composite materials are twisted continuously to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally the basalt coupled carbon fiber composite bioelectrode material is obtained. The prepared basalt coupled carbon fiber composite bioelectrode material is named MBFNW2.
[0062] The above-mentioned MBFNW2 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor includes the following steps:
[0063] (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell;
[0064] (2) Inoculation of microbial community: The electroactive microbial community in the sludge is inoculated into the anode of the reactor. The sludge used for inoculation is taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge is anaerobically cultured for one week, it is diluted with tap water at a sludge-to-water volume ratio of 1:2. 2L of diluted sludge is then introduced into the anode of the device.
[0065] (3) Cultivating biofilm: After inoculating sludge, a stable electroactive biofilm is formed after 7 days of cultivation;
[0066] (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it, and the pH of the wastewater is controlled to be 7.
[0067] (5) Operation: Apply an external voltage of 0.05V between the anode and cathode of the microbial electrolysis cell;
[0068] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0069] Example 3
[0070] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0071] (1) Using Soxhlet extraction, basalt fibers were placed in isopropanol and the original wetting agent on the surface of the basalt fibers was dissolved by heating and reflux. The heating and reflux temperature was 60℃ and the heating and reflux time was 24h. After Soxhlet extraction, the fibers were taken out, washed with water and dried to obtain clean basalt fibers.
[0072] (2) Etching treatment of basalt fiber: an etching solution was prepared by using 1 mol / L sodium hydroxide, 1 mol / L hydrochloric acid and 0.03 mol / L nitric acid. The clean basalt fiber was immersed in the etching solution for 60 min and the etching solution temperature was 40℃. After the reaction was completed, the fiber was taken out, washed with water and dried to obtain basalt fiber filler.
[0073] (3) After cutting the carbon fiber, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, then placed in acetone overnight for storage, and then dried. The carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods.
[0074] (4) Basalt fiber filler and carbon fiber are connected by strands in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material. The porosity of basalt fiber provides attachment points for biomolecules, while the conductivity of carbon fiber provides an electron transfer channel for electrochemical degradation.
[0075] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling. The ball-to-material ratio is 3:1, the ball mill speed is 300 r / min, and the ball milling time is 5 h to obtain mixed powder. Titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. One-dimensional nanomaterial silicon carbide nanowires (SiCnw) not only inherit the excellent properties of high strength and low thermal expansion coefficient of SiC, but also have better mechanical properties, such as higher strength and better toughness, due to its unique nanoscale effect.
[0076] (6) The mixed powder is placed in a graphite mold with a diameter of 1 mm and sintered in a spark plasma sintering furnace. The sintering temperature is 1000℃, the pressure is 45MPa, and the holding time is 5min to complete the coupling of SiCnw and Ti60 and obtain SiCnw / Ti60 composite material.
[0077] (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two SiCnw / Ti60 composite materials are twisted continuously to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally the basalt coupled carbon fiber composite bioelectrode material is obtained. The prepared basalt coupled carbon fiber composite bioelectrode material is named MBFNW3.
[0078] The above-mentioned MBFNW3 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor includes the following steps:
[0079] (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell;
[0080] (2) Inoculation of microbial community: The electroactive microbial community in the sludge is inoculated into the anode of the reactor. The sludge used for inoculation is taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge is anaerobically cultured for one week, it is diluted with tap water at a sludge-to-water volume ratio of 1:2. 2L of diluted sludge is then introduced into the anode of the device.
[0081] (3) Cultivating biofilm: After inoculating sludge, a stable electroactive biofilm is formed after 7 days of cultivation;
[0082] (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it, and the pH of the wastewater is controlled to be 7.
[0083] (5) Operation: Apply an external voltage of 0.1V between the anode and cathode of the microbial electrolysis cell;
[0084] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0085] Example 4
[0086] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0087] (1) Using Soxhlet extraction, basalt fibers were placed in cyclohexane and the original wetting agent on the surface of the basalt fibers was dissolved by heating and reflux. The heating and reflux temperature was 80℃ and the heating and reflux time was 72h. After Soxhlet extraction, the fibers were taken out, washed with water and dried to obtain clean basalt fibers.
[0088] (2) Etching treatment of basalt fiber: an etching solution was prepared by using 1.5 mol / L sodium hydroxide, 1.5 mol / L hydrochloric acid and 0.05 mol / L nitric acid. The clean basalt fiber was immersed in the etching solution for 120 min. The etching solution temperature was 80℃. After the reaction was completed, the fiber was taken out, washed with water and dried to obtain basalt fiber filler.
[0089] (3) After cutting the carbon fiber, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, then placed in acetone overnight for storage, and then dried. The carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods.
[0090] (4) Basalt fiber filler and carbon fiber are connected by strands in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material. The porosity of basalt fiber provides attachment points for biomolecules, while the conductivity of carbon fiber provides an electron transfer channel for electrochemical degradation.
[0091] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling. The ball-to-material ratio is 4:1, the ball mill speed is 400 r / min, and the ball milling time is 5 h to obtain mixed powder. Titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. One-dimensional nanomaterial silicon carbide nanowires (SiCnw) not only inherit the excellent properties of high strength and low thermal expansion coefficient of SiC, but also have better mechanical properties, such as higher strength and better toughness, due to its unique nanoscale effect.
[0092] (6) The mixed powder was placed in a graphite mold with a diameter of 1 mm and sintered in a spark plasma sintering furnace. The sintering temperature was 1200℃, the pressure was 50MPa, and the holding time was 15min to complete the coupling of SiCnw and Ti60 and obtain SiCnw / Ti60 composite material.
[0093] (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two SiCnw / Ti60 composite materials are twisted continuously to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally the basalt coupled carbon fiber composite bioelectrode material is obtained. The prepared basalt coupled carbon fiber composite bioelectrode material is named MBFNW4.
[0094] The above-mentioned MBFNW4 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor includes the following steps:
[0095] (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell;
[0096] (2) Inoculation of microbial community: The electroactive microbial community in the sludge was inoculated into the anode of the reactor. The sludge used for inoculation was taken from Yanjing Beer 4 Guilin Liquan Co., Ltd. After the fresh sludge was anaerobically cultured for one week, it was diluted with tap water at a sludge-to-water volume ratio of 1:2. 2L of diluted sludge was then introduced into the anode of the device.
[0097] (3) Cultivating biofilm: After inoculating sludge, a stable electroactive biofilm is formed after 7 days of cultivation;
[0098] (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it, and the pH of the wastewater is controlled to be 8.
[0099] (5) Operation: Apply an external voltage of 0.2V between the anode and cathode of the microbial electrolysis cell;
[0100] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0101] Example 5
[0102] This embodiment provides a method for preparing a basalt-coupled carbon fiber composite bioelectrode, comprising the following steps:
[0103] (1) Using Soxhlet extraction, basalt fibers were placed in petroleum ether and the original wetting agent on the surface of the basalt fibers was dissolved by heating and reflux. The heating and reflux temperature was 100℃ and the heating and reflux time was 72h. After Soxhlet extraction, the fibers were taken out, washed with water and dried to obtain clean basalt fibers.
[0104] (2) Etching treatment of basalt fiber: an etching solution was prepared by using 2 mol / L sodium hydroxide, 2 mol / L hydrochloric acid and 0.1 mol / L nitric acid. The clean basalt fiber was immersed in the etching solution for 120 min. The etching solution temperature was 100℃. After the reaction was completed, the fiber was taken out, washed with water and dried to obtain basalt fiber filler.
[0105] (3) After cutting the carbon fiber, it is soaked in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, then placed in acetone overnight for storage, and then dried. The carbon fiber has excellent high conductivity and excellent chemical stability. In wastewater treatment, carbon fiber can be used as an electrode material to accelerate the degradation process of pollutants through electrochemical methods.
[0106] (4) Basalt fiber filler and carbon fiber are connected by strands in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material. The porosity of basalt fiber provides attachment points for biomolecules, while the conductivity of carbon fiber provides an electron transfer channel for electrochemical degradation.
[0107] (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling. The ball-to-material ratio is 5:1, the ball mill speed is 500 r / min, and the ball milling time is 6 h to obtain mixed powder. Titanium alloy has high specific strength, excellent corrosion resistance and high conductivity. One-dimensional nanomaterial silicon carbide nanowires (SiCnw) not only inherit the excellent properties of high strength and low thermal expansion coefficient of SiC, but also have better mechanical properties, such as higher strength and better toughness, due to its unique nanoscale effect.
[0108] (6) The mixed powder was placed in a graphite mold with a diameter of 1 mm and sintered in a spark plasma sintering furnace. The sintering temperature was 1200℃, the pressure was 60MPa, and the holding time was 20min to complete the coupling of SiCnw and Ti60 and obtain SiCnw / Ti60 composite material.
[0109] (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two SiCnw / Ti60 composite materials are twisted continuously to tightly connect the basalt carbon fiber composite material and the SiCnw / Ti60 composite material, and finally the basalt coupled carbon fiber composite bioelectrode material is obtained. The prepared basalt coupled carbon fiber composite bioelectrode material is named MBFNW5.
[0110] The above-mentioned MBFNW5 is applied in a microbial electrolysis cell. The assembly method of the microbial electrolysis cell reactor includes the following steps:
[0111] (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell;
[0112] (2) Inoculation of microbial community: The electroactive microbial community in the sludge is inoculated into the anode of the reactor. The sludge used for inoculation is taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge is anaerobically cultured for one week, it is diluted with tap water at a sludge-to-water volume ratio of 1:2. 2L of diluted sludge is then introduced into the anode of the device.
[0113] (3) Cultivating biofilm: After inoculating sludge, a stable electroactive biofilm is formed after 7 days of cultivation;
[0114] (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it, and the pH of the wastewater is controlled to be 8.
[0115] (5) Operation: Apply an external voltage of 0.4V between the anode and cathode of the microbial electrolysis cell;
[0116] (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell is monitored regularly.
[0117] Comparative Example 1
[0118] Compared with Example 3, Comparative Example 1 used titanium alloy for connection when preparing basalt coupled carbon fiber composite bioelectrode, without adding SiCnw for improvement, and all other conditions remained unchanged.
[0119] Comparative Example 2
[0120] Compared with Example 3, Comparative Example 2 directly placed the electrode into the wastewater when preparing the microbial electrolysis cell, without inoculating sludge colonies, and all other conditions remained unchanged.
[0121] Comparative Example 3
[0122] Compared with Example 3, Comparative Example 3 used basalt fiber directly without etching when preparing basalt fiber, and all other conditions remained unchanged.
[0123] Comparative Example 4
[0124] Compared with Example 3, Comparative Example 4 used carbon fiber directly in the preparation of carbon fiber without soaking it in hydrochloric acid and sulfuric acid in sequence, and all other conditions remained unchanged.
[0125] Experimental Example
[0126] The performance of the basalt-coupled carbon fiber composite bioelectrodes prepared in Examples 1-5 and Comparative Examples 1-4 was monitored.
[0127] I. COD concentration in effluent
[0128] Using industrial wastewater with a COD concentration of 500 mg / L and a COD:N:P ratio of 100:5:1 as the influent, the COD concentration in the effluent was measured starting from the 5th day after the microbial electrolysis reactor was connected to the online automatic monitoring instrument. Data were collected every 5 days, with three sets of data collected each time, for a total of 6 measurements. The average COD concentration in the effluent is shown in Table 1.
[0129] Table 1
[0130]
[0131]
[0132] As shown in Table 1, the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials prepared in Examples 1-5 of this invention exhibit excellent COD removal rates. A comparison between Comparative Example 1 and Examples 1-5 shows that adding SiCnw to improve Ti60 can enhance the COD removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials. A comparison between Comparative Example 2 and Examples 1-5 shows that inoculating sludge bacteria can enhance the COD removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials. A comparison between Comparative Example 3 and Examples 1-5 shows that etching the basalt fibers can enhance the COD removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials. A comparison between Comparative Example 4 and Examples 1-5 shows that sequentially soaking the carbon fibers in hydrochloric acid and sulfuric acid can enhance the COD removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials.
[0133] II. Total nitrogen concentration in effluent
[0134] Using industrial wastewater with a COD of 500 mg / L and a COD:N:P ratio of 100:5:1 as influent, the total nitrogen concentration in the effluent was measured starting from the 5th day after the microbial electrolysis reactor was connected, under the control of an online automatic monitoring instrument. The monitoring values were recorded every 5 days, with three sets of data collected each time, for a total of 6 times. The average total nitrogen concentration in the effluent is shown in Table 2.
[0135] Table 2
[0136]
[0137]
[0138] As shown in Table 2, the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials prepared in Examples 1-5 of this invention exhibit excellent total nitrogen removal rates. A comparison between Comparative Example 1 and Examples 1-5 shows that adding SiCnw to improve Ti60 can increase the total nitrogen removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials. A comparison between Comparative Example 2 and Examples 1-5 shows that inoculating sludge bacteria can increase the total nitrogen removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials. A comparison between Comparative Example 3 and Examples 1-5 shows that etching the basalt fibers can increase the total nitrogen removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials. A comparison between Comparative Example 4 and Examples 1-5 shows that sequentially soaking the carbon fibers in hydrochloric acid and sulfuric acid can increase the total nitrogen removal rate of the microbial electrolysis cells of the basalt-coupled carbon fiber composite bioelectrode materials.
[0139] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
[0140] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a basalt-coupled carbon fiber composite bioelectrode, characterized in that, Includes the following steps: (1) Using Soxhlet extraction, basalt fibers are placed in a solvent and the original wetting agent on the surface of the basalt fibers is dissolved by heating and reflux. After Soxhlet extraction, the fibers are removed, washed with water and dried to obtain clean basalt fibers. In step (1), the solvent used is one of acetone, isopropanol, cyclohexane and petroleum ether. The heating and reflux temperature is 40~100℃ and the heating and reflux time is 12~72h. (2) Etching treatment of basalt fiber: Prepare an etching solution with sodium hydroxide, hydrochloric acid and nitric acid, immerse the clean basalt fiber in the etching solution, and the etching increases the specific surface area, surface roughness and adhesion of the fiber. After the reaction is completed, take it out, wash it with water and dry it to obtain basalt fiber filler; In step (2), the concentration of sodium hydroxide is 0.5~2 mol / L, the concentration of hydrochloric acid is 0.5~2 mol / L, the concentration of nitric acid is 0.01~0.1 mol / L, the etching time is 10~120 min, and the temperature of the etching solution is 20~100℃; (3) After cutting the carbon fiber, soak it in hydrochloric acid and sulfuric acid for more than 2 hours in sequence, put it in acetone overnight, and then take it out and dry it. (4) Basalt fiber filler and carbon fiber are braided and connected in a 2:1 ratio, and carbon fiber is connected to the end of basalt fiber to obtain basalt carbon fiber composite material. (5) Weigh Ti60 alloy powder and SiCnw, put them into a ball mill jar, and then place them in a planetary ball mill for ball milling to obtain mixed powder; in step (5), the ball-to-material ratio is 3~5:1; the ball mill speed is 300~500r / min, and the ball milling time is 4~6h; (6) The mixed powder is placed in a graphite mold with a diameter of 1 mm and sintered in a spark plasma sintering furnace to complete the coupling of SiCnw and Ti60, and finally obtain SiCnw / Ti60 composite material; in step (6), the sintering temperature is 1000~1200℃, the pressure is 40~60MPa, and the holding time is 5~20min; (7) The prepared basalt carbon fiber composite material is clamped with two SiCnw / Ti60 composite materials and the two SiCnw / Ti60 composite materials are twisted continuously to tightly connect the basalt carbon fiber composite material with the SiCnw / Ti60 composite material, thus obtaining the basalt coupled carbon fiber composite bioelectrode material.
2. A method for applying a basalt-coupled carbon fiber composite bioelectrode, characterized in that, The basalt-coupled carbon fiber composite bioelectrode is prepared by the method of claim 1. When applied in a microbial electrolysis cell, the assembly method of the microbial electrolysis cell reactor includes the following steps: (1) Assemble basalt coupled with carbon fiber composite bioelectrode material to obtain the anode and cathode of microbial electrolysis cell; (2) Inoculation of microbial community: The electroactive microbial community in the sludge is inoculated into the anode of the reactor; the sludge inoculated in step (2) is taken from Yanjing Beer Guilin Liquan Co., Ltd. After the fresh sludge is anaerobic cultured in the laboratory for one week, it is diluted with tap water at a sludge-to-water volume ratio of 1:2, and then 2L of diluted sludge is introduced into the anode of the device. (3) Cultivating biofilm: After inoculation, a stable electroactive biofilm is formed after 7 days of cultivation; (4) Wastewater addition: After a stable electroactive biofilm is formed, artificially prepared synthetic wastewater is immersed in it; in step (4), the pH of the wastewater is controlled to be 6~8; (5) Operation: Apply an external voltage between the anode and cathode of the microbial electrolysis cell; the voltage range in step (5) is 0.02~0.4V; (6) Performance monitoring: During operation, the performance of the microbial electrolysis cell shall be monitored regularly.
Citation Information
Patent Citations
Preparation method of nano-cellulose modified basalt fiber biological filler
CN115745143A
Electric strengthening device and method for strengthening biological denitrification of swine wastewater
CN116768416A
Treatment system and method for synchronously removing organic matters and sulfate in wastewater
CN117756300A